Permanent antistatic masterbatch for polyethylene film and preparation method thereof

Through the combination of modified carbon fiber and polyethylene wax, the conductive structure of the polyethylene film is formed, which solves the problem of adding a large amount of permanent antistatic agent in the polyethylene film and achieves a low-cost, low-haze permanent antistatic effect.

CN115926293BActive Publication Date: 2024-10-11SUZHOU DUCHAMPS ADVANCED MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211709273.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-29
Publication Date
2024-10-11
Estimated Expiration
2042-12-29

AI Technical Summary

Technical Problem

The existing polyethylene film contains a large amount of permanent antistatic agent, which results in complex processing technology, high cost, and affects the haze of the product, making it unable to meet the needs of long-term products.

Method used

Using a method of combining modified carbon fiber and polyethylene wax, the surface roughness and hydrophilicity of the carbon fiber are increased through oxidative etching and reduction treatments, and mixed with 2-alkyl imidazoline to form a conductive structure inside the polyethylene and an external one. Conductive surface layer to reduce the amount of antistatic agent added.

Benefits of technology

It achieves the permanent antistatic effect of the polyethylene film, reduces the amount of antistatic agent, simplifies the process, reduces the cost, avoids haze problems, and meets the surface resistance requirements for long-term use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention discloses a permanent antistatic masterbatch for polyethylene film, which mainly comprises: 100 parts of polyethylene, 0.1-1 parts of permanent antistatic agent, 1-2 parts of toughening agent, and 0.01-0.1 parts of 2-alkyl imidazoline; the permanent antistatic agent is modified carbon fiber. The present invention develops a new permanent antistatic agent for polyethylene, and experiments show that the surface resistance of the film prepared by the masterbatch of the present invention can be controlled within 10 5 About, meeting the requirements of permanent antistatic.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of films, and in particular to a permanent antistatic masterbatch for polyethylene, a preparation method and a polyethylene film. Background Art

[0002] Polyethylene (PE) is a thermoplastic resin obtained by polymerization of ethylene. Polyethylene is odorless, non-toxic, has excellent low temperature resistance (the lowest operating temperature can reach -100°C), good chemical stability, and can withstand the corrosion of most acids and alkalis (not resistant to oxidizing acids). It is insoluble in general solvents at room temperature, has low water absorption, and has excellent electrical insulation. Polyethylene can be processed using general thermoplastic molding methods. It has a wide range of uses, mainly used to make films, packaging materials, containers, pipes, monofilaments, wires and cables, daily necessities, etc. It can also be used as high-frequency insulation materials for televisions, radars, etc.

[0003] For polyethylene, it has good electrical insulation properties, and its film surface is prone to accumulate net charges, which affects the use of film products. In the prior art, the method to solve the net charge on the film surface is mainly to add antistatic agents. Antistatic agents can be divided into two categories: ordinary antistatic agents and permanent antistatic agents. The former has a validity period of 3 to 5 months. For ordinary antistatic agents, according to different usage methods, they can be divided into two types: external coating type and internal mixing type: external coating type antistatic agent refers to a type of antistatic agent used on the surface of polymer materials. It is generally attached to the surface of polymer materials by coating, spraying or dipping, and then dried at room temperature or hot air to form an antistatic coating. This type is mostly a cationic antistatic agent; mixed antistatic agent refers to a type of antistatic agent added to the resin during the processing of the product, generally non-ionic and anionic.

[0004] Since the effectiveness of common antistatic agents is generally 3 to 5 months, the surface resistivity is generally 10 13 ~10 15Ω•m, for special products that are used for a long time, this aging time is not satisfied, so a permanent antistatic agent is needed. The existing permanent antistatic agents are mainly enhanced conductive materials and conductive powders as antistatic fillers, mainly selected from one or several combinations of carbon powder, carbon fiber, metal powder, and metal fiber. For example, Chinese invention patent CN104403175A discloses a permanent antistatic polyolefin masterbatch, in which the antistatic agents mainly used are conductive materials and enhanced conductive powders as antistatic fillers. For another example, Chinese invention patent CN108084567A discloses a low-fog anti-adhesion masterbatch for polyethylene and a preparation method thereof, which uses a silicone microsphere as an anti-adhesion agent. However, these additive permanent antistatic agents often require a large addition amount (generally at least 10%), which requires the addition of a large amount of dispersant, which not only has a complex processing technology, high cost, and poor overall performance, but also a large addition amount can easily affect the haze of the product.

[0005] Therefore, how to reduce the amount of permanent antistatic agent while achieving the permanent antistatic effect is obviously of positive practical significance. Summary of the invention

[0006] The purpose of the present invention is to provide a permanent antistatic masterbatch for polyethylene, a preparation method and a polyethylene film.

[0007] In order to achieve the above-mentioned invention object, the technical solution of the present invention is: a permanent antistatic masterbatch for polyethylene film, which mainly comprises, by weight:

[0008] 100 parts of polyethylene, 0.1-1 parts of permanent antistatic agent, 1-2 parts of toughening agent, 0.01-0.1 parts of 2-alkyl imidazoline;

[0009] The permanent antistatic agent is a modified carbon fiber, and the modification method is as follows: the carbon fiber is oxidized by a strong acid to increase its surface roughness, and then reduced by a reducing agent to hydroxylate its surface, thereby obtaining the modified carbon fiber; the modified carbon fiber is in the shape of a long strip, and its length is 100 to 900 microns;

[0010] The toughening agent is polyethylene wax; the carbon number of the alkyl group in the 2-alkyl imidazoline is 1 to 4.

[0011] In the above, the permanent antistatic agent is preferably 0.5-0.9 parts, or 0.2 parts, 0.3 parts, 0.4 parts, 0.6 parts, 0.7 parts, or 0.8 parts. The toughening agent is preferably 1.4-1.7 parts, or 1.2 parts, 1.3 parts, 1.5 parts, 1.6 parts, 1.8 parts, or 1.9 parts. The 2-alkyl imidazoline is preferably 0.05-0.08 parts, or 0.02 parts, 0.03 parts, 0.04 parts, 0.06 parts, 0.07 parts, or 0.09 parts. The modified carbon fiber is in the shape of a long strip, and its length is preferably 400-700 microns, or 200 microns, 300 microns, 500 microns, 600 microns, or 800 microns.

[0012] In the above, the molecular weight of the polyethylene is 15000-19000. The polyethylene is selected from one or more of homopolymer polyethylene, copolymer polyethylene and metallocene polyethylene; the DSC melting point of component A is 120-135°C, the melt flow rate is 1-2g / 10min, and the density is 0.9-0.959g / cm 3 .

[0013] The polyethylene wax is prior art and has a CAS number of 9002-88-4.

[0014] Preferably, the preparation method is as follows:

[0015] (1) Preparing a permanent antistatic agent: adding a strong acid to the carbon fiber to oxidatively etch the carbon fiber to increase the polarity and roughness of the fiber surface;

[0016] Cooling to room temperature, washing with water until neutral, and drying; then dispersing the oxidized carbon fiber in tetrahydrofuran, adding a reducing agent for reduction to hydroxylate its surface; washing, drying, and obtaining the modified carbon fiber;

[0017] (2) Mixing polyethylene, toughening agent, 2-alkyl imidazoline and the permanent antistatic agent obtained in the above step (1) and fully mixing them by melting to form a uniform dispersion system; injecting them into a two-stage extruder in series to form a uniformly mixed melt, injecting supercritical carbon dioxide into the front section of the second stage extruder to mix the melt uniformly, extruding through a die head, cooling, pelletizing and drying to obtain the masterbatch.

[0018] Preferably, the strong acid is concentrated nitric acid or concentrated sulfuric acid; and the reducing agent is lithium aluminum hydride or sodium borohydride.

[0019] Preferably, the molecular weight of the polyethylene is 15000-19000, preferably 15000-16000.

[0020] Preferably, the masterbatch has a melt index of 2-4 g / min at 190° C. and a load of 2.16 kg.

[0021] Preferably, the ratio of the permanent antistatic agent to the toughening agent is 1:5-10 by mass.

[0022] The present invention also claims a method for preparing a permanent antistatic masterbatch, comprising the following steps:

[0023] (1) Preparing a permanent antistatic agent: adding a strong acid to the carbon fiber to oxidatively etch the carbon fiber to increase the polarity and roughness of the fiber surface;

[0024] Cooling to room temperature, washing with water until neutral, and drying; then dispersing the oxidized carbon fiber in tetrahydrofuran, adding a reducing agent for reduction to hydroxylate its surface; washing, drying, and obtaining the modified carbon fiber;

[0025] (2) Mixing polyethylene, toughening agent, 2-alkyl imidazoline and the permanent antistatic agent obtained in the above step (1) and fully mixing them by melting to form a uniform dispersion system; injecting them into a two-stage extruder in series to form a uniformly mixed melt, injecting supercritical carbon dioxide into the front section of the second stage extruder to mix the melt uniformly, extruding through a die head, cooling, pelletizing and drying to obtain the masterbatch.

[0026] Preferably, the extruder is a twin-screw extruder, the temperature of the extruder head is 160-200° C., and the speed of the twin-screw extruder is 100 r / min.

[0027] Preferably, the injection amount of the supercritical carbon dioxide is 10-50 g / min, and the injection pressure is 15-25 MPa.

[0028] The present invention also claims protection for a polyethylene film, comprising the above masterbatch or the masterbatch obtained by the above preparation method, wherein the mass percentage of the above masterbatch is 10-30%.

[0029] Preferably, the surface resistance of the polyethylene film is 1.0×10 5 ~9.9×10 5 .

[0030] The present invention firstly performs oxidation etching treatment on the carbon fiber to make its surface morphology rough, thereby increasing the mechanical meshing between the fibers. Meanwhile, by adding polyethylene wax, the distance between polyethylene macromolecular chains is increased, and the porosity is improved, so that the carbon fibers are interwoven with each other to form a three-dimensional network structure and dissolved in the polyethylene body, thereby forming a structure with excellent conductive performance inside the polyethylene; outside the polyethylene, since the carbon fiber surface is hydroxylated (i.e., hydrophilic) after being modified, when 2-alkyl imidazoline is blended with polyethylene, the oleophilic end of the 2-alkyl imidazoline is combined with the polyethylene, and the hydrophilic end extends out of the polyethylene, and attracts and drives the modified carbon fiber to partially extend out of the polyethylene (and / or the modified carbon fiber is connected to the hydrophilic end of the 2-alkyl imidazoline), thereby forming a conductive surface layer on the surface of the polyethylene, thereby forming a "core-shell structure" to achieve a permanent antistatic structure and effect.

[0031] By adopting the above technical solution, the present invention achieves the following technical effects:

[0032] 1. The present invention develops a new permanent antistatic agent for polyethylene. First, the carbon fiber is modified to obtain a rough surface structure, and polyethylene wax is used to increase the distance between polyethylene macromolecular chains, thereby forming a structure with excellent conductive properties inside the polyethylene (the carbon fibers are interwoven to form a three-dimensional network structure); at the same time, on the outside of the polyethylene, the modified carbon fiber is combined with 2-alkyl imidazoline, so that the modified carbon fiber partially extends out of the polyethylene (and / or the modified carbon fiber is connected to the hydrophilic end of the 2-alkyl imidazoline), thereby forming a conductive surface layer on the surface of the polyethylene, forming a "core-shell structure", and achieving a permanent antistatic structure and effect; experiments have shown that the surface resistance of the film prepared by the masterbatch of the present invention can be controlled within 10 5 About, meeting the requirements of permanent antistatic;

[0033] 2. Experimental findings show that the amount of the permanent antistatic agent added in the present invention can be very small, and there is no need to add other additives such as compatibilizers as in the prior art. The small amount added can also avoid the problem of high haze caused by a large amount added in the prior art.

[0034] 3. The preparation method of the present invention is simple and easy to implement, has low cost, and is suitable for popularization and application. DETAILED DESCRIPTION

[0035] The following is a clear and complete description of the technical solutions in the embodiments of the present invention in combination with the specific content of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the protection scope of the present invention.

[0036] Example 1

[0037] 1. Preparation of permanent antistatic agent

[0038] Concentrated nitric acid is added to the carbon fiber to oxidatively etch the carbon fiber to increase the polarity and roughness of the fiber surface; the carbon fiber is cooled to room temperature, washed with water until neutral, and dried; the oxidized carbon fiber is then dispersed in tetrahydrofuran, sodium borohydride is added for reduction to hydroxylate its surface; the modified carbon fiber is washed and dried to obtain the modified carbon fiber.

[0039] 2. Preparation of masterbatch

[0040] The masterbatch is composed of the following components: by weight percentage, 100 parts of polyethylene, 0.8 parts of permanent antistatic agent, 1.6 parts of toughening agent, and 0.1 parts of 2-alkyl imidazoline; the toughening agent is polyethylene wax;

[0041] The molecular weight of the polyethylene is 15000-17000, and homopolymer polyethylene is used.

[0042] The polyethylene, toughening agent, 2-alkyl imidazoline and permanent antistatic agent are mixed with the above formula, melted and fully mixed to form a uniform dispersion system; injected into a two-stage extruder in series to form a uniformly mixed melt, supercritical carbon dioxide is injected into the front section of the second stage extruder to mix evenly with the melt, extruded through a die head, cooled, pelletized and dried to obtain the masterbatch.

[0043] The extruder is a twin-screw extruder; the temperature of the extruder head is 180-200°C, the speed of the twin-screw extruder is 100r / min. The injection amount of the supercritical carbon dioxide is 45g / min, and the injection pressure is 18 MPa.

[0044] 3. Preparation of polyethylene film

[0045] The specific preparation method is as follows: the masterbatch is added to polyethylene at a mass percentage of 15%, and the masterbatch and polyethylene are injected into a twin-screw extruder through a feeder for melt extrusion, and the melt extrusion temperature is 190-220°C; the melt is cooled into a cast sheet through a quenching roller, and first stretched longitudinally at a stretching temperature of 170-180°C, cooled to 140-160°C, and then stretched transversely at a qualitative temperature of 110-120°C. The film enters a traction machine, and the traction roller temperature is maintained at 20-40°C. After flattening, it is rolled up, and the obtained film is aged for one week before the performance is measured. The film thickness is 100 microns.

[0046] Example 2

[0047] The same as Example 1, the only difference is the formula: 100 parts of polyethylene, 0.1 parts of permanent antistatic agent, 1 part of polyethylene wax, and 0.03 parts of 2-alkyl imidazoline.

[0048] Example 3

[0049] The same as Example 1, the only difference is the formula: 100 parts of polyethylene, 0.3 parts of permanent antistatic agent, 1 part of polyethylene wax, and 0.06 parts of 2-alkyl imidazoline.

[0050] Example 4

[0051] The same as Example 1, the only difference is the formula: 100 parts of polyethylene, 0.5 parts of permanent antistatic agent, 1 part of polyethylene wax, and 0.08 parts of 2-alkyl imidazoline.

[0052] Example 5

[0053] The same as Example 1, the only difference is the formula: 100 parts of polyethylene, 0.6 parts of permanent antistatic agent, 1.2 parts of polyethylene wax, and 0.09 parts of 2-alkyl imidazoline.

[0054] Example 6

[0055] The same as Example 1, the only difference is the formula: 100 parts of polyethylene, 1.0 part of permanent antistatic agent, 2 parts of polyethylene wax, and 0.1 part of 2-alkyl imidazoline.

[0056] Comparative Example 1

[0057] The same as Example 1, the only difference is the formula: 100 parts of polyethylene, 1.1 parts of permanent antistatic agent, 2 parts of polyethylene wax, and 0.1 parts of 2-alkyl imidazoline.

[0058] Comparative Example 2

[0059] The same as Example 1, the only difference is the formula: 100 parts of polyethylene, 1.3 parts of permanent antistatic agent, 2 parts of polyethylene wax, and 0.1 parts of 2-alkyl imidazoline.

[0060] Comparative Example 3

[0061] The same as Example 1, the only difference is the formula: 100 parts of polyethylene, 2 parts of permanent antistatic agent, 2 parts of polyethylene wax, and 0.1 parts of 2-alkyl imidazoline.

[0062] Comparative Example 4

[0063] The same as Example 1, the only difference is the formula: 100 parts of polyethylene, 10 parts of permanent antistatic agent, 2 parts of polyethylene wax, and 0.1 parts of 2-alkyl imidazoline.

[0064] Comparative Example 5

[0065] The same as Example 1, the only difference is the formula: 100 parts of polyethylene, 0.09 parts of permanent antistatic agent, 1 part of polyethylene wax, and 0.1 parts of 2-alkyl imidazoline.

[0066] Comparative Example 6

[0067] The same as Example 1, the only difference is the formula: 100 parts of polyethylene, 0.07 parts of permanent antistatic agent, 1 part of polyethylene wax, and 0.1 parts of 2-alkyl imidazoline.

[0068] Comparative Example 7

[0069] The same as Example 1, the only difference is the formula: 100 parts of polyethylene, 0.01 parts of permanent antistatic agent, 1 part of polyethylene wax, and 0.1 parts of 2-alkyl imidazoline.

[0070] Comparative Example 8

[0071] The same as Example 1, the only difference is the formula: 100 parts of polyethylene and 0.8 parts of permanent antistatic agent.

[0072] The films obtained in the above examples and comparative examples were subjected to performance tests, and the results are shown in the following table:

[0073]

[0074] As can be seen from the table above, the amount of permanent antistatic agent added and the formulation of the present invention (i.e., the amount of polyethylene wax and 2-alkyl imidazoline added) have a great influence on the surface resistance and haze of the film. The experiment found that only when the amount of permanent antistatic agent added is 0.1-1 part and the amount of polyethylene wax added is 1-2 parts, the surface resistance of the film can be controlled within 10 5 The haze is about 0.62, and the preferred ratio of the permanent antistatic agent to the polyethylene wax is 1:2.

[0075] When the amount of permanent antistatic agent added exceeds 1.0 part, the surface resistance will jump to 10 6 When the amount of permanent antistatic agent added is less than 0.1 parts, the surface resistance will jump to 10 7 Compared with Example 1 and Comparative Example 8, when the amount of permanent antistatic agent added is the same but polyethylene wax is not added, the surface resistance increases sharply and the antistatic effect cannot be achieved.

[0076] In addition, experiments have found that the ratio of permanent antistatic agent to polyethylene wax will also have a great influence on the surface resistance. When the ratio of permanent antistatic agent to polyethylene wax is 1:2 or above, it will have a good effect. When the ratio is less than 1:2, it will lead to an increase in surface resistance.

[0077] The detection methods of the above physical parameters are as follows:

[0078] Surface resistance: Refer to the national standard GB / T1410-2006 Test method for volume resistivity and surface resistivity of solid insulating materials.

[0079] Haze: Refer to the national standard GB / T2410-2008 Determination of light transmittance and haze of transparent plastics.

[0080] Tensile strength: The test is carried out in accordance with the national standard GB 13022-91 "Test method for tensile properties of plastic films".

[0081] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.

Claims

1. A permanent antistatic masterbatch for polyethylene film, characterized in that: According to the weight percentage, it mainly includes: 100 parts of polyethylene, 0.1-1 parts of permanent antistatic agent, 1-2 parts of toughening agent, 0.01-0.1 parts of 2-alkyl imidazoline; The permanent antistatic agent is a modified carbon fiber, and the modification method is as follows: the carbon fiber is oxidized by a strong acid to increase its surface roughness, and then reduced by a reducing agent to hydroxylate its surface, thereby obtaining the modified carbon fiber; the modified carbon fiber is in the shape of a long strip, and its length is 100 to 900 microns; The toughening agent is polyethylene wax; the carbon number of the alkyl group in the 2-alkyl imidazoline is 1 to 4; The ratio of the permanent antistatic agent to the polyethylene wax is 1:2; The preparation method of the permanent antistatic masterbatch is as follows: (1) Preparing a permanent antistatic agent: adding a strong acid to the carbon fiber to oxidatively etch the carbon fiber to increase the polarity and roughness of the fiber surface; Cooling to room temperature, washing with water until neutral, and drying; then dispersing the oxidized carbon fiber in tetrahydrofuran, adding a reducing agent for reduction to hydroxylate its surface; washing, drying, and obtaining the modified carbon fiber; (2) Mixing polyethylene, toughening agent, 2-alkyl imidazoline and the permanent antistatic agent obtained in the above step (1) and fully mixing them by melting to form a uniform dispersion system; injecting them into a two-stage extruder in series to form a uniformly mixed melt, injecting supercritical carbon dioxide into the front section of the second stage extruder to mix the melt uniformly, extruding through a die head, cooling, pelletizing and drying to obtain the masterbatch.

2. The permanent antistatic masterbatch according to claim 1, characterized in that: The strong acid is concentrated nitric acid or concentrated sulfuric acid; the reducing agent is lithium aluminum hydride or sodium borohydride.

3. The permanent antistatic masterbatch according to claim 1, characterized in that: The masterbatch has a melt index of 2 to 4 g / min at 190° C. and a load of 2.16 kg.

4. A method for preparing the permanent antistatic masterbatch according to any one of claims 1 to 3, characterized in that: The following steps are involved: (1) Preparing a permanent antistatic agent: adding a strong acid to the carbon fiber to oxidatively etch the carbon fiber to increase the polarity and roughness of the fiber surface; Cooling to room temperature, washing with water until neutral, and drying; then dispersing the oxidized carbon fiber in tetrahydrofuran, adding a reducing agent for reduction to hydroxylate its surface; washing, drying, and obtaining the modified carbon fiber; (2) Mixing polyethylene, toughening agent, 2-alkyl imidazoline and the permanent antistatic agent obtained in the above step (1) and fully mixing them by melting to form a uniform dispersion system; injecting them into a two-stage extruder in series to form a uniformly mixed melt, injecting supercritical carbon dioxide into the front section of the second stage extruder to mix the melt uniformly, extruding through a die head, cooling, pelletizing and drying to obtain the masterbatch.

5. The method for preparing the permanent antistatic masterbatch according to claim 4, characterized in that: The injection amount of the supercritical carbon dioxide is 10-50 g / min, and the injection pressure is 15-25 MPa.

6. A polyethylene film, comprising the masterbatch according to any one of claims 1 to 3 or the masterbatch obtained by the preparation method according to any one of claims 4 to 5, wherein the mass percentage of the masterbatch is 10 to 30%.

7. The polyethylene film according to claim 6, characterized in that The surface resistance of the polyethylene film is 1.0×10 5 ~9.9×10 5 ohm.