Preparation method of ultrahigh-conductivity electrode flat steel
Through the converter semi-steel smelting, LF electric heating refining, RH vacuum treatment and billet continuous casting, combined with dynamic matching casting speed and electromagnetic stirring, the problem of high resistivity of traditional cathode flat steel is successfully solved, and ultra-high conductive electrodes are achieved The high-quality production of flat steel improves the energy efficiency of aluminum electrolytic production.
Patent Information
- Application Number
- CN202411330886.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-15
AI Technical Summary
In the aluminum electrolysis production process, traditional cathode flat steel has a high resistivity leading to low power utilization efficiency. How to produce high-quality ultra-high conductive electrode flat steel to reduce energy consumption and improve production efficiency has become a research hotspot.
By controlling the oxygen activity of the steel liquid, the standstill time, the dynamic matching casting speed and electromagnetic stirring process during the casting process, the casting speed and electromagnetic stirring process are used. , realize precise regulation of cast billet solidification of ultra-high conductive electrode flat steel, reduce resistivity, and improve cast billet quality and rolling performance.
It realizes high-quality stable continuous casting of ultra-high conductive electrode flat steel, reduces the upward impact of deoxygenation products, improves the accuracy of solidification heat transfer, ensures that the resistivity meets the standard requirements, and improves the energy efficiency of aluminum electrolytic production.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of steel smelting, and in particular relates to a method for preparing ultra-high conductive electrode flat steel. Background Art
[0002] In the production process of aluminum, electrolytic preparation is the main aluminum production process in my country, and a large amount of electricity is consumed in its production process. As a result, electrolytic aluminum is one of the high-energy-consuming basic industries in my country's industrial production, and electricity costs occupy a dominant position, accounting for more than 40%. At present, the average direct electricity consumption per ton of aluminum in my country is about 13,000 KWh, while the theoretical direct electricity consumption per ton of aluminum is about 6,300 kWh, and the electricity utilization rate is about 48%, with a large space for energy saving and consumption reduction. Under the background of "dual carbon", energy saving and consumption reduction in aluminum production will play a leading role. Cathode flat steel, as an important component of the electrolytic cell in the production process of aluminum electrolysis, is generally used as the cathode of the electrolytic cell, which can play a role in evenly dividing the current and improving the current in the aluminum liquid. The quality of the electrode flat steel directly affects the production quality and energy consumption of aluminum electrolysis. Among them, the resistivity of the electrode flat steel is a key factor. The electrode flat steel with low resistivity can reduce the heat generation in the conductive process and improve the efficiency of electricity utilization.
[0003] The resistivity of electrode flat steel for electrolytic aluminum is mainly affected by internal factors such as chemical composition, purity, and organizational structure of the flat steel. With the continuous improvement of energy-saving and consumption-reducing requirements, traditional Q235A / B and Q195A / B cathode flat steels are gradually being eliminated and replaced by high-conductivity and ultra-high-conductivity electrode flat steels with lower resistivity.
[0004] How to produce high-quality ultra-high conductive electrode flat steel has become a hot research topic in this field. Summary of the invention
[0005] In view of this, the purpose of the present invention is to provide a method for preparing ultra-high conductivity electrode flat steel, which achieves precise control of the solidification of the ultra-high conductivity electrode flat steel ingot, the ingot has good low-multiple quality, and the flat steel obtained by rolling has good performance.
[0006] The present invention provides a method for preparing ultra-high conductive electrode flat steel, comprising the following steps:
[0007] The converter semi-steel smelting, LF electric heating refining, RH vacuum treatment, billet continuous casting, stacking slow cooling and rolling are carried out in sequence to obtain ultra-high conductive electrode flat steel;
[0008] The a[O] in the molten steel after the RH vacuum treatment is controlled at 20-30 ppm, and the contents of other chemical components meet the requirements of the finished product;
[0009] The molten steel after the RH vacuum treatment is sent to the continuous casting platform of the billet continuous casting and then allowed to stand for 8 to 10 minutes;
[0010] The cross-sectional size of the billet continuously cast is (300-400) mm×(400-500) mm;
[0011] The billet continuous casting adopts straight-through long nozzle casting, the inner diameter of the nozzle is 50-70mm, the superheat of the molten steel in the casting process is controlled at 20-40℃ as a whole, and the casting speed and electromagnetic stirring process are dynamically matched. The specific rules are: when the superheat is 20-25℃, the continuous casting speed is matched to 2.5t / min, the current intensity of the electromagnetic stirring of the crystallizer is 400-500A, the current frequency is 2.6-3.0Hz, and the current intensity of the electromagnetic stirring at the end of solidification is 0-50A, and the current frequency is 0-6.5Hz; when the superheat is 26-35℃, the continuous casting speed is matched to 2. 3~2.4t / min, the current intensity of electromagnetic stirring of the crystallizer is 400~500A, the current frequency is 2.6~3.0Hz, the current intensity of electromagnetic stirring at the end of solidification is 60~100A, the current frequency is 5.5~6.5Hz; when the superheat is 36~40℃, the matching continuous casting speed is 2.1~2.2t / min, the current intensity of electromagnetic stirring of the crystallizer is 400~500A, the current frequency is 2.6~3.0Hz, the current intensity of electromagnetic stirring at the end of solidification is 110~150A, the current frequency is 5.5~6.5Hz;
[0012] During the continuous casting of the billet, the secondary cooling adopts medium-strength cooling, and the specific water volume is 0.31-0.35L / kg 钢 .
[0013] Preferably, the cross-sectional dimensions of the billet are 320 mm×410 mm or 360 mm×450 mm.
[0014] Preferably, the chemical composition of the ultra-high conductive electrode flat steel includes: C≤0.008wt%, Si≤0.015wt%, Mn≤0.030wt%, P≤0.012wt%, S≤0.007wt%, and the balance is Fe.
[0015] Preferably, the endpoint C content of the converter semi-steel smelting is ≤0.030wt%, and the tapping temperature is ≥1650°C.
[0016] Preferably, the LF electric heating refining is carried out with argon blowing and stirring throughout the whole process, and the temperature at the end of refining is controlled at 1630-1650°C.
[0017] Preferably, the circulating gas flow rate of the RH vacuum treatment is 1000-1400 NL / min, the vacuum treatment time is ≥12 min, and the vacuum treatment end temperature is controlled at 1600-1610° C.
[0018] Preferably, the surface temperature of the blank when the stacking slow cooling is started is greater than 600° C., and the slow cooling time is greater than or equal to 18 hours.
[0019] Preferably, the temperature of the casting during the rolling is 1000±20°C.
[0020] Compared with the prior art, the present invention provides a method for preparing ultra-high conductive electrode flat steel. The method provided by the present invention comprises the following steps: sequentially carrying out converter semi-steel smelting, LF electric heating refining, RH vacuum treatment, billet continuous casting, stacking slow cooling and rolling to obtain ultra-high conductive electrode flat steel; a[O] in the molten steel after the RH vacuum treatment is controlled at 20-30ppm, and the contents of other chemical components meet the requirements of the finished product; the molten steel after the RH vacuum treatment is sent to a continuous casting platform for billet continuous casting and then allowed to stand for 8-10min; the cross-sectional size of the billet continuous casting is (300-400)mm×(400-500)mm; the billet continuous casting adopts straight-through long nozzle casting, the inner diameter of the nozzle is 50-70mm, the superheat of the molten steel in the casting process is controlled at 20-40°C as a whole, the casting speed and the electromagnetic stirring process are dynamically matched, and the specific rules are: when the superheat is 20-25°C, the continuous casting pulling speed is matched to 2.5t / min, and the electromagnetic stirring of the crystallizer is The current intensity is 400-500A, the current frequency is 2.6-3.0Hz, the current intensity of electromagnetic stirring at the end of solidification is 0-50A, and the current frequency is 0-6.5Hz; when the superheat is 26-35°C, the continuous casting pulling speed is matched to 2.3-2.4t / min, the current intensity of electromagnetic stirring of the crystallizer is 400-500A, the current frequency is 2.6-3.0Hz, and the current intensity of electromagnetic stirring at the end of solidification is 60-100A, and the current frequency is 5.5-6.5Hz; when the superheat is 36-40°C, the continuous casting pulling speed is matched to 2.1-2.2t / min, the current intensity of electromagnetic stirring of the crystallizer is 400-500A, the current frequency is 2.6-3.0Hz, and the current intensity of electromagnetic stirring at the end of solidification is 110-150A, and the current frequency is 5.5-6.5Hz; during the continuous casting of the square billet, the secondary cooling adopts medium-strength cooling, and the specific water volume is 0.31-0.35L / kg 钢 . The method provided by the present invention successfully realizes high-quality and stable continuous casting of ultra-high conductive electrode flat steel billets. Among them, through sufficient standing, the floating removal of deoxidation products is more thorough, and the negative impact of nozzle nodules in continuous casting of billets with smaller cross-sectional sizes than slabs is greatly reduced; more importantly, according to the highly sensitive characteristics of solidification heat transfer, precise dynamic process matching is formulated, and the precise adjustment of the superheat of the casting steel liquid, combined electromagnetic stirring and casting speed, as well as the precise control of the secondary cooling intensity, is achieved. The precise control of the solidification of the ultra-high conductive electrode flat steel billet is achieved, the billet has good low-multiple quality, and the various properties of the flat steel obtained by rolling meet the standard requirements well, among which 100% of the key indicator of resistivity meets the standard requirements. DETAILED DESCRIPTION
[0021] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0022] The present invention provides a method for preparing ultra-high conductive electrode flat steel, comprising the following steps:
[0023] The converter semi-steel smelting, LF electric heating refining, RH vacuum treatment, billet continuous casting, stacking slow cooling and rolling are carried out in sequence to obtain ultra-high conductive electrode flat steel.
[0024] In the preparation method provided by the present invention, the endpoint C content of the converter semi-steel smelting is preferably ≤0.030wt%; the steel tapping temperature of the converter semi-steel smelting is preferably ≥1650°C; during the converter semi-steel smelting process, alloys are added according to the target alloy and content in the steel, and active lime is preferably added in a quantitative manner.
[0025] In the preparation method provided by the present invention, a certain amount of slag is added during the LF electric heating refining process; the LF electric heating refining is preferably carried out with argon blowing and stirring throughout the process, and the steel liquid surface is strictly prohibited from violently churning during the argon blowing process; the temperature at the end of the LF electric heating refining is preferably controlled at 1630-1650°C.
[0026] In the preparation method provided by the present invention, the circulating gas flow rate of the RH vacuum treatment is preferably 1000-1400NL / min; the time of the RH vacuum treatment is preferably ≥12min; and the end temperature of the RH vacuum treatment is preferably controlled at 1600-1610°C.
[0027] In the preparation method provided by the present invention, a[O] (oxygen activity - oxygen in the steel liquid consists of two parts, one part is oxide, i.e., non-metallic inclusions, and the other part is free oxygen, represented by a[O]) in the steel liquid after the RH vacuum treatment is controlled at 20 to 30 ppm, specifically 20 ppm, 21 ppm, 22 ppm, 23 ppm, 24 ppm, 25 ppm, 26 ppm, 27 ppm, 28 ppm, 29 ppm or 30 ppm; the contents of other chemical components meet the requirements of the finished product.
[0028] In the preparation method provided by the present invention, the molten steel after RH vacuum treatment is sent to the continuous casting platform for continuous casting of square billets and then allowed to stand for a period of preferably 8 to 10 minutes, specifically 8 minutes, 8.5 minutes, 9 minutes, 9.5 minutes or 10 minutes.
[0029] In the preparation method provided by the present invention, the cross-sectional size of the square billet continuously cast is (300-400) mm×(400-500) mm; wherein the short side size can be specifically 300 mm, 310 mm, 320 mm, 330 mm, 340 mm, 350 mm, 360 mm, 370 mm, 380 mm, 390 mm or 400 mm, and the long side size can be specifically 400 mm, 410 mm, 420 mm, 430 mm, 440 mm, 450 mm, 460 mm, 470 mm, 480 mm, 490 mm or 500 mm.
[0030] In the preparation method provided by the present invention, the continuous casting of the square billet adopts straight-through long nozzle casting, and the inner diameter of the nozzle is 50-70 mm, specifically 50 mm, 55 mm, 60 mm, 65 mm or 70 mm.
[0031] In the preparation method provided by the present invention, during the continuous casting of the square billet, the superheat of the molten steel in the casting process is controlled at 20-40°C as a whole, and the casting speed and the electromagnetic stirring process are dynamically matched. The specific rules are: when the superheat is 20-25°C, the continuous casting pulling speed is matched to 2.5t / min, the current intensity of the electromagnetic stirring of the crystallizer is 400-500A, specifically 400A, 410A, 420A, 430A, 440A, 450A, 460A, 470A, 480A, 490A or 500A, the current frequency of the electromagnetic stirring of the crystallizer is 2.6-3.0Hz, specifically 2.6Hz, 2.7Hz, 2.8Hz, 2.9Hz or 3.0Hz, the current intensity of the electromagnetic stirring at the end of solidification is 0-50A, specifically The current frequency at the end of solidification is 0A, 5A, 10A, 15A, 20A, 25A, 30A, 35A, 40A, 45A or 50A, the current frequency at the end of solidification is 0-6.5Hz, specifically 0Hz, 0.5Hz, 1Hz, 1.5Hz, 2Hz, 2.5Hz, 3Hz, 3.5Hz, 4Hz, 4.5Hz, 5Hz, 5.5Hz, 6Hz or 6.5Hz; when the superheat is 26-35℃, the continuous casting speed is matched to 2.3-2.4t / min, the current intensity of the electromagnetic stirring of the crystallizer is 400-500A, specifically 400A, 410A, 420A, 430A, 440A, 450A, 460A, 470A, 480A, 490A or 500A, and the electromagnetic stirring of the crystallizer is The current frequency of electromagnetic stirring at the end of solidification is 2.6-3.0Hz, specifically 2.6Hz, 2.7Hz, 2.8Hz, 2.9Hz or 3.0Hz, the current intensity of electromagnetic stirring at the end of solidification is 60-100A, specifically 60A, 65A, 70A, 75A, 80A, 85A, 90A, 95A or 100A, the current frequency of electromagnetic stirring at the end of solidification is 5.5-6.5Hz, specifically 5.5Hz, 5.6Hz, 5.7Hz, 5.8Hz, 5.9Hz, 6.0Hz, 6.1Hz, 6.2Hz, 6.3Hz, 6.4Hz or 6.5Hz; when the superheat is 36-40℃, the continuous casting speed is matched to 2.1-2.2t / min, and the current intensity of electromagnetic stirring of the crystallizer is 400 The current frequency of electromagnetic stirring of the crystallizer is 2.6-3.0 Hz, specifically 2.6 Hz, 2.7 Hz, 2.8 Hz, 2.9 Hz or 3.0 Hz. The current intensity of electromagnetic stirring at the end of solidification is 110-150 A, specifically 110 A, 115 A, 120 A, 125 A, 130 A, 135 A, 140 A, 145 A or 150 A. The current frequency of electromagnetic stirring at the end of solidification is 5.5-6.5 Hz, specifically 5.5 Hz, 5.6 Hz, 5.7 Hz, 5.8 Hz, 5.9 Hz, 6.0Hz, 6.1Hz, 6.2Hz, 6.3Hz, 6.4Hz or 6.5Hz. .
[0032] In the preparation method provided by the present invention, during the continuous casting of the square billet, the secondary cooling adopts medium-strong cooling, and the specific water volume is 0.31-0.35 L / kg. 钢 , specifically 0.31L / kg 钢 , 0.32L / kg 钢 、0.33L / kg 钢 、0.34L / kg 钢 or 0.35L / kg 钢 .
[0033] In the preparation method provided by the present invention, the surface temperature of the blank when the stacking slow cooling is started is preferably greater than 600° C.; and the time of the stacking slow cooling is preferably ≥18 h.
[0034] In the preparation method provided by the present invention, the temperature of the casting during the rolling is preferably 1000±20°C.
[0035] In the preparation method provided by the present invention, the chemical composition of the ultra-high conductive electrode flat steel includes: C≤0.008wt%, Si≤0.015wt%, Mn≤0.030wt%, P≤0.012wt%, S≤0.007wt%, and the balance Fe and other inevitable impurities.
[0036] The method provided by the present invention successfully realizes high-quality and stable continuous casting of ultra-high conductive electrode flat steel billets. Among them, by fully standing, the deoxidation products are more thoroughly removed by floating, and the negative impact of the continuous casting nozzle nodules of billets with smaller cross-sectional sizes than slabs is greatly reduced; more importantly, according to the highly sensitive characteristics of solidification heat transfer, accurate dynamic process matching is formulated, and the precise adjustment of the superheat of the casting steel liquid, combined electromagnetic stirring and casting speed, as well as the precise control of the secondary cooling intensity, is achieved. The solidification of the ultra-high conductive electrode flat steel billet is precisely controlled, the billet has good low-multiple quality, and the various properties of the flat steel obtained by rolling meet the standard requirements well, among which 100% of the key indicator of resistivity meets the standard requirements.
[0037] For the purpose of greater clarity, the invention is described in detail through the following examples.
[0038] Example 1
[0039] This embodiment is that a certain enterprise adopts the method of the present invention to produce HYT2 ultra-high conductivity electrode flat steel billet continuous casting, and the continuous casting section size is 320mm×410mm. The process technology flow is: converter semi-steel smelting - LF electric heating refining - RH vacuum treatment - large square billet (section size: 320mm×410mm) continuous casting - stacking slow cooling - rolling.
[0040] The key technical parameters involved in this embodiment are actually implemented as follows:
[0041] (1) The content of a[O] in the molten steel after RH vacuum treatment is controlled at 20-25 ppm, and the content of other chemical components meets the requirements of the finished product; (2) Furthermore, the molten steel after RH exits the station is placed on the continuous casting platform for 8-9 minutes; (3) A straight-through long nozzle is used for casting, and the inner diameter of the nozzle is 50-52 mm; (4) The superheat of the molten steel during the casting process is controlled at 20-40°C as a whole; the casting speed and electromagnetic stirring process are dynamically matched: the superheat is 20-25°C, the continuous casting speed is matched to 2.5 t / min, the current intensity of the electromagnetic stirring of the crystallizer is 470-500A, the current frequency is 2.6 Hz, and the current intensity of the electromagnetic stirring at the end of solidification is 50A, current frequency 5.5Hz; superheat 26~35℃, matching continuous casting speed 2.3~2.4t / min, current intensity of electromagnetic stirring of crystallizer 470~500A, current frequency 2.8Hz, current intensity of electromagnetic stirring at the end of solidification 100A, current frequency 6.0Hz; superheat 36~40℃, matching continuous casting speed 2.1~2.2t / min, current intensity of electromagnetic stirring of crystallizer 470~500A, current frequency 3.0Hz, current intensity of electromagnetic stirring at the end of solidification 150A, current frequency 6.5Hz; secondary cooling adopts medium-strong cooling, specific water volume 0.33~0.35L / kg 钢 .
[0042] The above-mentioned continuous casting process includes the following as a whole according to the flow direction of the molten steel: the ladle filled with molten steel is suspended on the continuous casting turntable and allowed to stand still, and after the casting of the previous furnace is completed, it is rotated to the casting position, a long water nozzle is installed on the ladle outlet, and the outlet slide device is started to allow the molten steel to flow from the bottom of the ladle through the long water nozzle into the impact zone of the tundish, and the molten steel in the impact zone enters the injection zone after the tundish retaining wall stabilizes the flow, and the molten steel in the injection zone enters the crystallizer from the immersed water nozzle of each continuous casting flow to start the solidification process. In the crystallizer, the molten steel quickly forms a solidified billet shell under the action of quenching, and as the billet leaves the crystallizer, the billet shell continuously advances toward the center of the billet under the action of secondary cooling to achieve the advancement of the solidification front. In the process of advancing the solidification front, due to the heat transfer and solidification characteristics of this type of steel, its columnar crystals are very easy to develop, and the tendency of intercrystalline cracks is serious. The solidification structure evolution is regulated by implementing a suitable secondary cooling intensity (provided by the present invention) and matching it with an appropriate electromagnetic stirring process, thereby achieving high-quality billet continuous casting production.
[0043] In addition to the above key technical points that must be implemented as required, this embodiment requires other continuous casting system processes and other process processes to be implemented in coordination with conventional operations, for example:
[0044] Converter semi-steel smelting: end point C≤0.030%, steel tapping temperature≥1650℃, alloy is added according to the target alloy and content in the steel, and 400kg of active lime is added quantitatively; LF electric heating refining: 1100kg of slag is added, argon is blown and stirred throughout the process, and the steel liquid surface is strictly prohibited from violent churning during the argon blowing process, and the temperature at the end of LF is controlled at 1630-1650℃; RH vacuum treatment: circulating gas flow rate 1000-1400NL / min, vacuum treatment ≥12min, and vacuum end temperature is controlled at 1600-1610℃; stacking slow cooling: stacking slow cooling is started when the billet surface temperature is>600℃, and the slow cooling time is ≥18h; rolling: the billet is heated to 1000±20℃ for rolling.
[0045] The 320mm×410mm cross-section HYT2 ultra-high conductivity electrode flat steel ingot obtained by the test was pickled and tested at low magnification. The results showed that the ingot had good low-magnification quality, with a loose center of 0.5 grade, no middle cracks, no subcutaneous bubbles, and a center segregation of 0.5 grade. The resistivity of the rolled flat steel at 20°C was 10.5μΩ·cm (the standard requirement is ≤13μΩ·cm).
[0046] Example 2
[0047] This embodiment is that a certain enterprise adopts the method of the present invention to carry out continuous casting production of HYT2 ultra-high conductivity electrode flat steel billet, and the continuous casting section size is 360mm×450mm. The process technology flow is: converter semi-steel smelting - LF electric heating refining - RH vacuum treatment - large square billet (section size: 360mm×450mm) continuous casting - stacking slow cooling - rolling.
[0048] The key technical parameters involved in this embodiment are actually implemented as follows:
[0049] (1) a[O] in the molten steel after RH vacuum treatment is controlled at 25-30 ppm, and the contents of other chemical components meet the requirements of the finished product; (2) Furthermore, the molten steel after RH exits the station is placed on the continuous casting platform for 9-10 min; (3) A straight-through long nozzle is used for casting, with an inner diameter of 66-70 mm; (4) The superheat of the molten steel during the casting process is controlled at 20-40°C as a whole; the casting speed and electromagnetic stirring process are dynamically matched: the superheat is 20-25°C, the continuous casting speed is matched to 2.5 t / min, the current intensity of the electromagnetic stirring of the crystallizer is 400-450A, the current frequency is 2.6 Hz, and the electromagnetic stirring at the end of solidification is Current intensity 0A, current frequency 0Hz; superheat 26~35℃, matching continuous casting speed 2.3~2.4t / min, current intensity of electromagnetic stirring of crystallizer 400~450A, current frequency 2.8Hz, current intensity of electromagnetic stirring at the end of solidification 60A, current frequency 5.5Hz; superheat 36~40℃, matching continuous casting speed 2.1~2.2t / min, current intensity of electromagnetic stirring of crystallizer 400~450A, current frequency 3.0Hz, current intensity of electromagnetic stirring at the end of solidification 110A, current frequency 6.5Hz; secondary cooling adopts medium-strength cooling, specific water volume 0.31~0.32L / kg 钢 .
[0050] In this embodiment, except that the above-mentioned key technical points must be implemented as required, other continuous casting system processes and other process processes need to be implemented in coordination with conventional operations. For details, please refer to Example 1.
[0051] The 360mm×450mm cross-section HYT2 ultra-high conductivity electrode flat steel ingot obtained from the test was subjected to pickling low-power detection. The results showed that the low-power quality of the ingot was good, with the center of the ingot being loose at level 0.5, no intermediate cracks, no subcutaneous bubbles, and the center segregation at level 0.5 accounting for 97%. The resistivity of the rolled flat steel at 20°C was 10.1-10.4μΩ·cm (the standard requirement is ≤13μΩ·cm).
[0052] Example 3
[0053] This embodiment is that a certain enterprise adopts the method of the present invention to produce HYT2 ultra-high conductivity electrode flat steel billet continuous casting, and the continuous casting section size is 320mm×410mm. The process technology flow is: converter semi-steel smelting - LF electric heating refining - RH vacuum treatment - large square billet (section size: 320mm×410mm) continuous casting - stacking slow cooling - rolling.
[0054] The key technical parameters involved in this embodiment are actually implemented as follows:
[0055] (1) The content of a[O] in the molten steel after RH vacuum treatment is controlled at 24-27 ppm, and the content of other chemical components meets the requirements of the finished product; (2) Furthermore, the molten steel after RH exits the station is placed on the continuous casting platform for 8-10 min; (3) A straight-through long nozzle is used for casting, and the inner diameter of the nozzle is 55-57 mm; (4) The superheat of the molten steel during the casting process is controlled at 20-40°C as a whole; Dynamic matching of casting speed and electromagnetic stirring process: superheat 20-25°C, matching continuous casting speed 2.5 t / min, current intensity of electromagnetic stirring of the crystallizer 470-500 A, current frequency 2.6 Hz, current intensity of electromagnetic stirring at the end of solidification 3 0A, current frequency 5.5Hz; superheat 26~35℃, matching continuous casting speed 2.3~2.4t / min, current intensity of electromagnetic stirring of crystallizer 480~500A, current frequency 2.8Hz, current intensity of electromagnetic stirring at the end of solidification 70A, current frequency 6.0Hz; superheat 36~40℃, matching continuous casting speed 2.1~2.2t / min, current intensity of electromagnetic stirring of crystallizer 470~480A, current frequency 3.0Hz, current intensity of electromagnetic stirring at the end of solidification 140~150A, current frequency 6.5Hz; secondary cooling adopts medium-strong cooling, specific water volume 0.34~0.35L / kg 钢 .
[0056] In this embodiment, except that the above-mentioned key technical points must be implemented as required, other continuous casting system processes and other process processes need to be implemented in coordination with conventional operations. For details, please refer to Example 1.
[0057] The 320mm×410mm cross-section HYT2 ultra-high conductivity electrode flat steel ingot obtained by the test was pickled and tested at low magnification. The results showed that the ingot had good low-magnification quality, with a loose center of 0.5 grade, no middle cracks, no subcutaneous bubbles, and a center segregation of 0.5 grade. The resistivity of the rolled flat steel at 20°C was 9.7-10.4μΩ·cm (the standard requirement is ≤13μΩ·cm).
[0058] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing ultra-high conductive electrode flat steel, characterized in that: The following steps are involved: The converter semi-steel smelting, LF electric heating refining, RH vacuum treatment, billet continuous casting, stacking slow cooling and rolling are carried out in sequence to obtain ultra-high conductive electrode flat steel; The a[O] in the molten steel after the RH vacuum treatment is controlled at 20-30 ppm, and the contents of other chemical components meet the requirements of the finished product; The molten steel after the RH vacuum treatment is sent to the continuous casting platform of the billet continuous casting and then allowed to stand for 8 to 10 minutes; The cross-sectional size of the billet continuously cast is (300-400) mm×(400-500) mm; The billet continuous casting adopts straight-through long nozzle casting, the inner diameter of the nozzle is 50-70mm, the superheat of the molten steel in the casting process is controlled at 20-40℃ as a whole, and the casting speed and electromagnetic stirring process are dynamically matched. The specific rules are: when the superheat is 20-25℃, the continuous casting speed is matched to 2.5t / min, the current intensity of the electromagnetic stirring of the crystallizer is 400-500A, the current frequency is 2.6-3.0Hz, and the current intensity of the electromagnetic stirring at the end of solidification is 0-50A, and the current frequency is 0-6.5Hz; when the superheat is 26-35℃, the continuous casting speed is matched to 2. 3~2.4t / min, the current intensity of electromagnetic stirring of the crystallizer is 400~500A, the current frequency is 2.6~3.0Hz, the current intensity of electromagnetic stirring at the end of solidification is 60~100A, the current frequency is 5.5~6.5Hz; when the superheat is 36~40℃, the matching continuous casting speed is 2.1~2.2t / min, the current intensity of electromagnetic stirring of the crystallizer is 400~500A, the current frequency is 2.6~3.0Hz, the current intensity of electromagnetic stirring at the end of solidification is 110~150A, the current frequency is 5.5~6.5Hz; During the continuous casting of the billet, the secondary cooling adopts medium-strength cooling, and the specific water volume is 0.31-0.35L / kg 钢 .
2. The preparation method according to claim 1, characterized in that: The cross-sectional dimensions of the square billet are 320 mm×410 mm or 360 mm×450 mm.
3. The preparation method according to claim 1, characterized in that: The chemical composition of the ultra-high conductive electrode flat steel includes: C≤0.008wt%, Si≤0.015wt%, Mn≤0.030wt%, P≤0.012wt%, S≤0.007wt%, and the balance is Fe.
4. The preparation method according to claim 1, characterized in that: The final C content of the converter semi-steel smelting is ≤0.030wt%, and the steel tapping temperature is ≥1650°C.
5. The preparation method according to claim 1, characterized in that: The LF electric heating refining is performed with argon blowing and stirring throughout the whole process, and the temperature at the end of the refining is controlled at 1630-1650°C.
6. The preparation method according to claim 1, characterized in that: The circulating gas flow rate of the RH vacuum treatment is 1000-1400 NL / min, the vacuum treatment time is ≥12 min, and the vacuum treatment end temperature is controlled at 1600-1610° C.
7. The preparation method according to claim 1, characterized in that: When the stacking slow cooling is started, the surface temperature of the blank is greater than 600° C., and the slow cooling time is greater than or equal to 18 hours.
8. The preparation method according to claim 1, characterized in that: The temperature of the casting during the rolling is 1000±20°C.
Citation Information
Cited By
Continuous casting control method for high-conductivity steel bar large-section rectangular blank
CN121223033A
Production control method of ultrahigh conductive electrode flat steel bloom for aluminum electrolysis
CN121227966A
Production control method of ultra-high conductive electrode flat steel bloom for aluminum electrolysis