A Y-type molecular sieve / macroporous alumina hybrid composite material and its synthesis method
Synthesis of Y-type molecular sieve/macroporous alumina hybrid composite material through eutectic hybridization principle, solving the problem of catalytic cracking of heavy oil by limiting microporous structure of Y-type zeolite molecular sieve, achieving efficient heavy oil conversion and low coke yield, with good Application prospects.
Patent Information
- Application Number
- CN202211610795.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-12
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2042-12-12
AI Technical Summary
The microporous structure of the existing Y-type zeolite molecular sieve limits the diffusion and mass transfer process of heavy oil macromolecules and cannot meet the needs of heavy oil catalytic cracking. The existing pore structure modulation technology has complex synthesis processes and high cost and structural damage.
Using eutectic hybridization principle, Y-type molecular sieve/macroporous alumina hybrid composite was synthesized, and a hybrid symbiotic structure between Y-type molecular sieve and macroporous alumina was formed by room temperature stirring and water bath treatment. Combined with autoclave crystallization, it was prepared. Material with excellent mesoporous structure.
It significantly improves the heavy oil conversion capacity, reduces the coke yield, excellent physical and chemical performance of the product, simple preparation process, low cost, and is suitable for the design and development of new high-performance FCC catalysts.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to a Y-type molecular sieve / macroporous alumina hybrid composite material and a synthesis method thereof, belonging to the technical field of catalytic material synthesis. Technical Background
[0002] At present, fluid catalytic cracking (FCC) is still the main domestic refining process, especially for the secondary processing of heavy crude oil, and the performance of FCC catalyst is a key influencing factor, which has a decisive influence on the overall reaction performance of the FCC unit. At present, the catalysts used in the FCC units of major domestic refineries are mostly semi-synthetic FCC catalysts, which are mainly composed of three components: Y-type zeolite molecular sieve, binder and matrix, among which Y-type zeolite molecular sieve is the core active component. However, since the main pore structure of conventional Y-type zeolite molecular sieve is a microporous structure (<2nm), it will seriously affect the diffusion and mass transfer process of heavy oil macromolecules in its structure, thereby greatly limiting the catalytic cracking reaction process of heavy oil macromolecules on its surface, which also makes it difficult for conventional Y-type zeolite molecular sieves to meet the requirements of the current heavy oil catalytic cracking process.
[0003] In order to solve the above problems, the existing technical methods mainly introduce "secondary medium and large pore" structural units into the Y-type zeolite molecular sieve structure to adjust the pore structure properties of the Y-type zeolite molecular sieve, thereby improving its diffusion and mass transfer performance for heavy oil macromolecules. Specifically, this type of technical method is currently based on two methods, namely "in situ synthesis" and "post-synthesis modification". Among them, in situ synthesis is to construct the "medium and large pore structural units" in situ in the Y-type molecular sieve structure during the synthesis of the Y-type molecular sieve by adopting a special synthesis method; post-synthesis modification is to modify the Y-type zeolite molecular sieve after it is synthesized, such as using high-temperature hydrothermal treatment, acid / base extraction and other post-modification methods, so as to introduce the "medium and large pore structural units" into its structure.
[0004] The above two methods have their own advantages and disadvantages. The in-situ synthesis method has better physical and chemical properties of the product, but its synthesis process is usually complicated and cumbersome, and most of these methods currently use special and expensive organic templates; the post-synthesis modification method is relatively simple, but the post-modification process will inevitably destroy the structure of the Y-type molecular sieve to a certain extent, making the physical and chemical properties of its product relatively poor. Due to the above reasons, the application of the existing technical methods in practice is greatly limited, which greatly hinders the design and development of new high-performance heavy oil catalytic cracking FCC catalysts. Summary of the invention
[0005] In view of the current situation that the pore structure properties of Y-type zeolite molecular sieves are difficult to meet the requirements of the mass transfer and diffusion performance of molecular sieves in the heavy oil catalytic cracking process, as well as the defects and shortcomings of the existing pore structure property modulation technology methods, the purpose of the present invention is to provide a Y-type molecular sieve / macroporous alumina hybrid composite material and a synthesis method thereof. Compared with conventional Y-type molecular sieves, the pore structure (especially the mesoporous structure) of the Y-type molecular sieve / macroporous alumina hybrid composite material has excellent performance and can well meet the needs of the heavy oil catalytic cracking process. At the same time, compared with the existing technical methods, the Y-type molecular sieve / macroporous alumina hybrid composite material has the significant advantages of simple preparation process and low raw material cost, and has good application prospects.
[0006] The present invention provides a method for synthesizing a Y-type molecular sieve / macroporous alumina hybrid composite material, comprising the following steps:
[0007] (1) Mixing sodium silicate, sodium aluminate and deionized water at room temperature for 0.5 to 3 hours, then aging at a water bath temperature of 30° C. to 55° C. for 4 to 24 hours, and cooling to room temperature to obtain a Y-type molecular sieve precursor solution;
[0008] (2) at room temperature, respectively mixing aluminum salt and sodium aluminate with deionized water and stirring until the aluminum salt and sodium aluminate are completely dissolved, thereby preparing an acidic aluminum source solution and an alkaline aluminum source solution;
[0009] (3) slowly adding the Y-type molecular sieve precursor solution and the alkaline aluminum source solution to the acidic aluminum source solution at a water bath temperature of 50°C to 95°C and under continuous stirring, respectively, by a parallel addition method until the pH value of the system reaches 6.5, and then adjusting the pH value of the system to 7 to 10 with an ammonia solution, and then allowing to stand for aging for 0.5 to 5 hours;
[0010] (4) adjusting the pH of the slurry system obtained in (3) to 11-14 with a dilute sodium hydroxide solution, then transferring it to an autoclave, standing it for crystallization at a temperature of 80°C-150°C for 12-48 hours, filtering, washing, drying and ammonium exchange to obtain the Y-type molecular sieve / macroporous alumina hybrid composite material.
[0011] The synthesis method provided by the present invention, wherein the mass ratio of sodium silicate, sodium aluminate and deionized water in step (1) is sodium silicate (calculated as SiO2): sodium aluminate (calculated as Al2O3): deionized water = 2-20:1:20-200, preferably 5-15:1:50-150.
[0012] In the synthesis method provided by the present invention, the aluminum salt in step (2) can be one or more of aluminum chloride, aluminum nitrate, aluminum sulfate, and hydroxyaluminum chloride, preferably aluminum sulfate.
[0013] The synthesis method provided by the present invention, wherein the mass ratio of the aluminum salt to deionized water in step (2) is aluminum salt (calculated as Al2O3):deionized water=1:3-30, preferably 5-10.
[0014] The synthesis method provided by the present invention, wherein the mass ratio of sodium aluminate to deionized water in step (2) is sodium aluminate (calculated as Al2O3): deionized water = 1:2-20, preferably 4-10.
[0015] In the synthesis method provided by the present invention, the filtering, washing, drying and ammonium exchange in step (3) are all common methods in the art and are not particularly limited by the present invention.
[0016] The Y-type molecular sieve / macroporous alumina hybrid composite material is obtained by any of the above-mentioned synthesis methods.
[0017] The present invention is based on the principle of "eutectic hybridization" and synthesizes a Y-type molecular sieve / macroporous alumina hybrid composite material. In the material structure, the Y-type molecular sieve and the macroporous alumina are in a hybrid symbiotic state, forming a composite crystal phase structure of "you have me, I have you", so that the material can simultaneously combine the high cracking activity of the Y-type molecular sieve and the pore structure performance advantages of the macroporous alumina material with large pore volume and large specific surface area. Therefore, the material will be able to well solve the defects of the current conventional Y-type molecular sieve heavy oil macromolecule mass transfer and diffusion performance, greatly improve the heavy oil conversion capacity of the current Y-type molecular sieve, and significantly reduce its coke yield. In addition, compared with the existing related technical methods, the method of the present invention not only has excellent product physical and chemical properties, but also has the significant advantages of low cost and simple process, and thus has good practical application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Attached photos Figure 1 The XRD spectrum of the Y-type molecular sieve / macroporous alumina hybrid composite material C3 sample synthesized by the method of the present invention. As can be seen from the figure, the C3 sample simultaneously shows the characteristic X-ray diffraction peaks of the Y-type molecular sieve and the macroporous alumina, indicating that the sample contains both the Y-type molecular sieve and the macroporous alumina components. DETAILED DESCRIPTION
[0019] The following is a detailed description of the embodiments of the present invention: This embodiment is implemented on the premise of the technical solution of the present invention, and a detailed implementation method and process are given, but the protection scope of the present invention is not limited to the following embodiments. The experimental methods in the following embodiments without specifying specific conditions are usually carried out under conventional conditions.
[0020] Raw material sources and specifications
[0021] Y-type molecular sieve (hydrogen type), aluminum sol and kaolin, Shanxi Tengmao Technology Co., Ltd., qualified products; aluminum sulfate (Al2(SO4)3·18H2O), sodium aluminate (NaAlO), sodium silicate (Na2SiO3·9H2O), sodium hydroxide (NaOH) and ammonia water (25%), Sinopharm Group, analytical grade reagents.
[0022] Sample characterization and evaluation
[0023] The crystallinity analysis of the samples was carried out on a D / max-2200PC X-ray diffractometer produced by Rigaku, Japan. The X-ray diffractometer has an operating voltage of 40 kV, a current of 20 mA, CuKα radiation, a phase scanning angle of 5 to 50°, and a scanning rate of 10 (°) / min; a crystallinity scanning angle of 22.5 to 25.0°, and a scanning rate of 1 (°) / min;
[0024] The specific surface area and pore volume parameters of the samples were measured on the ASAP3000 N2 adsorption-desorption instrument produced by Micromeritics, USA. The molecular sieve loading was about 0.0600g, and it was first pre-treated by vacuum degassing at 300℃ for 8h to remove moisture and residual impurities in the molecular sieve, and then the adsorption-desorption operation was carried out at liquid nitrogen temperature. The specific surface area and pore volume of the molecular sieve samples were determined by BET, t-plot and other methods;
[0025] The heavy oil catalytic cracking reaction performance of the FCC catalyst sample was carried out on an advanced catalytic cracking evaluation unit (ACE) with a reaction temperature of 530°C, a catalyst-to-oil ratio of 5, catalyst aging conditions of 800°C, 17h, 100% water vapor, and feed oil properties as shown in Table 1.
[0026] Table 1 Raw oil properties
[0027]
[0028]
[0029] Example 1
[0030] The method of the present invention is used to synthesize Y-type molecular sieve / macroporous alumina hybrid composite material
[0031] (1) At room temperature, 1185 g of sodium silicate, 80.4 g of sodium aluminate and 7500 g of deionized water were mixed and stirred for 0.5 hour, then aged in a water bath at 30° C. for 24 hours, and cooled to room temperature to obtain a Y-type molecular sieve precursor solution.
[0032] (2) At room temperature, 326.8 g of aluminum sulfate and 250 g of deionized water were mixed and stirred until the aluminum sulfate was dissolved to obtain an acidic aluminum source solution; 80.4 g of sodium aluminate and 255 g of deionized water were mixed and stirred until the sodium aluminate was completely dissolved to obtain an alkaline aluminum source solution.
[0033] (3) In a water bath at 95°C and with continuous stirring, the Y-type molecular sieve precursor solution and the alkaline aluminum source solution are slowly added to the acidic aluminum source solution in parallel until the pH value of the system reaches 6.5, and then the pH value of the system is adjusted to 7 with an ammonia solution, followed by aging for 0.5 hours.
[0034] (4) The pH of the slurry system obtained in (3) was adjusted to 11 with a dilute sodium hydroxide solution, and then transferred to an autoclave and allowed to stand for crystallization at 150° C. for 12 hours. After filtration, washing, drying and ammonium exchange, a Y-type molecular sieve / macroporous alumina hybrid composite material C1 was obtained.
[0035] Example 2
[0036] The method of the present invention is used to synthesize Y-type molecular sieve / macroporous alumina hybrid composite material
[0037] (1) At room temperature, 1991 g of sodium silicate, 96.5 g of sodium aluminate and 7800 g of deionized water were mixed and stirred for 1 hour, then aged in a water bath at 35° C. for 20 hours, and cooled to room temperature to obtain a Y-type molecular sieve precursor solution.
[0038] (2) At room temperature, 392.2 g of aluminum sulfate and 360 g of deionized water were mixed and stirred until the aluminum sulfate was dissolved to obtain an acidic aluminum source solution; 96.5 g of sodium aluminate and 330 g of deionized water were mixed and stirred until the sodium aluminate was completely dissolved to obtain an alkaline aluminum source solution.
[0039] (3) At a water bath temperature of 90° C. and under continuous stirring, the Y-type molecular sieve precursor solution and the alkaline aluminum source solution are slowly added to the acidic aluminum source solution in parallel until the pH value of the system reaches 6.5, and then the pH value of the system is adjusted to 7.5 with an aqueous ammonia solution, followed by aging for 1 hour.
[0040] (4) The pH value of the slurry system obtained in (3) is adjusted to 12 with a dilute sodium hydroxide solution, and then transferred to an autoclave and allowed to stand for crystallization at 130° C. for 18 hours. After filtration, washing, drying and ammonium exchange, a Y-type molecular sieve / macroporous alumina hybrid composite material C2 is obtained.
[0041] Example 3
[0042] The method of the present invention is used to synthesize Y-type molecular sieve / macroporous alumina hybrid composite material
[0043] (1) At room temperature, 2986 g of sodium silicate, 112.5 g of sodium aluminate and 7800 g of deionized water were mixed and stirred for 1.5 hours, then aged in a water bath at 40° C. for 16 hours, and cooled to room temperature to obtain a Y-type molecular sieve precursor solution.
[0044] (2) At room temperature, 457.5 g of aluminum sulfate and 490 g of deionized water were mixed and stirred until the aluminum sulfate was dissolved to obtain an acidic aluminum source solution; 112.5 g of sodium aluminate and 455 g of deionized water were mixed and stirred until the sodium aluminate was completely dissolved to obtain an alkaline aluminum source solution.
[0045] (3) At a water bath temperature of 80° C. and under continuous stirring, the Y-type molecular sieve precursor solution and the alkaline aluminum source solution are slowly added to the acidic aluminum source solution in parallel until the pH value of the system reaches 6.5, and then the pH value of the system is adjusted to 8 with an ammonia solution, followed by aging for 2 hours.
[0046] (4) The pH of the slurry system obtained in (3) was adjusted to 12.5 with a dilute sodium hydroxide solution, and then transferred to an autoclave and allowed to stand for crystallization at 110° C. for 24 hours. After filtration, washing, drying and ammonium exchange, a Y-type molecular sieve / macroporous alumina hybrid composite material C3 was obtained.
[0047] Example 4
[0048] The method of the present invention is used to synthesize Y-type molecular sieve / macroporous alumina hybrid composite material
[0049] (1) At room temperature, 4170 g of sodium silicate, 128.6 g of sodium aluminate and 7200 g of deionized water were mixed and stirred for 2.0 hours, then aged in a water bath at 45° C. for 12 hours, and cooled to room temperature to obtain a Y-type molecular sieve precursor solution.
[0050] (2) At room temperature, 522.9 g of aluminum sulfate and 640 g of deionized water were mixed and stirred until the aluminum sulfate was dissolved to obtain an acidic aluminum source solution; 128.6 g of sodium aluminate and 600 g of deionized water were mixed and stirred until the sodium aluminate was completely dissolved to obtain an alkaline aluminum source solution.
[0051] (3) In a water bath at 70°C and with continuous stirring, the Y-type molecular sieve precursor solution and the alkaline aluminum source solution are slowly added to the acidic aluminum source solution in parallel until the pH value of the system reaches 6.5, and then the pH value of the system is adjusted to 8.5 with an aqueous ammonia solution, followed by aging for 3 hours.
[0052] (4) The pH of the slurry system obtained in (3) was adjusted to 13 with a dilute sodium hydroxide solution, and then transferred to an autoclave and allowed to stand for crystallization at 100° C. for 30 hours. After filtration, washing, drying and ammonium exchange, a Y-type molecular sieve / macroporous alumina hybrid composite material C4 was obtained.
[0053] Example 5
[0054] The method of the present invention is used to synthesize Y-type molecular sieve / macroporous alumina hybrid composite material
[0055] (1) At room temperature, 5545 g of sodium silicate, 144.7 g of sodium aluminate and 6300 g of deionized water were mixed and stirred for 2.5 hours, then aged in a water bath at 50° C. for 8 hours, and cooled to room temperature to obtain a Y-type molecular sieve precursor solution.
[0056] (2) At room temperature, 588.2 g of aluminum sulfate and 810 g of deionized water were mixed and stirred until the aluminum sulfate was dissolved to obtain an acidic aluminum source solution; 144.7 g of sodium aluminate and 765 g of deionized water were mixed and stirred until the sodium aluminate was completely dissolved to obtain an alkaline aluminum source solution.
[0057] (3) In a water bath at 60°C and with continuous stirring, the Y-type molecular sieve precursor solution and the alkaline aluminum source solution are slowly added to the acidic aluminum source solution in parallel until the pH value of the system reaches 6.5, and then the pH value of the system is adjusted to 9 with an aqueous ammonia solution, followed by aging for 4 hours.
[0058] (4) The pH of the slurry system obtained in (3) was adjusted to 13.5 with a dilute sodium hydroxide solution, and then transferred to an autoclave and allowed to stand for crystallization at 90° C. for 36 hours. After filtration, washing, drying and ammonium exchange, a Y-type molecular sieve / macroporous alumina hybrid composite material C5 was obtained.
[0059] Example 6
[0060] The method of the present invention is used to synthesize Y-type molecular sieve / macroporous alumina hybrid composite material
[0061] (1) At room temperature, 7109 g of sodium silicate, 160.8 g of sodium aluminate and 5000 g of deionized water were mixed and stirred for 3 hours, then aged in a water bath at 55° C. for 4 hours, and cooled to room temperature to obtain a Y-type molecular sieve precursor solution.
[0062] (2) At room temperature, 653.6 g of aluminum sulfate and 1000 g of deionized water were mixed and stirred until the aluminum sulfate was dissolved to obtain an acidic aluminum source solution; 160.8 g of sodium aluminate and 950 g of deionized water were mixed and stirred until the sodium aluminate was completely dissolved to obtain an alkaline aluminum source solution.
[0063] (3) At a water bath temperature of 50° C. and under continuous stirring, the Y-type molecular sieve precursor solution and the alkaline aluminum source solution are slowly added to the acidic aluminum source solution in parallel until the pH value of the system reaches 6.5, and then the pH value of the system is adjusted to 10 with an ammonia solution, followed by aging for 5 hours.
[0064] (4) The pH of the slurry system obtained in (3) is adjusted to 14 with a dilute sodium hydroxide solution, and then transferred to an autoclave and allowed to stand for crystallization at 80° C. for 48 hours. After filtration, washing, drying and ammonium exchange, a Y-type molecular sieve / macroporous alumina hybrid composite material C6 is obtained.
[0065] Example 7
[0066] Preparation of FCC catalyst containing conventional Y-type molecular sieve (hydrogen type)
[0067] According to the mass ratio of molecular sieve: aluminum sol (calculated by Al2O3 mass): kaolin = 35:12:53, the measured Y-type molecular sieve (hydrogen type), aluminum sol and kaolin are mixed and slurried, and then spray-formed, calcined, washed with water and dried to obtain FCC catalyst-1.
[0068] Example 8
[0069] Preparation of FCC catalyst containing Y-type molecular sieve / macroporous alumina hybrid composite material of the present invention
[0070] According to the mass ratio of Y-type molecular sieve / macroporous alumina hybrid composite material: aluminum sol (calculated by Al2O3 mass): kaolin = 35:12:53, the measured Y-type molecular sieve / macroporous alumina hybrid composite material C3, aluminum sol and kaolin are mixed and slurried, and then spray-formed, calcined, washed with water and dried to obtain FCC catalyst-2.
[0071] Table 2 lists the pore structure property parameters of different samples. It can be seen that compared with conventional Y-type molecular sieves, the total specific surface area and total pore volume of the Y-type molecular sieve / macroporous alumina hybrid composite materials C1-C6 synthesized in this patent have been greatly improved, and the mesopore specific surface area and mesopore volume contained are also significantly higher than the former, which will be able to effectively solve the current conventional Y-type molecular sieves The defect of poor mass transfer and diffusion performance of heavy oil macromolecules, thereby greatly improving the heavy oil catalytic cracking reaction performance of FCC catalysts.
[0072] Table 2 Pore structure properties of different samples
[0073]
[0074] Table 3 lists the heavy oil catalytic cracking reaction performance of different FCC catalysts. It can be seen that the heavy oil catalytic cracking reaction performance of the FCC catalyst-2 using the synthetic Y-type molecular sieve / macroporous alumina hybrid composite material of the present invention has been significantly improved compared with the FCC catalyst-1 using the conventional Y-type molecular sieve. Compared with FCC catalyst-1, the heavy oil and coke yields of FCC catalyst-2 decreased by 1.19 and 1.28 percentage points, respectively, while the gasoline and total liquid yields increased by 3.02 and 2.96 percentage points, respectively.
[0075] Table 3 Heavy oil catalytic cracking reaction performance of different FCC catalysts
[0076]
[0077] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for synthesizing a Y-type molecular sieve / macroporous alumina hybrid composite material, characterized in that The steps include: (1) Mix sodium silicate, sodium aluminate and deionized water at room temperature for 0.5 to 3 hours, then place in a water bath at 30°C to 55°C for aging for 4 to 24 hours, and cool to room temperature to obtain a Y-type molecular sieve precursor solution; (2) at room temperature, respectively mixing aluminum salt and sodium aluminate with deionized water and stirring until the aluminum salt and sodium aluminate are completely dissolved, thereby preparing an acidic aluminum source solution and an alkaline aluminum source solution, respectively; the aluminum salt is one or more of aluminum chloride, aluminum nitrate, aluminum sulfate, and aluminum hydroxychloride; (3) At a water bath temperature of 50°C to 95°C and under continuous stirring, the Y-type molecular sieve precursor solution and the alkaline aluminum source solution are slowly added to the acidic aluminum source solution in a parallel flow manner until the pH value of the system reaches 6.5, and then the pH value of the system is adjusted to 7 to 10 with an ammonia solution, and then the system is allowed to stand for aging for 0.5 to 5 hours; (4) adjusting the pH of the slurry system obtained in (3) to 11 to 14 with a dilute sodium hydroxide solution, then transferring it to an autoclave, standing it for crystallization at 80° C. to 150° C. for 12 to 48 hours, filtering, washing, drying and ammonium exchange to obtain the Y-type molecular sieve / macroporous alumina hybrid composite material.
2. The synthesis method according to claim 1, characterized in that: The mass ratio of sodium silicate, sodium aluminate and deionized water in step (1) is sodium silicate: sodium aluminate: deionized water = 2 ~ 20: 1: 20 ~ 200; wherein sodium silicate is calculated as SiO2 and sodium aluminate is calculated as Al2O3.
3. The synthesis method according to claim 2, characterized in that: The mass ratio of sodium silicate, sodium aluminate and deionized water in step (1) is sodium silicate: sodium aluminate: deionized water = 5 ~ 15: 1: 50 ~ 150; wherein sodium silicate is calculated as SiO2 and sodium aluminate is calculated as Al2O3.
4. The synthesis method according to claim 1, characterized in that: The aluminum salt in step (2) is aluminum sulfate.
5. The synthesis method according to claim 1, characterized in that: The mass ratio of aluminum salt to deionized water in step (2) is aluminum salt: deionized water = 1:3-30; wherein the aluminum salt is calculated as Al2O3.
6. The synthesis method according to claim 1, characterized in that: The mass ratio of sodium aluminate to deionized water in step (2) is sodium aluminate: deionized water = 1:2-20; wherein sodium aluminate is calculated as Al2O3.
7. A Y-type molecular sieve / macroporous alumina hybrid composite material, characterized in that: The Y-type molecular sieve / macroporous alumina hybrid composite material is obtained according to the synthesis method described in any one of claims 1-6.