A hollow spherical silicon dioxide with adjustable specific surface area and its preparation method and application

Hollow spherical silica particles are synthesized by soft template method and calcined at high temperature to adjust the specific surface area, which solves the problems of complex preparation process and high cost of metal oxide nanomaterials in existing transparent thermal insulation coatings, and achieves efficient and low-cost transparent Thermal insulation coating is prepared with excellent ultraviolet and infrared blocking properties and good thermal insulation effect.

CN115924924BActive Publication Date: 2024-10-22HENAN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211011039.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-08-23
Publication Date
2024-10-22
Estimated Expiration
2042-08-23

AI Technical Summary

Technical Problem

The metal oxide nanomaterials used in existing transparent heat-insulating coatings have complex preparation processes and high costs, making it difficult to achieve simple and efficient large-scale production. They are also hard, which affects the preparation cycle and fineness.

Method used

The soft template method is used to synthesize hollow spherical silica, and the specific surface area is controlled by high-temperature calcination to prepare hollow spherical silica particles with lower hardness and high transparency, which are used as paint fillers and stirred at high speed through a simple disperser. Reaching fineness, suitable for industrial production.

Benefits of technology

A transparent heat-insulating coating that achieves high UV and infrared blocking rates, shortens the preparation cycle, has low cost, is suitable for large-scale production, and can achieve 89% UV and 90% infrared blocking while ensuring visible light transmittance. rate, the insulation temperature difference reaches 9℃.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 220823135425
    Figure 220823135425
  • Figure 220823135429
    Figure 220823135429
  • Figure 220823135432
    Figure 220823135432
Patent Text Reader

Abstract

The present invention proposes a method for preparing hollow spherical silica with adjustable specific surface area, comprising: 1) synthesizing hollow spherical silica with different particle sizes by a soft template method; 2) controlling the calcination temperature to adjust the specific surface area of ​​the hollow spherical silica. The prepared hollow spherical silica with different specific surface areas has a low thermal conductivity and excellent visible light transmittance, and is an ideal filler for transparent thermal insulation coatings, which can be used in the fields of construction, automobiles, trains, and aircraft glass. The method has a simple process and low cost, and has extremely high application value and broad market prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of transparent heat-insulating material production, and specifically relates to hollow spherical silicon dioxide with adjustable specific surface area, and a preparation method and application thereof. Background Art

[0002] Some spaces where humans live (such as houses and vehicles) need to have two major functions: insulation and lighting. Although ordinary glass has good transparency, it has poor infrared and ultraviolet blocking performance, so the development of transparent thermal insulation coatings is of great significance.

[0003] The research on transparent thermal insulation coatings in the United States, Japan, South Korea and other countries started relatively early, and the research focus was mainly on metal oxide nanomaterials, such as ITO (indium tin oxide) and ATO (antimony tin oxide). First, the prepared nano metal oxide is formulated into a stable and dispersed aqueous or oily slurry, and then applied to the coating to obtain a multifunctional transparent coating with heat insulation, UV and infrared blocking properties. The main disadvantage of this type of filler is that the hardness is relatively large, and the preparation of the slurry requires complex process flows such as ball milling and sand milling to obtain a slurry with suitable fineness; the preparation cycle is long and the cost is expensive. Therefore, it is urgent to develop a new type of functional filler that not only has a good transparent thermal insulation effect, but also can achieve simple and efficient large-scale preparation. Summary of the invention

[0004] The purpose of the present invention is to overcome and solve the problems and defects existing in the prior art, and to provide a hollow spherical silica with adjustable specific surface area, which has a simple preparation process, easy to control reaction conditions, low cost, and is suitable for industrial production; the prepared hollow spherical silica is used as a filler for a coating to obtain a transparent thermal insulation coating with a higher ultraviolet and infrared blocking rate, which is expected to replace the metal oxides in the coating filler and become a new generation of transparent thermal insulation coating.

[0005] The invention also provides a preparation method and application of the hollow spherical silica.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] A method for preparing hollow spherical silica with adjustable specific surface area comprises two steps: synthesizing hollow spherical silica by a soft template method and regulating specific surface area by high temperature calcination, as follows:

[0008] 1) Synthesis of hollow spherical silica with different particle sizes by soft template method: a surfactant (as a spherical soft template), a silane coupling agent (as a surface modifier), tetraethyl orthosilicate (TEOS) and an ethanol aqueous solution are subjected to hydrolysis and condensation reaction under alkaline conditions to obtain a mesoporous spherical silica slurry; and then a high-temperature hydrothermal reaction is performed to obtain a hollow spherical silica slurry;

[0009] 2) The hollow spherical silica slurry is washed, dried, crushed and calcined to obtain hollow spherical silica with adjustable specific area.

[0010] Specifically, in step 1), the surfactant is one or more of hexadecyltrimethylammonium bromide, dodecylammonium chloride, sodium dodecyl sulfate, hexadecyltrimethylammonium chloride, and the like.

[0011] Furthermore, in step 1), the silane coupling agent is one or more of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, dimethyldiethoxysilane, hexamethyldisilazane, etc.

[0012] Specifically, in the ethanol aqueous solution of step 1), the molar ratio of ethanol to water is 1: (10-30); ethanol is industrial alcohol with a concentration of 95%. One or more organic bases such as triethanolamine, diethanolamine, triethylamine, diethylamine, etc. are selected to adjust the pH value to alkaline (pH=9-12).

[0013] Furthermore, in step 1), the temperature of the hydrolysis condensation reaction (mainly used for the hydrolysis condensation and surface modification of TEOS) is 30-60° C., and the reaction time is 1-5 h.

[0014] Furthermore, in step 1), the mass ratio of the surfactant to tetraethyl orthosilicate is 1:(5-30), and the molar ratio of the silane coupling agent to tetraethyl orthosilicate is 1:(2-20).

[0015] Specifically, in step 1), the hydrothermal reaction temperature is 110-180° C., and the reaction time is 6-16 hours.

[0016] Specifically, in step 2), the specific surface area, pore volume and pore diameter of the hollow spherical silica are adjusted by calcining at a temperature of 500-1100° C. and a calcining time of 2-12 h.

[0017] The present invention provides hollow spherical silica with adjustable specific surface area prepared by the above method. The hollow spherical silica with different specific surface areas has a particle outer diameter of 50-500nm, a wall thickness of 2-60nm, and a specific surface area of ​​20-600m 2 / g. The prepared hollow spherical silica has a complete shell, good sphericity and uniform particle size distribution.

[0018] The present invention also provides application of the hollow spherical silica with adjustable specific surface area in transparent heat-insulating coatings.

[0019] The preparation process provided by the present invention is simple, the reaction conditions are easy to control, the cost is low, and it is suitable for industrial production. The hollow spherical silica prepared is used as a filler for the coating to obtain a transparent heat-insulating coating with a high ultraviolet and infrared blocking rate, which is expected to replace the metal oxides in the coating filler and become a new generation of transparent heat-insulating coating. Compared with the prior art, the present invention has the following beneficial effects:

[0020] 1) The hollow spherical silica particles with adjustable specific surface area prepared by the present invention have relatively low hardness. As fillers in thermal insulation coatings, they can be made into slurry with the required fineness only by high-speed stirring in a disperser. The entire preparation cycle of the transparent thermal insulation coating is short and can be completed in 1 hour;

[0021] 2) The hollow spherical silica with adjustable specific surface area prepared by the present invention is used as a filler to prepare a transparent heat-insulating coating. Under the condition of maintaining a transmittance of 70% for visible light, the blocking rates for ultraviolet rays and infrared rays can reach 89% and 90% respectively, and the heat-insulating temperature difference can reach 9°C;

[0022] 3) The preparation method provided by the present invention has the characteristics of simple process and low cost, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The SEM image (a) and TEM image (b) of the 50nm hollow spherical silica in Example 1 calcined at 500°C are shown in the figure. It can be seen from the figure that after calcination at 500°C, the 50nm hollow spherical silica still maintains a complete shell and sphericity;

[0024] Figure 2 The TEM images of 100nm hollow spherical silica in Example 2 (a), Example 3 (b), Example 4 (c), and Example 5 (d) are calcined at 500℃, 700℃, 900℃, and 1000℃, respectively. It can be seen from the images that after calcination at different temperatures, the 100nm hollow spherical silica still maintains a complete shell and sphericity, and the surface is more dense.

[0025] Figure 3 TEM images (a) of the 200 nm hollow spherical silica calcined at 500° C. in Example 6 and (b) of the 300 nm hollow spherical silica calcined at 500° C. in Example 7. It can be seen from the figures that the 200 nm and 300 nm hollow spherical silicas still maintain a complete shell and sphericity after being calcined at 500° C.

[0026] Figure 4 The data shows the change in thermal insulation performance of 50nm hollow spherical silica calcined at 500℃ at different addition amounts in the coating. DETAILED DESCRIPTION

[0027] The present invention is described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0028] In the following examples, all the raw materials used are common commercial products that can be directly purchased in the art. Ethanol is industrial alcohol with a concentration of 95%.

[0029] Example 1

[0030] A method for preparing hollow spherical silica with adjustable specific surface area comprises the following steps:

[0031] 1) Weigh 22.5 g of hexadecyltrimethylammonium chloride, 180 g of triethanolamine, 225 g of ethanol, 1950 g of pure water, and 75 g (0.38 mol) of γ-mercaptopropyltrimethoxysilane into a 5 L high-pressure reactor (the pH of the mixed solution is 10), add 450 g (2.16 mol) of TEOS under stirring at 60 ° C, and react at a constant temperature for 3 hours. In this step, a mesoporous spherical silica slurry is obtained;

[0032] 2) Based on step 1), the temperature is raised to 160° C. for hydrothermal reaction for 10 h to obtain hollow spherical silica slurry;

[0033] 3) The slurry obtained in step 2) was filtered and washed three times with ethanol and pure water respectively, and the filter cake was dried and crushed. The treated white powder was calcined at 500°C in a muffle furnace for 11 hours, and finally the shell was intact, with an outer diameter of 50nm, a wall thickness of 6nm, and a specific surface area of ​​550.7m 2 / g, pore volume 1.6cm 3 / g, hollow spherical silica with a pore size of 20.9nm (the SEM and TEM images are shown in Figure 1 ).

[0034] Embodiment 2:

[0035] A method for preparing hollow spherical silica with adjustable specific surface area comprises the following steps:

[0036] 1) Weigh 30g of hexadecyltrimethylammonium bromide, 375g of triethanolamine, 270g of ethanol, 1800g of pure water, and 120g (0.54mol) of γ-aminopropyltriethoxysilane into a 5L autoclave (pH of the mixed solution is 9), add 600g (2.88mol) of TEOS under stirring at 30°C, and react at a constant temperature for 1h. In this step, a mesoporous spherical silica slurry is obtained;

[0037] 2) Based on step 1), the temperature was raised to 110° C. for hydrothermal reaction for 16 h to obtain hollow spherical silica slurry;

[0038] 3) The slurry obtained in step 2) was filtered and washed three times with ethanol and pure water respectively, and the filter cake was dried and crushed. The treated white powder was calcined at 500°C in a muffle furnace for 11 hours to obtain a shell with an intact outer diameter of 100nm, a wall thickness of 17nm, and a specific surface area of ​​542.5m 2 / g, pore volume 1.7cm 3 / g, hollow spherical silica with a pore size of 30.2nm.

[0039] Example 3

[0040] A method for preparing hollow spherical silica with adjustable specific surface area comprises the following steps:

[0041] 1) Weigh 27 g of hexadecyltrimethylammonium chloride, 375 g of triethanolamine, 270 g of ethanol, 1800 g of pure water, and 90 g (0.38 mol) of γ-glycidyloxypropyltrimethoxysilane into a 5 L high-pressure reactor (the pH of the mixed solution is 10), add 600 g (2.88 mol) of TEOS under stirring at 30 ° C, and react at a constant temperature for 1 hour. In this step, a mesoporous spherical silica slurry is obtained;

[0042] 2) Based on step 1), the temperature is raised to 120° C. for hydrothermal reaction for 15 h to obtain hollow spherical silica slurry;

[0043] 3) The slurry obtained in step 2) was filtered and washed three times with ethanol and pure water respectively, and the filter cake was dried and crushed. The treated white powder was calcined at 700°C in a muffle furnace for 8 hours to obtain a shell with an intact outer diameter of 100nm, a wall thickness of 18nm, and a specific surface area of ​​391.3m 2 / g, pore volume 1.1cm 3 / g, hollow spherical silica with a pore size of 19.1nm.

[0044] Example 4

[0045] A method for preparing hollow spherical silica with adjustable specific surface area comprises the following steps:

[0046] 1) Weigh 45 g of hexadecyltrimethylammonium bromide, 375 g of diethanolamine, 270 g of ethanol, 2100 g of pure water, and 90 g (0.46 mol) of γ-mercaptopropyltrimethoxysilane into a 5 L high-pressure reactor (the pH of the mixed solution is 10), add 600 g (2.88 mol) of TEOS under stirring at 30 ° C, and react at a constant temperature for 1 hour. In this step, a mesoporous spherical silica slurry is obtained;

[0047] 2) Based on step 1), the temperature is raised to 140° C. for hydrothermal reaction for 14 h to obtain hollow spherical silica slurry;

[0048] 3) The slurry obtained in step 2) was filtered and washed three times with ethanol and pure water respectively, and the filter cake was dried and crushed. The treated white powder was calcined at 900°C in a muffle furnace for 4 hours to obtain a shell with an intact outer diameter of 100nm, a wall thickness of 15nm, and a specific surface area of ​​163.2m 2 / g, pore volume 0.7cm 3 / g, hollow spherical silica with a pore size of 9.8nm.

[0049] Example 5

[0050] A method for preparing hollow spherical silica with adjustable specific surface area comprises the following steps:

[0051] 1) Weigh 30 g of hexadecyltrimethylammonium chloride, 300 g of triethanolamine, 270 g of ethanol, 1650 g of pure water, and 75 g (0.51 mol) of dimethyldiethoxysilane into a 5 L high-pressure reactor (the pH of the mixed solution is 10), add 750 g (3.60 mol) of TEOS under stirring at 50 ° C, and react at a constant temperature for 2 h. In this step, a mesoporous spherical silica slurry is obtained;

[0052] 2) Based on step 1), the temperature is raised to 160° C. for hydrothermal reaction for 10 h to obtain hollow spherical silica slurry;

[0053] 3) The slurry obtained in step 2) was filtered and washed three times with ethanol and pure water respectively, and the filter cake was dried and crushed. The treated white powder was calcined at 1000°C in a muffle furnace for 2 hours to obtain a shell with an intact outer diameter of 100nm, a wall thickness of 16nm, and a specific surface area of ​​70.1m 2 / g, pore volume 0.2cm 3 / g, hollow spherical silica with a pore size of 8.4nm.

[0054] The BET data of the hollow spherical silica prepared at different calcination temperatures in Examples 2 to 5 are shown in Table 1. The results in Table 1 show that hollow spherical silica with different specific surface areas, pore volumes and pore diameters can be obtained by controlling the calcination temperature.

[0055] Table 1, BET test data of 100nm hollow spherical silica at different calcination temperatures

[0056] .

[0057] Example 6

[0058] A method for preparing hollow spherical silica with adjustable specific surface area comprises the following steps:

[0059] 1) Weigh 40g of hexadecyltrimethylammonium chloride, 180g of triethanolamine, 225g of ethanol, 1950g of pure water, and 75g (0.38mol) of γ-mercaptopropyltrimethoxysilane into a 5L high-pressure reactor (the pH of the mixed solution is 10), add 450g (2.16mol) of TEOS under stirring at 60°C, and react at a constant temperature for 3h. In this step, a mesoporous spherical silica slurry is obtained;

[0060] 2) Based on step 1), the temperature is raised to 160° C. for hydrothermal reaction for 10 h to obtain hollow spherical silica slurry;

[0061] 3) The slurry obtained in step 2) was filtered and washed three times with ethanol and pure water respectively, and the filter cake was dried and crushed. The treated white powder was calcined at 500°C in a muffle furnace for 11 hours to obtain a shell with an intact outer diameter of 200nm, a wall thickness of 40nm, and a specific surface area of ​​500.7m 2 / g, pore volume 1.8cm 3 / g, hollow spherical silica with a pore size of 20.9nm.

[0062] Example 7

[0063] A method for preparing hollow spherical silica with adjustable specific surface area comprises the following steps:

[0064] 1) Weigh 50g of sodium dodecyl sulfate, 375g of triethanolamine, 270g of ethanol, 1800g of pure water, and 105g (0.42mol) of γ-methacryloxypropyltrimethoxysilane into a 5L high-pressure reactor (the pH of the mixed solution is 10), add 600g (2.88mol) of TEOS under stirring at 30°C, and react at a constant temperature for 1h. In this step, a mesoporous spherical silica slurry is obtained;

[0065] 2) raising the temperature based on step 1) and hydrothermally reacting at 130° C. for 15 h to obtain hollow spherical silica slurry;

[0066] 3) The slurry obtained in step 2) was filtered and washed three times with ethanol and pure water respectively, and the filter cake was dried and crushed. The treated white powder was calcined at 500°C in a muffle furnace for 11 hours to obtain a shell with an intact outer diameter of 300nm, a wall thickness of 50nm, and a specific surface area of ​​438.7m 2 / g, pore volume 1.9cm 3 / g, hollow spherical silica with a pore size of 21.2nm.

[0067] Application test

[0068] A method for preparing a transparent heat-insulating hollow spherical silica / waterborne polyacrylate composite coating and film comprises the following steps:

[0069] 1) The hollow spherical silicon dioxide powder obtained in Example 1 was re-dispersed in pure water and stirred at high speed for 30 minutes to obtain a slurry of the desired fineness (concentration of 20%);

[0070] 2) adding the slurry obtained in step 1) into a mixed solution consisting of a water-based polyacrylate emulsion, a wetting agent (CF-10), a dispersant (DN01), a defoamer (BYK022), and a leveling agent (RM2020) (the mass ratio is 100:1:1:1:10), and stirring at high speed in a disperser for 30 minutes to obtain a hollow spherical silica / water-based polyacrylate composite coating;

[0071] 3) The composite coating obtained in step 2) is coated on a glass substrate by a coating device and dried at room temperature. The coating thickness is 75 μm, thereby obtaining a transparent heat-insulating hollow spherical silica / waterborne polyacrylate composite film.

[0072] Table 2, optical properties of hollow spherical silica (50nm) calcined at 500℃ at different addition amounts in the coating (the addition amount is based on the proportion of polyacrylate)

[0073] .

[0074] The optical performance test standard of the transparent thermal insulation coating is carried out in accordance with GBT 2680-2021 (index requirements: visible light transmittance: ≥60%, ultraviolet blocking rate: ≥60%, infrared blocking rate: ≥70%), and the results are shown in Table 2. The results of Table 2 show that the transparent thermal insulation coating prepared by the present invention (taking 50nm hollow spherical silica as an example, with an addition amount of 15%-25%) has a high blocking rate for ultraviolet and infrared rays while ensuring good visible light transmittance, with an ultraviolet blocking rate of more than 78% and an infrared blocking rate of more than 70%.

[0075] The thermal insulation performance test standard of transparent thermal insulation coatings is carried out in accordance with GBT 2680-2021. Figure 4 The data on the change of thermal insulation performance of hollow spherical silica at different addition amounts in coatings are given. Figure 4 The results show that when the hollow spherical silica is added in an amount of 25%, the maximum thermal insulation temperature difference reaches 9°C, indicating that the transparent thermal insulation coating prepared by the present invention has good thermal insulation performance.

[0076] In summary, it can be seen that the hollow spherical silica with different specific surface areas prepared by the present invention has a low thermal conductivity and excellent visible light transmittance, and is an ideal filler for transparent thermal insulation coatings, which can be used in the fields of construction, automobiles, trains, aircraft glass, etc.; and the method has a simple process and low cost, and has extremely high application value and broad market prospects.

[0077] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes that do not deviate from the present invention should be equivalent replacement modes and are included in the protection scope of the present invention.

Claims

1. Application of hollow spherical silica with adjustable specific surface area in transparent thermal insulation coating, characterized in that: The hollow spherical silica with adjustable specific area is prepared by the following steps: 1) subjecting a surfactant, a silane coupling agent, tetraethyl orthosilicate and an ethanol aqueous solution to a hydrolysis condensation reaction under alkaline conditions to obtain a mesoporous spherical silica slurry; and then subjecting the slurry to a hydrothermal reaction to obtain a hollow spherical silica slurry; 2) The hollow spherical silica slurry is washed, dried, crushed and calcined to obtain hollow spherical silica with adjustable specific area; In step 1), the surfactant is one or more of hexadecyltrimethylammonium bromide, dodecylammonium chloride, sodium dodecyl sulfate, and hexadecyltrimethylammonium chloride; In step 1), the silane coupling agent is one or more of γ-aminopropyltriethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, dimethyldiethoxysilane, and hexamethyldisilazane; Step 1) In the ethanol aqueous solution, the molar ratio of ethanol to water is 1: (10-30); one or more of triethanolamine, diethanolamine, triethylamine, and diethylamine are selected to adjust the pH value to 9-12; In step 1), the hydrolysis condensation reaction temperature is 30-60°C, the reaction time is 1-5h; the molar ratio of silane coupling agent to tetraethyl orthosilicate is 1:(2-20); In step 1), the hydrothermal reaction temperature is 110-180°C and the reaction time is 6-16h; In step 2), the calcination temperature is 500-1100°C and the calcination time is 2-12h; The hollow spherical silica with adjustable specific surface area is used as a filler to prepare a transparent heat-insulating coating. Under the condition of maintaining a transmittance of 70% for visible light, the blocking rates for ultraviolet rays and infrared rays reach 89% and 90% respectively, and the heat-insulating temperature difference reaches 9°C.