A slurry for back electrode with high conversion efficiency

By using a specific ratio and particle size combination of coated glass powder and silver powder in the slurry for the back electrode of the solar cell, a suitable network structure is formed, which solves the problems of low light conversion efficiency and insufficient adhesion in the existing technology, and significantly improves Improve the light conversion efficiency and silver paste performance of solar cells.

CN115938643BActive Publication Date: 2024-10-11JIANGSU RIYU PHOTOVOLTAIC NEW MATERIAL CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310041544.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-12
Publication Date
2024-10-11
Estimated Expiration
2043-01-12

AI Technical Summary

Technical Problem

The photoconversion efficiency of the existing slurry used for the back electrode of solar cells is low, and the reaction between the glass powder and the passivation film affects the performance, resulting in insufficient adhesion and affecting the photoelectric conversion efficiency.

Method used

The coated glass powder is combined with silver powder of a specific particle size, and the inorganic glass powder is coated with silica sol to form a small-particle coated glass powder with a mass ratio higher than that of the silver powder. It is combined with an inorganic binder and an organic carrier to form a suitable network structure to improve adhesion and adjust silver paste properties.

Benefits of technology

It significantly improves the light conversion efficiency of solar cells, reduces the reaction between glass powder and passivation film, provides sufficient adhesion, and optimizes the performance of silver paste with less silver powder consumption.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the technical field of slurry for back electrodes, and specifically to a slurry for back electrodes with high conversion efficiency, comprising silver powder, coated glass powder, inorganic binder and organic carrier, wherein the coated glass powder is a coated powder of silica sol coated inorganic glass powder, the mass ratio of the silver powder to the coated glass powder is 1:2-5, and the D50 of the silver powder is 10-20 μm, and the D50 of the coated glass powder is 0.1-0.8 μm. The slurry for back electrodes of the present invention can not only reduce the reaction of glass powder and passivation film while providing sufficient adhesion, but also can well adjust the performance of silver paste, thereby significantly improving the light conversion efficiency of the battery, and the amount of silver powder used is small.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of slurry for back electrodes, and in particular to slurry for back electrodes with high conversion efficiency. Background Art

[0002] With the continuous improvement of the photoelectric conversion efficiency of solar cells, the average efficiency of large-scale production of monocrystalline silicon solar cells has approached 18.5%. The composition of the solar cell electrode paste has gradually increased its influence on the photoelectric conversion efficiency, especially the types of silver paste on the back of solar cells are constantly updated. At this time, the sintering conditions of the aluminum paste on the back electrode of the solar cell and the coordination of the silver paste on the front side are very important.

[0003] Crystalline silicon solar cells are devices that can respond to light energy and convert it into electrical energy. Silver paste is one of the main raw materials that affect the electrical performance of crystalline silicon solar cells. Silver paste is mainly composed of silver powder, glass powder, organic carrier and some additives. Glass powder is a more important component. During sintering, the glass powder melts and bonds the silver powder to the silicon substrate to provide adhesion for the paste. If the amount of glass powder is not appropriate, it will either lead to insufficient adhesion, or a reaction between the glass powder and the passivation film may occur, or it will affect the paste performance, thereby affecting the light conversion efficiency.

[0004] In short, the light conversion efficiency of the back electrode slurry is low and needs to be further improved. Summary of the invention

[0005] The purpose of the present invention is to overcome the defect that the light conversion efficiency of the back electrode slurry in the prior art needs to be improved, and to provide a back electrode slurry with high conversion efficiency, which can not only reduce the reaction between glass powder and passivation film while providing sufficient adhesion, but also can well adjust the performance of silver paste, thereby significantly improving the light conversion efficiency of the battery, and using less silver powder.

[0006] In order to achieve the above-mentioned object, the present invention provides a slurry for a back electrode with high conversion efficiency, comprising silver powder, coated glass powder, an inorganic binder and an organic carrier, wherein the coated glass powder is a coated powder of inorganic glass powder coated with silica sol, the mass ratio of the silver powder to the coated glass powder is 1:2-5, and the D50 of the silver powder is 10-20 μm, and the D50 of the coated glass powder is 0.1-0.8 μm.

[0007] Preferably, the mass ratio of the silver powder to the coated glass powder is 1:2-3.

[0008] Preferably, in the coated glass powder, the thickness of the silica sol coating layer is 2%-6% of the overall diameter of the coated glass powder.

[0009] More preferably, in the coated glass powder, the thickness of the silica sol coating layer is 2%-4% of the overall diameter of the coated glass powder.

[0010] Preferably, the mass ratio of the silver powder to the coated glass powder, the inorganic binder and the organic carrier is 1:2-5:0.01-0.06:0.2-0.5.

[0011] More preferably, the mass ratio of the silver powder to the coated glass powder, the inorganic binder and the organic carrier is 1:2-3:0.01-0.04:0.2-0.4.

[0012] Preferably, the inorganic binder is selected from oxides of V and Cr, and the weight ratio of the oxides of V and Cr is 1:0.1-0.7.

[0013] Preferably, the organic carrier is selected from ethyl cellulose and terpineol, and the weight ratio of ethyl cellulose to terpineol is 1:1.2-2.

[0014] Preferably, the inorganic glass powder is selected from oxides of Bi, Si, Zn, and Al and the weight ratio thereof is 3-6:1:1:0.1-0.5.

[0015] Preferably, the D50 of the silver powder is 10-15 μm, and the D50 of the encapsulated glass powder is 0.1-0.3 μm.

[0016] Beneficial Effects

[0017] Compared with the prior art, the slurry for the back electrode provided by the present invention adopts a coated glass powder of a specific particle size to match a silver powder of a specific particle size and a suitable mass ratio thereof, wherein the particle size of the coated glass powder is smaller than the particle size of the silver powder, and the mass of the coated glass powder is higher than the mass of the silver powder, which can not only provide sufficient adhesion while reducing the reaction between the glass powder and the passivation film, but also can well bond the silver powder to form a specific suitable network structure after the coated glass powder is melted, which can not only play a good bonding role, but also can well adjust the performance of the silver paste, thereby significantly improving the light conversion efficiency of the battery, and the amount of silver powder used is small. Among them, since the particle size of the coated glass powder is smaller than the particle size of the silver powder, and the mass of the coated glass powder is higher than the mass of the silver powder, before melting, the coated glass powder will be dispersed around the silver powder, which is more conducive to the subsequent regulation of the performance of the silver powder; after melting, when the above-mentioned network structure is formed, the molten state of the glass powder will well provide sufficient adhesion and bonding force, and at the same time play a good role in regulating the silver paste. Under the same conditions, if the particle size of the coated glass powder is not smaller than that of the silver powder, or the mass of the coated glass powder is not higher than that of the silver powder, then the adjustment of the silver paste performance cannot achieve the above purpose, and the improvement of light conversion efficiency is limited. DETAILED DESCRIPTION

[0018] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0019] The invention provides a slurry for a back electrode with high conversion efficiency, comprising silver powder, coated glass powder, an inorganic binder and an organic carrier, wherein the coated glass powder is a coated powder of inorganic glass powder coated with silica sol, the mass ratio of the silver powder to the coated glass powder is 1:2-5, the D50 of the silver powder is 10-20 μm, and the D50 of the coated glass powder is 0.1-0.8 μm.

[0020] Preferably, the D50 of the silver powder is 10-15 μm, and the D50 of the coated glass powder is 0.1-0.3 μm. Under this preferred solution, it is more conducive to improving the light conversion efficiency of the battery.

[0021] Preferably, the mass ratio of the silver powder to the coated glass powder is 1:2-3. Under this preferred solution, it is more conducive to improving the light conversion efficiency of the battery.

[0022] Preferably, in the coated glass powder, the thickness of the silica sol coating layer is 2%-6% of the overall diameter of the coated glass powder.

[0023] More preferably, in the coated glass powder, the thickness of the silica sol coating layer is 2%-4% of the overall diameter of the coated glass powder. Under this preferred solution, it can play an insulating and coating role on the glass powder, and can quickly break when melted to release the glass powder, thereby further improving the light conversion efficiency of the battery.

[0024] Preferably, the mass ratio of the silver powder to the coated glass powder, the inorganic binder and the organic carrier is 1:2-5:0.01-0.06:0.2-0.5.

[0025] More preferably, the mass ratio of the silver powder to the coated glass powder, the inorganic binder and the organic carrier is 1:2-3:0.01-0.04:0.2-0.4. Under this preferred solution, it is beneficial to better adjust the performance of the silver paste and improve the light conversion efficiency of the battery.

[0026] In the present invention, as long as the coated glass powder can achieve the above-mentioned structure and composition, those skilled in the art can prepare it by any existing method (such as the coated glass powder involved in CN105621896B), or obtain it commercially.

[0027] Preferably, the inorganic binder is selected from oxides of V and Cr, and the weight ratio of the oxides of V and Cr is 1:0.1-0.7.

[0028] Preferably, the organic carrier is selected from ethyl cellulose and terpineol, and the weight ratio of ethyl cellulose to terpineol is 1:1.2-2.

[0029] Preferably, the inorganic glass powder is selected from oxides of Bi, Si, Zn, and Al and the weight ratio thereof is 3-6:1:1:0.1-0.5.

[0030] The present invention will be described in detail below through examples.

[0031] Example 1

[0032] A slurry for a back electrode with high conversion efficiency, characterized in that it includes silver powder, coated glass powder, inorganic binder and organic carrier, wherein the coated glass powder is a coated powder of silica sol coated inorganic glass powder, and the D50 of the silver powder is 12μm, and the D50 of the coated glass powder is 0.2μm. In the coated glass powder, the thickness of the silica sol coating layer is 2% of the overall diameter of the coated glass powder. The mass ratio of the silver powder to the coated glass powder, the inorganic binder and the organic carrier is 1:2:0.02:0.3. The inorganic binder is selected from the oxides of V and Cr, and the weight ratio of the oxides of V and Cr is 1:0.2. The organic carrier is selected from ethyl cellulose and pine alcohol, and the weight ratio of the ethyl cellulose and pine alcohol is 1:1.5. The inorganic glass powder is selected from the oxides of Bi, Si, Zn, and Al, and the weight ratio thereof is 4:1:1:0.1.

[0033] Example 2

[0034] The process is carried out in accordance with Example 1, except that the thickness of the silica sol coating layer is 6% of the overall diameter of the coated glass powder.

[0035] Example 3

[0036] The process is carried out in accordance with Example 1, except that the thickness of the silica sol coating layer is 5% of the overall diameter of the coated glass powder.

[0037] Example 4

[0038] The process is carried out in accordance with Example 1, except that the mass ratio of the silver powder to the encapsulated glass powder is 1:5.

[0039] Example 5

[0040] The process is carried out in accordance with Example 1, except that the mass ratio of the silver powder to the encapsulated glass powder is 1:4.

[0041] Comparative Example 1

[0042] The process is carried out in accordance with Example 1, except that the glass powder is not coated, that is, the coated glass powder is replaced by pure glass powder.

[0043] Comparative Example 2

[0044] The process is carried out in accordance with Example 1, except that the D50 of the encapsulated glass powder is 12 μm.

[0045] Comparative Example 3

[0046] The process is carried out in accordance with Example 1, except that the mass ratio of the silver powder to the encapsulated glass powder is 1:0.8.

[0047] Test Case

[0048] The slurries obtained in the above embodiments and comparative examples were respectively printed on a P-type single crystal silicon substrate with a diameter of 100 mm, and placed in an infrared tunnel furnace for sintering at 800° C. to obtain a solar cell, and its photoelectric conversion efficiency was tested using a JT-1 transistor characteristic plotter, wherein the relative photoelectric conversion efficiency improvement of each embodiment compared with comparative example 1 is shown in Table 1. Relative photoelectric conversion efficiency improvement = (photoelectric conversion efficiency of the target embodiment - photoelectric conversion efficiency of comparative example 1) / photoelectric conversion efficiency of comparative example 1.

[0049] Table 1

[0050] Example No. Relative light conversion efficiency improvement, % Example 1 8 Example 2 5.5 Example 3 4 Example 4 6 Example 5 5.5 Comparative Example 2 2 Comparative Example 3 3.5

[0051] It can be seen from the results in Table 1 that the embodiments of the present invention have significantly better effects.

[0052] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.

Claims

1. A slurry for a back electrode with high conversion efficiency, characterized in that: The invention comprises silver powder, coated glass powder, inorganic binder and organic carrier, wherein the coated glass powder is a coated powder of inorganic glass powder coated with silica sol, the mass ratio of the silver powder to the coated glass powder is 1:2-5, the D50 of the silver powder is 10-20 μm, and the D50 of the coated glass powder is 0.1-0.8 μm.

2. The back electrode slurry according to claim 1, characterized in that: The mass ratio of the silver powder to the coated glass powder is 1:2-3.

3. The back electrode slurry according to claim 1, characterized in that: In the coated glass powder, the thickness of the silica sol coating layer is 2%-6% of the overall diameter of the coated glass powder.

4. The slurry for back electrode according to claim 3, characterized in that: In the coated glass powder, the thickness of the silica sol coating layer is 2%-4% of the overall diameter of the coated glass powder.

5. The slurry for back electrode according to claim 1, characterized in that: The mass ratio of the silver powder to the coated glass powder, the inorganic binder and the organic carrier is 1:2-5:0.01-0.06:0.2-0.

5.

6. The slurry for back electrode according to claim 5, characterized in that: The mass ratio of the silver powder to the coated glass powder, the inorganic binder and the organic carrier is 1:2-3:0.01-0.04:0.2-0.

4.

7. The slurry for back electrode according to claim 1, characterized in that: The inorganic binder is selected from oxides of V and Cr, and the weight ratio of the oxides of V and Cr is 1:0.1-0.

7.

8. The slurry for back electrode according to claim 1, characterized in that: The organic carrier is selected from ethyl cellulose and terpineol, and the weight ratio of ethyl cellulose to terpineol is 1:1.2-2.

9. The slurry for back electrode according to claim 1, characterized in that: The inorganic glass powder is selected from oxides of Bi, Si, Zn, and Al and the weight ratio thereof is 3-6:1:1:0.1-0.

5.

10. The slurry for back electrode according to claim 1, characterized in that: The D50 of the silver powder is 10-15 μm, and the D50 of the coated glass powder is 0.1-0.3 μm.

Citation Information

Patent Citations

  • Glass powder for back electrode paste of solar cells and its preparation method

    CN105621896B

  • Low-resistance high-efficiency lead-free back silver pulp for amorphous silicon solar battery

    CN104505139A

  • Glass powder for back electrode slurry of solar battery and preparation method of glass powder

    CN105621896A

  • Silver conductor paste for back electrode of battery

    CN112908511A

  • Ag paste composition for forming electrode and silicon solar cell using the same

    KR1020130063266A