Ultra-low carbon nitrogen molten steel and smelting method thereof
Through the smelting method that combines the electric furnace and the RH refining furnace, and the use of lance injection technology and vacuum refining technology, the carbon and nitrogen content in the molten steel was successfully reduced, solving the problem of difficulty in controlling the carbon and nitrogen content in the steel in the existing technology, and improving Improve production stability and reduce carbon emissions.
Patent Information
- Application Number
- CN202310009421.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-03
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-01-03
AI Technical Summary
Existing steelmaking technology is difficult to effectively reduce the carbon and nitrogen content in steel, especially in the production of advanced steel grades, resulting in a decrease in the high-temperature strength and high-temperature plasticity of steel. Moreover, the existing method has poor stability, and the carbon emissions during the electric furnace smelting process are relatively high. high.
An electric furnace is used for raw material melting and decarburization and dephosphorization. Oxygen and carbon powder are sprayed through a spray gun. The molten steel is then sent to the RH refining furnace for deep decarburization and nitrogen vacuum refining. Powder spraying technology is used until the carbon content in the molten steel is ≤0.05wt%. , the nitrogen content is ≤0.04wt%, and the content is further reduced by vacuum refining.
It achieves stable control of carbon and nitrogen content in molten steel below 0.003wt%, reduces carbon emissions, improves production stability, and is suitable for the production of high-grade ultra-low carbon nitrogen steel.
Smart Images

Figure CN115927788B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of steelmaking, and in particular to an ultra-low carbon-nitrogen molten steel and a smelting method thereof. Background Art
[0002] Generally, nitrogen exists as an impurity element in steel, and its content affects the high-temperature strength and high-temperature plasticity of steel, and nitrogen will reduce the deep drawing performance of steel. Many high-grade thin plates or thick steel plates have stringent requirements on the carbon content and nitrogen content in steel, usually requiring the finished carbon content in steel to be controlled below 50ppm and the nitrogen content to be controlled below 40ppm; some varieties, such as high-grade automotive plates, silicon steel and other products, have lower requirements for carbon content and nitrogen content, even below 30ppm. Generally, a converter is used as a roughing furnace to produce the above-mentioned steel varieties, but because the electric furnace uses scrap steel as raw material, the nitrogen content in the molten steel at the end of the smelting process is generally 70-120ppm due to the ionization effect of the arc. In the prior art, the denitrification effect is usually ensured by controlling the nitrogen content in the raw material or by applying the electric furnace electromotive force between the molten iron and the slag to make the carbon boil and promote deep decarburization to denitrify and further increase the vacuum treatment, but the stability is poor. For example, the patent document with application number CN201810580268.5 discloses a method for smelting low-nitrogen steel in an electric furnace, which uses EAF furnace primary smelting + LF furnace refining + VD furnace vacuum smelting and continuous casting pouring process to reduce the nitrogen content in the finished steel (nitrogen content ≤ 0.0040% or 40ppm). However, in the EAF furnace primary smelting process, this method needs to add molten iron (the amount of molten iron added is 35-55%), which is not conducive to reducing carbon emissions. For example, the patent document with application number CN201811132581.9 discloses a method for efficiently smelting low-nitrogen steel using an electric furnace, which uses a double-shell electric furnace with two furnace shells for smelting, and uses the arc power supply system of the double-shell electric furnace to alternately power and heat the two furnace shells, wherein when powering and heating one of the two furnace shells, the other furnace shell is sequentially performed in the following steps: charging, molten pool sealing, and spraying combustion medium and oxygen to start smelting. This method uses two power supply systems, which are essentially two electric furnaces and are relatively expensive. It uses hollow electrodes to blow argon to avoid nitrogen in the furnace, but because the electric furnace itself is not a completely closed system, nitrogen will still be inhaled from the furnace door and the four holes in the furnace cover and then enter the molten steel, resulting in a higher nitrogen content in the finished steel. Summary of the invention
[0003] In view of the above-mentioned shortcomings of the prior art, the present application provides an ultra-low carbon and nitrogen molten steel and a smelting method thereof to reduce the carbon content and nitrogen content in the obtained finished molten steel and improve production stability.
[0004] In order to achieve the above-mentioned invention object, the technical solution of this application is as follows:
[0005] In a first aspect, the present application provides a method for smelting ultra-low carbon nitrogen molten steel, comprising the following steps:
[0006] The raw materials are placed in an electric furnace, and spray guns are arranged on the furnace wall and the furnace door of the electric furnace, wherein 2≤the number of spray guns located on the furnace wall of the electric furnace≤6, and the raw materials are sequentially processed through the charge melting stage, the decarburization and dephosphorization stage, and the powder spraying and decarbonization and denitrification stage until the oxygen content of the molten steel is ≥600ppm, and then the molten steel is sent to the RH refining furnace for deep decarburization and denitrification vacuum refining to obtain the ultra-low carbon and nitrogen molten steel, wherein the powder spraying and decarbonization and denitrification stage includes: using a plurality of spray guns on the furnace wall of the electric furnace to spray the molten steel at the same time until the carbon content of the molten steel is ≤0.05wt%, and the nitrogen content is ≤0.04wt%.
[0007] Optionally, the spray gun is a double-channel spray gun.
[0008] Optionally, during the charge melting stage, the spray gun is used to spray ≤2500m 3 / h of oxygen.
[0009] Optionally, during the decarburization and dephosphorization stage, the spray gun is used to simultaneously spray oxygen and carbon powder.
[0010] Optionally, during the decarburization and dephosphorization stage, the oxygen flow rate is ≤3000m 3 / h, the flow rate of carbon powder ≤40kg / min.
[0011] Optionally, in the decarburization and dephosphorization stage, the carbon content in the molten steel is treated to be ≤0.10wt%-0.15wt%.
[0012] Optionally, in the powder spraying and decarbonization and denitrification stage, an inert gas and a metal oxide powder are sprayed simultaneously by a spray gun.
[0013] Optionally, in the powder spraying and decarbonizing and denitrifying stage, the flow rate of the inert gas is ≤3000m3 / h, and the flow rate of the metal oxide powder is ≤40kg / min.
[0014] Optionally, the particle size of the metal oxide powder is ≤0.1 mm.
[0015] In a second aspect, the present application also provides an ultra-low carbon nitrogen molten steel smelted according to the smelting method as described above.
[0016] The ultra-low carbon nitrogen molten steel and smelting method thereof of the present application have the following beneficial effects:
[0017] The present application uses an electric furnace as a roughing furnace and an RH refining furnace as a vacuum refining furnace. Through the stages of raw material charging, charge melting, decarburization and dephosphorization, powder spraying deep decarburization and nitrogen removal, and vacuum refining, the carbon and nitrogen contents in the finished molten steel can be stably controlled to be below 0.003wt%.
[0018] The process flow of this application is short and compact, and can stably control the carbon content and nitrogen content in molten steel at a low level, which is conducive to the production of high-grade ultra-low carbon and nitrogen steel.
[0019] By adopting the method of the present application for smelting, no molten iron is needed in the electric furnace smelting process, which is conducive to reducing carbon emissions and promoting the production and application of low-carbon green steel products. It should be understood that the above general description and the detailed description below are only exemplary and explanatory and cannot limit the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The drawings herein are incorporated into the specification and constitute a part of the specification, showing embodiments consistent with the present application, and together with the specification, are used to explain the principles of the present application. Obviously, the drawings described below are only some embodiments of the present application, and for those of ordinary skill in the art, other drawings can be obtained based on these drawings without creative work. In the drawings:
[0021] Figure 1 This is a flow chart of the smelting method of ultra-low carbon nitrogen molten steel in Example 1. DETAILED DESCRIPTION
[0022] The following will refer to the accompanying drawings and preferred embodiments to illustrate the embodiments of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways according to different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention, not for limiting the scope of protection of the present invention. Unless otherwise specified, "wt%" refers to the mass percentage.
[0023] The present application provides a method for smelting ultra-low carbon nitrogen molten steel, comprising the following steps:
[0024] The raw materials are placed in an electric furnace with double-flow spray guns on the furnace wall and the furnace door, wherein 2≤the number of spray guns on the furnace wall≤6, and processed in sequence through the charge melting stage, the decarburization and dephosphorization stage, and the powder spraying and decarburization and denitrification stage until the oxygen content of the molten steel is ≥600ppm, and then the molten steel is sent to the RH refining furnace for deep decarburization and denitrification vacuum refining to obtain ultra-low carbon and nitrogen molten steel.
[0025] In the melting stage of the charge, a double-channel spray gun is used to spray ≤2500m 3 / h of oxygen;
[0026] In the decarburization and dephosphorization stage, a dual-channel spray gun is used to spray oxygen and carbon powder simultaneously, where the oxygen flow rate is ≤3000m 3 / h, the flow rate of carbon powder ≤40kg / min, until the carbon content in molten steel ≤0.10wt%-0.15wt%;
[0027] The powder spraying and decarbonization stage includes: using a double-channel spray gun located on the furnace wall of the electric furnace to simultaneously spray inert gas and metal oxide powder with a particle size of ≤0.1mm to the molten steel, wherein the flow rate of the inert gas is ≤3000m 3 / h, the flow rate of metal oxide powder is ≤40kg / min, until the carbon content in the molten steel is ≤0.05wt%, and the nitrogen content is ≤0.04wt%.
[0028] In a second aspect, the present application also provides an ultra-low carbon nitrogen molten steel smelted according to the smelting method as described above.
[0029] The scheme of the present invention is illustrated by specific embodiments below. It should also be understood that the following embodiments are only used to specifically illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values exemplified below.
[0030] Example 1
[0031] A smelting method for ultra-low carbon nitrogen molten steel, the specific steps are as follows:
[0032] Raw material charging: The raw materials (specifically, solid iron-containing raw materials such as scrap steel and metallized pellets) are placed in a 150t electric furnace with one double-flow channel spray gun at the furnace door and three double-flow channel spray guns at the furnace wall;
[0033] Charge melting stage: The electrode is lowered to melt the raw materials. The first stage oxygen supply operation is performed by changing the gear of the transformer electrically connected to the electric furnace and using the double-flow spray gun at the furnace wall and the furnace door to control the melting process and obtain molten steel. Specifically, oxygen is sprayed through the double-flow spray gun at the furnace wall and the furnace door. The spray flow rate of the double-flow spray gun at the furnace door is 1800m 3 / h of oxygen, using a double-channel spray gun at the furnace wall with a spray flow rate of 1800m 3 / h of oxygen;
[0034] Decarburization and dephosphorization stage: The second stage oxygen supply operation is carried out through the double-flow spray gun at the furnace wall and the furnace door until the carbon content in the molten steel is 0.10wt%. Specifically, the blowing flow rate through the double-flow spray gun at the furnace door is 2200m 3 / h of oxygen, through the double-channel spray gun at the furnace wall, with a flow rate of 2200m3 / h of oxygen and 25kg / min of carbon powder. After testing, the carbon content in the molten steel after treatment by this process is 0.10wt% and the phosphorus content is 0.015wt%;
[0035] Powder spraying and decarbonization stage: The double-channel spray gun on the furnace wall simultaneously sprays the molten steel with a flow rate of 2500m 3 / h of argon and a metal oxide powder with a particle size of ≤0.1mm (specifically, the main components are iron ore powder, manganese ore powder and manganese oxide) with a flow rate of 20kg / min, until the carbon content in the molten steel is 0.045wt% (detected in accordance with "GB / T 223.86-2009 Determination of total carbon content of steel and alloys", the same below), and the nitrogen content is 0.028wt% (detected in accordance with "GB / T223.37-2020 Determination of nitrogen content in steel and alloys - Distillation separation indigo blue spectrophotometry", the same below), stop powder spraying, wait until the oxygen content in the molten steel is 680ppm, and then tap without deoxidation to enter the next stage. At this time, the nitrogen content in the molten steel is 0.041wt%;
[0036] Vacuum smelting: The molten steel is sent to the RH refining furnace for vacuum refining. The RH refining furnace is treated according to the ultra-low carbon treatment mode to obtain ultra-low carbon and nitrogen molten steel.
[0037] Five batches were smelted according to the method of this embodiment, and the carbon content and nitrogen content of the molten steel obtained from different batches were detected. The results are shown in Table 1, wherein the nitrogen content was detected in accordance with "GB / T 223.37-2020 Determination of Nitrogen Content of Steel and Alloy-Indigo Blue Spectrophotometric Method for Distillation Separation", and the carbon content was detected in accordance with "GB / T 223.86-2009 Determination of Total Carbon Content of Steel and Alloy".
[0038] Table 1 Test results
[0039] source Nitrogen content Carbon content Batch 1# 0.0027wt% 0.0022wt% Batch 2# 0.0028wt% 0.0021wt% Batch 3# 0.0030wt% 0.0020wt% Batch 4# 0.0028wt% 0.0022wt% Batch 5# 0.0029wt% 0.0020wt%
[0040] It can be seen from Table 1 that the carbon content and nitrogen content in the molten steel obtained from batches 1#-5# are both ≤0.003wt%. This result shows that the present application uses an electric furnace as a roughing furnace and an RH refining furnace as a vacuum refining furnace, and through raw material charging, charge melting, decarburization and dephosphorization, powder spraying deep decarburization and nitrogen removal, vacuum refining and other stages, the carbon content and nitrogen content can be stably controlled to be below 0.003wt%.
[0041] The above embodiments are merely illustrative of the principles and effects of the present invention, and are not intended to limit the present invention. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by a person of ordinary skill in the art without departing from the spirit and technical ideas disclosed by the present invention shall still be covered by the claims of the present invention.
Claims
1. A method for smelting ultra-low carbon nitrogen molten steel, characterized in that: The following steps are involved: The raw materials are placed in an electric furnace, wherein the furnace wall and the furnace door of the electric furnace are both provided with spray guns, wherein 2≤the number of spray guns located on the furnace wall of the electric furnace≤6, and the raw materials are sequentially processed through the furnace charge melting stage, the decarburization and dephosphorization stage, and the powder spraying and decarburization and denitrification stage until the oxygen content of the molten steel is ≥600ppm, and then the molten steel is sent to the RH refining furnace for deep decarburization and denitrification vacuum refining to obtain the ultra-low carbon and nitrogen molten steel, wherein the powder spraying and decarburization and denitrification stage includes: using a plurality of spray guns located on the furnace wall of the electric furnace to spray the molten steel at the same time until the carbon content in the molten steel is ≤0.05wt% and the nitrogen content is ≤0.04wt%; The spray gun adopts a double-flow channel spray gun; During the melting stage of the furnace charge, the spray gun is used to spray ≤2500m 3 / h of oxygen; In the decarburization and dephosphorization stage, the spray gun is used to simultaneously spray with a flow rate of ≤3000m 3 / h of oxygen and carbon powder with a flow rate of ≤40kg / min, to treat the molten steel until the carbon content is ≤0.10wt%; In the powder spraying decarbonization and nitrogen removal stage, the spray gun is used to simultaneously spray with a flow rate of ≤3000m 3 / h of inert gas and metal oxide powder with a flow rate of ≤40kg / min.
2. The method for smelting ultra-low carbon nitrogen molten steel according to claim 1, characterized in that: The particle size of the metal oxide powder is ≤0.1 mm.
3. An ultra-low carbon nitrogen molten steel obtained by the smelting method according to claim 1 or 2.
Citation Information
Cited By
Nitrogen-dominated bake-hardened ultralow-carbon steel for automobile outer plate and manufacturing method of nitrogen-dominated bake-hardened ultralow-carbon steel
CN121896543A