A MXene / silicon-carbon composite negative electrode material and its preparation method and application
By preparing MXene/silicon carbon composite anode material, using spray granulation and high-temperature treatment to form a core-shell structure, the problems of low capacity and easy powderization of the negative electrode material in the prior art are solved, and the circulation and rate performance of lithium-ion batteries are improved. Achieve efficient battery performance improvement.
Patent Information
- Application Number
- CN202310037035.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-10
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-01-10
AI Technical Summary
The negative electrode materials of existing lithium-ion batteries, especially commercial graphite materials, have low capacity and are easily powdered during charging and discharging, resulting in damage to the electrode conductive network, affecting cycle life and rate performance, and spontaneous collapse and reloading between MXene layers. The stack reduces Li+ adsorption sites and conductivity, limiting battery performance.
Using MXene/silicon carbon composite anode material, prepared by spray granulation and high-temperature treatment, MXene/TiN/nano-silicon/amorphous carbon composite with core-shell structure is formed, and the structural stability and interface are improved by using the amorphous carbon cladding layer. Stability, nano-silicon is evenly distributed in the void, enhancing the cycling and rate performance of the battery.
It effectively alleviates the volume expansion problem of silicon negative electrode material, improves the circulation performance and rate performance of lithium-ion batteries, the first discharge capacity reaches ≥1200mAh/g, the first charge and discharge efficiency is ≥70.0%, and maintains the mechanical stability of the negative electrode structure and Conductive properties.
Smart Images

Figure BDA0004049176290000081
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of negative electrode materials for lithium-ion batteries, and specifically relates to a MXene / silicon-carbon composite negative electrode material and a preparation method and application thereof. Background Art
[0002] Lithium-ion batteries have a series of advantages such as high specific capacity, stable operating voltage, good safety, and no memory effect. Therefore, they are widely used in many portable electronic equipment such as laptops, mobile phones, and instruments. With the rapid development of various electronic devices and electric vehicles, people have higher and higher requirements for the energy and cycle life of lithium-ion batteries. The negative electrode material is an important component of the battery. Together with the positive electrode material, it determines the key performance of the lithium-ion battery such as cycle life, capacity and safety, and has become the focus of research in various countries.
[0003] Currently, the specific capacity of commercial graphite-based negative electrode materials is low, only 372mAh / g, which limits the improvement of the overall capacity of lithium-ion batteries and can no longer meet market demand. It is reported that the theoretical lithium storage capacity of silicon is as high as 4200mAh / g, and the lithium insertion platform is slightly higher than that of graphite, with less safety hazards, and it is an excellent substitute for graphite-based negative electrode materials; however, silicon shows a volume change of up to 300% during the charge and discharge process, which can easily lead to the pulverization of silicon particles, the destruction of the conductive network inside the electrode, and poor conductivity.
[0004] In recent years, two-dimensional materials have shown great advantages in the field of energy storage due to their large specific surface area and short ion transmission path. MXene is a type of two-dimensional transition metal carbide with a graphene-like structure. It has a high specific surface area, good conductivity and hydrophilicity, and is expected to be an ideal matrix material for constructing nanocomposite structures. The prior art has reported the use of MXene and nano-silicon composites to alleviate the volume effect of silicon materials and improve the cycle performance of batteries. However, the MXene layers will spontaneously collapse and stack, greatly reducing the specific surface area of MXene and reducing Li + The collapse and stacking of MXene will lead to a significant increase in the resistivity of the MXene in the vertical interlayer direction, further hindering the Li + transmission, affecting the rate performance of the material. Summary of the invention
[0005] In order to improve the deficiencies of the prior art, the present invention provides a MXene / silicon-carbon composite negative electrode material and a preparation method and application thereof. The MXene / silicon-carbon composite negative electrode material can effectively alleviate the problem of volume expansion of silicon negative electrode materials, and the lithium-ion battery composed of the MXene / silicon-carbon composite negative electrode material has better cycle performance and rate performance.
[0006] Specifically, the present invention provides the following technical solutions:
[0007] A method for preparing a MXene / silicon-carbon composite negative electrode material, the method comprising the following steps:
[0008] (1) MXene, an organic carbon source, an organic solvent and a dispersant are ball-milled and then spray-granulated to obtain a precursor A;
[0009] (2) subjecting the precursor A of step (1) to high temperature treatment at 700° C. to 900° C. to obtain a precursor B;
[0010] (3) ultrasonically mixing the precursor B, nano-silicon, organic carbon source, organic solvent and dispersant of step (2), removing the organic solvent, and obtaining precursor C;
[0011] (4) The precursor C of step (3) is subjected to high-temperature carbonization treatment at 700° C. to 900° C. to obtain the MXene / silicon-carbon composite negative electrode material.
[0012] According to the present invention, in step (1), the MXene is obtained by acid corrosion and washing of MAX phase powder material using a method well known to those skilled in the art, and the MAX phase material includes one or more of Ti3AlC2, Ti2AlC, and Ti3AlCN.
[0013] According to the present invention, in step (1), the MXene includes at least one of Ti3C2 and Ti2C.
[0014] According to the present invention, in step (1), the MXene is a MXene nanosheet.
[0015] According to the present invention, in step (1), the dispersant is selected from at least one of nitrogen methyl pyrrolidone, polyethylene imine and polyvinyl alcohol; the organic carbon source is selected from at least one of asphalt, epoxy resin, phenolic resin and sucrose; and the organic solvent is selected from at least one of anhydrous ethanol, propanol, acetone, ethylene glycol and butanol.
[0016] According to the present invention, in step (1), the ball milling mixing is carried out in a planetary ball mill, and the rotation speed of the ball mill is 20r / min to 100r / min.
[0017] According to the present invention, in step (1), the ball milling mixing is carried out under an argon protective atmosphere.
[0018] According to the present invention, in step (1), the mass ratio of the MXene to the organic carbon source is 1:(0.05-0.2), preferably 1:(0.1-0.15), for example, 1:0.1, 1:0.11, 1:0.12, 1:0.13, 1:0.14, 1:0.15.
[0019] According to the present invention, in step (1), the mass ratio of the MXene to the organic solvent is 1:(1-8), preferably 1:(2-6), for example, 1:2, 1:3, 1:4, 1:5, 1:6.
[0020] According to the present invention, in step (1), the mass ratio of the MXene to the dispersant is 1:(0.01-0.05), preferably 1:(0.01-0.03), for example, 1:0.01, 1:0.02, 1:0.03.
[0021] According to the present invention, in step (1), the spray granulation is carried out in a spray granulation device, the feed inlet temperature of the spray granulation device is controlled at 170°C to 200°C, and the discharge port temperature is controlled at 80°C to 100°C.
[0022] According to the present invention, in step (1), the morphology of the precursor A is a "popcorn" spherical structure, and the precursor A is a "popcorn" spherical structure formed by bonding MXene nanosheets with an organic carbon source, and there are gaps between the MXene nanosheets.
[0023] According to the present invention, in step (1), the median particle size D of the precursor A is 50 It is 8μm to 20μm, for example, 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm, 16μm, 17μm, 18μm, 19μm or 20μm.
[0024] According to the present invention, in step (2), the high temperature treatment is carried out in a mixed atmosphere of ammonia and argon, and the volume ratio of ammonia to argon is (10-20):100.
[0025] According to the present invention, in step (2), the heating rate of the high temperature treatment is 2°C / min to 5°C / min.
[0026] According to the present invention, in step (2), the high temperature treatment time is 1 h to 10 h.
[0027] According to the present invention, in step (2), after the high temperature treatment is completed, the step of cooling to room temperature and screening is also included.
[0028] According to the present invention, in step (2), the organic carbon source in the spherical matrix of the precursor A is cracked into amorphous carbon during the heat treatment with ammonia and argon, and the Ti atoms on the outer surface of the MXene two-dimensional nanosheets are converted into TiN.
[0029] According to the present invention, in step (2), the precursor B is composed of MXene, TiN and amorphous carbon, and the mass ratio of MXene, TiN and amorphous carbon is 1: (0.01-0.05): (0.05-0.2), preferably 1: (0.01-0.03): (0.1-0.15). Among them, amorphous carbon bonds MXene nanosheets to form a spherical conductor, TiN is evenly distributed on the surface of MXene nanosheets, and there are gaps between MXene nanosheets.
[0030] According to the present invention, in step (3), the median particle size D of the nano-silicon is 50 It is 20nm~500nm.
[0031] According to the present invention, in step (3), the mass ratio of the precursor B to nano-silicon is 1:(0.01-0.3), preferably 1:(0.1-0.2), for example, 1:0.1, 1:0.12, 1:0.15, 1:0.18, 1:0.2.
[0032] According to the present invention, in step (3), the mass ratio of the precursor B to the organic carbon source is 1:(0.001-0.015), preferably 1:(0.005-0.01), for example, 1:0.005, 1:0.006, 1:0.007, 1:0.008, 1:0.009, 1:0.01.
[0033] According to the present invention, in step (3), the mass ratio of the precursor B to the organic solvent is 1:(0.001-0.02), preferably 1:(0.003-0.015), for example, 1:0.003, 1:0.005, 1:0.008, 1:0.010, 1:0.012, 1:0.015.
[0034] According to the present invention, in step (3), the mass ratio of the precursor B to the dispersant is 1:(0.005-0.015), preferably 1:(0.006-0.01), for example, 1:0.006, 1:0.007, 1:0.008, 1:0.009, 1:0.01.
[0035] According to the present invention, in step (3), the dispersant is selected from at least one of nitrogen methyl pyrrolidone, polyethylene imine and polyvinyl alcohol; the organic carbon source is selected from at least one of asphalt, epoxy resin, phenolic resin and sucrose; and the organic solvent is selected from at least one of anhydrous ethanol, propanol, acetone, ethylene glycol and butanol.
[0036] According to the present invention, in step (3), the nano-silicon is evenly distributed on the outer surface and in the gaps of the precursor B, which can further improve the capacity of the material.
[0037] According to the present invention, in step (3), the ultrasonic mixing time is 2-10 hours.
[0038] According to the present invention, in step (3), the organic solvent is removed by evaporation.
[0039] According to the present invention, in step (4), the high-temperature carbonization treatment is carried out in an inert atmosphere, and the inert atmosphere is nitrogen or argon.
[0040] According to the present invention, in step (4), the heating rate of the high temperature carbonization treatment is 2°C / min to 5°C / min.
[0041] According to the present invention, in step (4), the high temperature carbonization treatment time is 1 hour to 6 hours.
[0042] According to the present invention, in step (4), the MXene / silicon-carbon composite negative electrode material is composed of MXene, TiN, nano-silicon and amorphous carbon, wherein the mass ratio of MXene, TiN, nano-silicon and amorphous carbon is 1:(0.01-0.05):(0.01-0.3):(0.05-0.2), preferably 1:(0.01-0.03):(0.1-0.2):(0.1-0.2).
[0043] According to the present invention, in step (4), the amorphous carbon coating layer formed after high-temperature carbonization treatment of the organic carbon source is used as the coating layer of the silicon-carbon composite negative electrode material; the introduction of the carbon coating layer can prevent direct contact between the electrolyte and nano-silicon, so that the material has good structural stability and interface stability, thereby improving the initial efficiency and cycle performance of the battery.
[0044] The present invention also provides a MXene / silicon-carbon composite negative electrode material prepared by the above method.
[0045] According to the present invention, the MXene / silicon-carbon composite negative electrode material has a core-shell structure, wherein the core is a composite formed by MXene / TiN / nano-silicon / amorphous carbon; and the shell is amorphous carbon.
[0046] According to the present invention, the thickness of the amorphous carbon is 3 μm to 10 μm.
[0047] According to the present invention, the first discharge capacity of the MXene / silicon-carbon composite negative electrode material is ≥1200 mAh / g, and the first charge and discharge efficiency is ≥70.0%.
[0048] The present invention also provides the use of the above MXene / silicon-carbon composite negative electrode material in a lithium-ion battery, preferably as a negative electrode material for a lithium-ion battery.
[0049] Beneficial effects of the present invention:
[0050] (1) The present invention firstly adopts spray drying technology for secondary granulation, and uses an organic carbon source to bond MXene nanosheets into a "popcorn" spherical matrix with a fluffy multi-void structure. Then, during the heat treatment with ammonia and argon, the organic carbon source in the spherical matrix is cracked into amorphous carbon, and the Ti atoms on the outer surface of the MXene two-dimensional nanosheet are converted into TiN. When TiN with high strength and good conductivity and amorphous carbon with high tensile strength work together, the disadvantage that the negative electrode structure is easily destroyed during repeated charge and discharge can be overcome, and the integrity and mechanical stability of the macroscopic structure of the spherical conductive matrix can be maintained. The fluffy spherical structure provides a buffer space for the volume expansion of nano-silicon, thereby improving the cycle performance of the composite negative electrode material.
[0051] (2) The MXene-based multi-voided spherical conductor prepared by the present invention is conducive to uniformly dispersing and filling nano-Si into the voids of the spherical conductive matrix, and improves the tap density of the spherical conductive matrix. Finally, the amorphous carbon coating avoids direct contact between nano-Si and the electrolyte, thereby improving the initial efficiency of the battery.
[0052] (3) The spherical MXene / silicon-carbon composite negative electrode material prepared by the present invention has the characteristic of isotropy, which is conducive to the embedding of lithium ions from multiple directions, thereby improving the rate performance of the negative electrode material. DETAILED DESCRIPTION
[0053] The preparation method of the present invention will be described in further detail below in conjunction with specific examples. It should be understood that the following examples are only exemplary illustrations and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.
[0054] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods; the reagents, materials, etc. used in the following examples, unless otherwise specified, can be obtained from commercial channels.
[0055] Example 1
[0056] 10 g MXene (Ti3C2), 1 g asphalt, 30 g propanol, and 0.1 g nitrogen methyl pyrrolidone were mixed and placed in a planetary ball mill (speed 30 r / min, Ar) for 5 hours and spray dried to obtain precursor A (D 5013μm). The feed inlet temperature of the spray drying equipment was 190℃, the outlet temperature was 94℃, and the atomization frequency was 50Hz. Precursor A was placed in a rotary furnace, argon gas was introduced at a flow rate of 10L / min, the temperature was raised to 900℃, ammonia gas was introduced at a flow rate of 1L / min, and continued for 6.0h. The introduction of ammonia gas was stopped, and the precursor B was obtained by screening after cooling to room temperature. 10g of precursor B and 1g of nano-Si (D 50 50nm), 0.05g asphalt, 0.1g ethanol and 0.003 polyvinyl alcohol were mixed, and after ultrasonic stirring for 3 hours, the solvent was evaporated to obtain a precursor C, and the precursor C was subjected to high-temperature carbonization treatment at 750°C for 4 hours under nitrogen protection to obtain the MXene / silicon-carbon composite negative electrode material. The mass ratio of MXene, TiN, nano-silicon and amorphous carbon is 1:0.03:0.12:0.1.
[0057] Example 2
[0058] 10 g MXene (Ti3C2), 1.2 g sucrose, 40 g propanol, and 0.15 g nitrogen methyl pyrrolidone were mixed and placed in a planetary ball mill (speed 50 r / min, Ar) for 4 hours and spray dried to obtain precursor A (D 50 15μm). The feed inlet temperature of the spray drying equipment is 180℃, the outlet temperature is 85℃, and the atomization frequency is 50Hz. Precursor A is placed in a rotary furnace, argon gas is introduced at a flow rate of 15L / min, the temperature is raised to 800℃, ammonia gas is introduced at a flow rate of 3L / min, and the temperature is continued for 4.0h. The introduction of ammonia gas is stopped, and the precursor B is obtained by screening after cooling to room temperature; 10g of precursor B and 1.5g of nano-Si (D 50 40nm), 0.08g asphalt, 0.15g ethanol and 0.005g polyvinyl alcohol were mixed, and after ultrasonic stirring for 6 hours, the solvent was evaporated to obtain a precursor C, and the precursor C was subjected to high-temperature carbonization treatment at 850°C for 3 hours under nitrogen protection to obtain the MXene / silicon-carbon composite negative electrode material. The mass ratio of MXene, TiN, nano-silicon and amorphous carbon is 1:0.012:0.15:0.15.
[0059] Example 3
[0060] 10 g MXene (Ti3C2), 1.5 g epoxy resin, 60 g propanol, and 0.15 g nitrogen methyl pyrrolidone were mixed and placed in a planetary ball mill (speed 80 r / min, Ar) for 6 hours and spray dried to obtain precursor A (D 5017μm). The feed inlet temperature of the spray drying equipment was 190℃, the outlet temperature was 90℃, and the atomization frequency was 50Hz. Precursor A was placed in a rotary furnace, and argon gas was introduced at a flow rate of 15L / min. The temperature was raised to 800℃, and ammonia was introduced at a flow rate of 2L / min for 7.0h. The introduction of ammonia was stopped, and the precursor B was obtained by screening after cooling to room temperature. 10g of precursor B and 2.0g of nano-Si (D 50 30nm), 0.1g asphalt, 0.15g ethanol and 0.005g polyvinyl alcohol were mixed, and after ultrasonic stirring for 10 hours, the solvent was evaporated to obtain a precursor C, and the precursor C was subjected to high-temperature carbonization treatment at 800°C for 3 hours under nitrogen protection to obtain the MXene / silicon-carbon composite negative electrode material. The mass ratio of MXene, TiN, nano-silicon and amorphous carbon is 1:0.02:0.2:0.2.
[0061] Comparative Example 1
[0062] 10 g MXene (Ti3C2), 1 g nano-Si (50 nm), 1 g asphalt, 30 g propanol, and 0.1 g nitrogen methyl pyrrolidone were mixed and placed in a planetary ball mill (rotation speed 30 r / min, Ar) for 5 hours and spray dried to obtain precursor A (D 50 13μm). The feed inlet temperature of the spray drying equipment is 190℃, the discharge port temperature is 94℃, and the atomization frequency is 50Hz. Precursor A is placed in a rotary furnace, argon gas is introduced at a flow rate of 10L / min, the temperature is raised to 900℃, ammonia gas is introduced at a flow rate of 1L / min, and it lasts for 6.0h. The introduction of ammonia gas is stopped, and the precursor B is obtained by screening at room temperature; 10g of precursor B, 0.05g of asphalt and 0.1g of ethanol are mixed, ultrasonically stirred for 3 hours, and the solvent is evaporated to obtain precursor C. Precursor C is subjected to high-temperature carbonization treatment at 750℃ under nitrogen protection for 4h to obtain the MXene / silicon-carbon composite negative electrode material. The mass ratio of MXene, nano-silicon and amorphous carbon is 1:0.12:0.1.
[0063] Electrochemical performance test:
[0064] Semi-electric test method: The composite negative electrode material prepared in the embodiment and comparative example: conductive carbon black (SP): carboxymethyl cellulose (CMC): styrene-butadiene rubber (SBR) = 95:1:1.5:2.5 (mass ratio) was mixed evenly and applied on the copper foil. The coated electrode was placed in a vacuum drying oven at 120°C for 12 hours. The simulated battery assembly was carried out in a Braun glove box protected by argon. The electrolyte was 1M-LiPF6+EC:DEC:DMC (volume ratio was 1:1:1). The metal lithium sheet was the counter electrode. The simulated battery test was carried out in a 5V, 10mA Xinwei battery test cabinet. The charge and discharge voltage was 0.01-1.5V, and the charge and discharge rate was 0.1C. The first capacity and efficiency obtained by the test are listed in Table 1.
[0065] Full battery test method: A full battery was assembled using the composite material prepared in the embodiment and the comparative example as the negative electrode, lithium cobalt oxide as the positive electrode, and 1M-LiPF6+EC:DEC:DMC (volume ratio 1:1:1) solution as the electrolyte. The battery was charged and discharged at room temperature at a rate of 0.1C, with a voltage range of 3.0-4.2V. The cycle performance obtained from the test is listed in Table 1.
[0066] Maximum charging rate test method:
[0067] The battery cells were charged to 100% SOC at different rates, and then disassembled in a low temperature and low humidity environment to observe the lithium deposition on the negative electrode sheet.
[0068] Table 1. Electrochemical performance test results
[0069]
[0070] The above is an explanation of the embodiments of the present invention. However, the present invention is not limited to the above embodiments. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a MXene / silicon-carbon composite negative electrode material, the method comprising the following steps: (1) MXene, an organic carbon source, an organic solvent and a dispersant are ball-milled and then spray-granulated to obtain a precursor A; (2) subjecting the precursor A of step (1) to high temperature treatment at 700° C. to 900° C. to obtain a precursor B; (3) ultrasonically mixing the precursor B, nano-silicon, organic carbon source, organic solvent and dispersant of step (2), removing the organic solvent, and obtaining precursor C; (4) subjecting the precursor C of step (3) to a high temperature carbonization treatment at 700° C. to 900° C. to obtain the MXene / silicon-carbon composite negative electrode material; In step (2), the high temperature treatment is carried out in a mixed atmosphere of ammonia and argon, and the volume ratio of ammonia to argon is (10-20):100; In step (2), the high temperature treatment time is 1h~10h; In step (2), the precursor B is composed of MXene, TiN and amorphous carbon, and the mass ratio of MXene, TiN and amorphous carbon is 1: (0.01-0.05): (0.05-0.2); Amorphous carbon bonds MXene nanosheets to form spherical conductors, TiN is evenly distributed on the surface of MXene nanosheets, and there are gaps between MXene nanosheets; In step (4), the high temperature carbonization treatment is carried out in an inert atmosphere, and the inert atmosphere is nitrogen or argon; In step (4), the high temperature carbonization treatment time is 1h~6h; In step (4), the MXene / silicon-carbon composite negative electrode material is composed of MXene, TiN, nano-silicon and amorphous carbon, wherein the mass ratio of MXene, TiN, nano-silicon and amorphous carbon is 1: (0.01-0.05): (0.01-0.3): (0.05-0.2).
2. The preparation method according to claim 1, wherein In step (1), the MXene includes at least one of Ti3C2 and Ti2C; the dispersant is selected from at least one of nitrogen methyl pyrrolidone, polyethylene imine and polyvinyl alcohol; the organic carbon source is selected from at least one of asphalt, epoxy resin, phenolic resin and sucrose; the organic solvent is selected from at least one of anhydrous ethanol, propanol, acetone, ethylene glycol and butanol.
3. The preparation method according to claim 1, wherein In step (1), the ball milling mixing is carried out under an argon protective atmosphere.
4. The preparation method according to claim 1, wherein In step (1), the mass ratio of the MXene to the organic carbon source is 1:(0.05-0.2).
5. The preparation method according to claim 1, wherein In step (1), the mass ratio of the MXene to the organic solvent is 1:(1-8).
6. The preparation method according to claim 1, wherein In step (1), the mass ratio of the MXene to the dispersant is 1:(0.01-0.05).
7. The preparation method according to claim 1, wherein In step (1), the spray granulation is carried out in a spray granulation device, the feed inlet temperature of the spray granulation device is controlled at 170°C to 200°C, and the discharge port temperature is controlled at 80°C to 100°C.
8. The preparation method according to claim 1, wherein In step (1), the morphology of the precursor A is a "popcorn" spherical structure. The precursor A is a "popcorn" spherical structure formed by bonding MXene nanosheets with an organic carbon source, and there are gaps between the MXene nanosheets.
9. The preparation method according to claim 1, wherein In step (3), the median particle size D of the nano-silicon is 50 It is 20nm~500nm.
10. The preparation method according to claim 1, wherein: In step (3), the mass ratio of the precursor B to nano-silicon is 1:(0.01-0.3).
11. The preparation method according to claim 1, wherein: In step (3), the mass ratio of the precursor B to the organic carbon source is 1:(0.001-0.015).
12. The preparation method according to claim 1, wherein: In step (3), the mass ratio of the precursor B to the organic solvent is 1:(0.001-0.02).
13. The preparation method according to claim 1, wherein In step (3), the mass ratio of the precursor B to the dispersant is 1:(0.005-0.015).
14. The preparation method according to claim 1, wherein: In step (3), the dispersant is selected from at least one of nitrogen methyl pyrrolidone, polyethylene imine and polyvinyl alcohol; the organic carbon source is selected from at least one of asphalt, epoxy resin, phenolic resin and sucrose; and the organic solvent is selected from at least one of anhydrous ethanol, propanol, acetone, ethylene glycol and butanol.
15. A MXene / silicon-carbon composite negative electrode material prepared by the method according to any one of claims 1 to 14.
16. The MXene / silicon-carbon composite negative electrode material according to claim 15, wherein: The MXene / silicon-carbon composite negative electrode material has a core-shell structure, wherein the core is a composite formed by MXene / TiN / nano silicon / amorphous carbon; and the shell is amorphous carbon.
17. The MXene / silicon-carbon composite negative electrode material according to claim 15, wherein: The thickness of the amorphous carbon is 3 μm to 10 μm.
18. Use of the MXene / silicon-carbon composite negative electrode material according to any one of claims 15 to 17 in a lithium-ion battery.