A nickel-manganese oxide positive electrode material and its preparation method and use
By forming nickel manganese oxide nanosheets with a porous structure, the problem of structural instability and poor electrochemical performance of the cathode material of lithium-ion batteries is solved, high cycle and rate performance are improved, and excellent lithium storage performance and stability are provided. .
Patent Information
- Application Number
- CN202310177804.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-02-28
AI Technical Summary
Existing lithium-ion battery cathode materials have problems such as structural instability and poor electrochemical performance, especially under high rate and long cycle conditions, which affects the performance of the battery.
Porous nickel manganese oxide nanosheets are used as the cathode material. The nickel zinc precursor is formed under the action of etchant and manganese salt to form a nickel manganese zinc three-metal based nanosheet structure, and the porous structure is formed through sintering, which improves the material's durability. Structural stability and electrochemical performance.
The structural stability and lithium storage performance of the nickel manganese oxide cathode material have been improved, and the cycle and rate performance of the battery have been improved. The capacity retention rate after 500 cycles at 0.1C can reach more than 87.48%, and the capacity retention rate after 1,000 cycles is The capacity retention rate can reach more than 76.70%, and the rate performance can reach more than 68.05%.
Smart Images

Figure BDA0004101524350000121 
Figure BDA0004101524350000122 
Figure BDA0004101524350000131
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium ion batteries and relates to a nickel-manganese oxide positive electrode material and a preparation method and application thereof. Background Art
[0002] Mn has valence diversity and Ni has high activity. Both are transition metals in the first period. They have attracted widespread attention from the scientific research community due to their abundance in the earth, high electrochemical activity and controllable compound morphology. In recent years, nickel-manganese-based compounds have great development prospects due to their excellent electrochemical properties and the synergistic effect between the two elements. In addition, the coexistence of Ni and Mn elements can redistribute electron density through charge transfer and even rearrange their electronic structure. Therefore, people are committed to preparing low-cost and high-efficiency nickel-manganese-based compounds and using them as positive electrode materials for lithium-ion batteries.
[0003] CN105047900A discloses a method and equipment for preparing a nano-sheet lithium nickel manganese oxide material. That is, firstly prepare a nickel-manganese coprecipitate by a coprecipitation method, then calcine to obtain a nickel-manganese oxide, then calcine with a lithium salt to obtain a spinel lithium nickel manganese oxide compound, and finally coat the particle surface with a uniform layer of titanium / or zirconium metal oxide. However, in the process of mixing the homogeneous precursor with the lithium salt and then calcining at high temperature, there is incomplete mixing, resulting in an impure product phase, and the crystal structure of the synthesized nano-sheet lithium nickel manganese oxide is irregular and agglomerated, which affects the Li during charging and discharging. + diffusion pathway, impairing the rate performance of the battery.
[0004] US20080107968A1 discloses the use of a solid phase method to prepare lithium nickel manganese oxide. However, due to the uncontrollable particle growth, Mn 3+ More manganese dissolves in the electrolyte, affecting the structural stability of the material, making the material less stable during long cycles.
[0005] CN102569776A discloses a method for preparing a spherical high-voltage positive electrode material spinel high-voltage nickel manganese lithium oxide, which is prepared by a hydrothermal-solid phase two-step method. That is, a nickel source, a manganese source, and a doped element compound solution are evenly mixed with a sodium / ammonium carbonate solution, and then a surfactant is added, and then a spherical nickel manganese carbonate coprecipitate is prepared under hydrothermal conditions, and a spherical nickel manganese oxide is obtained after washing, drying and calcining; finally, the spherical nickel manganese oxide is mixed with a lithium source by liquid phase ball milling, dried, and sintered to obtain a positive electrode active material. This method not only has a complex production process, but also has harsh reaction conditions, and a large amount of byproduct sodium / ammonium salt is produced during the preparation process, which is not suitable for industrial production.
[0006] In view of the actual application prospects of power batteries, it is necessary to develop long-cycle lithium-ion battery cathode materials with high current density. After a lot of research, it is found that the existing lithium-ion cathode materials still have many shortcomings. For example, bulk compounds often show shortcomings such as insufficient exposure of active sites and poor conductivity. The two-dimensional structure can obtain a high specific surface area, which is conducive to the full exposure of active sites and the rapid transmission of electrolytes and electrons. In addition, the anisotropic properties of two-dimensional materials make them a new type of nanomaterial. In addition, the good mechanical properties of the two-dimensional structure are of profound significance for the realization of high-capacity and high-rate lithium-ion battery cathode materials. However, the shortcomings of the existing two-dimensional structure that are easy to transform and have poor thermal stability have greatly affected the electrochemical properties of the material.
[0007] Therefore, how to obtain a nickel-manganese-based positive electrode material with stable structure and excellent electrochemical performance is a technical problem that needs to be solved urgently. Summary of the invention
[0008] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a nickel-manganese oxide positive electrode material and its preparation method and use. The present invention provides a nickel-manganese oxide nanosheet with a porous structure, which has a stable structure and excellent lithium storage performance, and improves the cycle and rate performance of the battery.
[0009] To achieve this object, the present invention adopts the following technical solutions:
[0010] In a first aspect, the present invention provides a nickel manganese oxide positive electrode material, wherein the morphology of the nickel manganese oxide positive electrode material is a porous nanosheet structure.
[0011] The present invention provides a nickel-manganese oxide nanosheet with a porous structure, a porous two-dimensional sheet structure, and a porous two-dimensional sheet structure, which forms an interconnected network architecture format, is more conducive to the transmission of electrons and ions, has a stable structure, and has excellent lithium storage performance, thereby improving the cycle and rate performance of the battery.
[0012] In a second aspect, the present invention further provides a method for preparing the nickel manganese oxide positive electrode material as described in the first aspect, the preparation method comprising the following steps:
[0013] (1) mixing a nickel salt, a zinc salt, an organic ligand and a solvent to react to obtain a nickel-zinc precursor;
[0014] (2) mixing the nickel-zinc precursor, manganese salt, etchant and solvent described in step (1) to obtain nickel-manganese-zinc based nanosheets;
[0015] (3) Sintering the nickel-manganese-zinc-based nanosheets described in step (2) to obtain the nickel-manganese oxide positive electrode material.
[0016] The preparation method provided by the present invention obtains a nickel-zinc precursor (nickel-zinc organic skeleton, spindle-like structure). Under the action of an etchant and a manganese salt, the etchant attacks the surface of the nickel-zinc precursor, and the surface is etched and hydrolyzed. Due to the presence of the manganese salt, the inside and outside of the precursor are affected by the metal ion pressure difference and the nano effect, and Mn 2+ After penetrating into the precursor skeleton, under the dual effects of etching and manganese ions, the original nickel-zinc precursor structure collapsed and reorganized to form a nickel-manganese-zinc tri-metal-based nanosheet structure. After further sintering, the zinc element volatilized to form holes on the surface of the nanosheet, and finally a nickel-manganese oxide nanosheet structure with a porous structure was obtained. When used as a positive electrode material, it has excellent lithium storage performance, thereby improving the battery's cycle and rate performance.
[0017] In the present invention, if the nickel-manganese-zinc organic skeleton is directly obtained and then sintered, a lamellar structure cannot be obtained, and if no etchant is added in step (2), the reorganization of the nanosheets cannot be achieved, and ultimately a porous nanosheet cannot be obtained.
[0018] Preferably, the nickel salt in step (1) includes any one of nickel chloride hexahydrate, nickel nitrate or nickel acetate, or a combination of at least two of them.
[0019] Preferably, the zinc salt in step (1) includes any one of zinc chloride, zinc nitrate or zinc acetate, or a combination of at least two of them.
[0020] Preferably, the organic ligand in step (1) comprises fumaric acid.
[0021] Preferably, the solvent in step (1) comprises N,N-dimethylformamide.
[0022] Preferably, the reaction in step (1) comprises an oil bath heating reaction.
[0023] Preferably, the temperature of the oil bath heating reaction is 85-120°C, for example, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C or 120°C.
[0024] Preferably, after the reaction in step (1) is completed, centrifugation and washing are performed in sequence.
[0025] The step (1) provided by the present invention is a conventional process for preparing a metal organic framework, that is, the selection of its organic ligand and the preparation process are conventional technical means to obtain the nickel zinc precursor of the present invention.
[0026] Preferably, in step (2), the mass ratio of the nickel zinc precursor to the manganese salt is (2-10):1, for example, 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, 9:1 or 10:1.
[0027] In the present invention, if the mass ratio of the nickel-zinc precursor to the manganese salt is too large, the pressure difference inside and outside the precursor will be too large, the manganese ions will penetrate faster, and the disintegration and recombination will be too fast to obtain nanosheets with loose structure. If the mass ratio is too small, it will affect the reaction rate and it is easy to obtain thick nanosheets with hard structure.
[0028] Preferably, the etchant in step (2) comprises an acid.
[0029] In the present invention, an acid is selected as an etchant. During the reaction process of step (2), H + Attacking the surface of the spindle-like organic precursor (Ni-Zn precursor), Mn 2+ The concentration of ions will affect the internal and external osmotic pressure difference, which will ultimately affect the etching rate. The presence of an acidic environment makes Mn 2+ The concentration does not need to be too large, that is, the acid and the manganese salt in the present invention interact with each other and work synergistically to achieve the collapse of the original precursor structure, thereby forming a new nickel-manganese-zinc nanosheet structure.
[0030] Preferably, the mass volume ratio of the nickel zinc precursor to the acid is 25:(5-25) mg / mL, such as 25:5, 25:10, 25:15, 25:20 or 25:25.
[0031] The acid provided in the present invention is a commercially available concentrated acid series, and the molar amount of the acid is 0.1 mmol. If the mass-to-volume ratio of the nickel-zinc precursor to the acid is too large, that is, the amount of acid added is too small, it is not conducive to the occurrence of the reaction, affecting the reaction efficiency and the reorganization of the nanosheets. If the mass-to-volume ratio is too small, that is, the amount of acid added is too much, it will lead to a violent reaction and obtain loose and broken nanosheets.
[0032] Preferably, the acid comprises hydrochloric acid.
[0033] Preferably, step (2) further comprises a buffer.
[0034] In the present invention, adding a buffer during the reaction process of step (2) can further regulate the morphology of the obtained nanosheets, making the reaction rate uniform and the product morphology uniform. If no buffer is added, the reaction rate will be too fast and the morphology of the product will be affected.
[0035] Preferably, the mass ratio of the buffer to the nickel-zinc precursor is (2-6):1, such as 2:1, 3:1, 4:1, 5:1 or 6:1.
[0036] In the present invention, if the mass ratio of the buffer to the nickel-zinc precursor is too small, it is not conducive to slowing down the etching rate, while if it is too large, it will lead to a too slow reaction rate.
[0037] Preferably, the buffer comprises urea and / or aqueous ammonia.
[0038] In the present invention, urea and / or ammonia water are selected as buffering agents to mitigate the reaction rate.
[0039] Preferably, the reaction in step (2) comprises an oil bath heating reaction and / or a water bath heating reaction.
[0040] Preferably, the reaction temperature of the oil bath heating reaction is 80-110°C, for example, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C or 110°C.
[0041] Preferably, the reaction time of the oil bath heating is 90 to 180 min, for example, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min or 180 min, etc.
[0042] Preferably, the temperature of the water bath heating reaction is ≥80°C, such as 80°C, 85°C, 90°C or 95°C.
[0043] Preferably, the reaction time of the water bath heating reaction is 90 to 240 min, for example, 90 min, 100 min, 110 min, 120 min, 130 min, 140 min, 150 min, 160 min, 170 min, 180 min, 190 min, 200 min, 210 min, 220 min, 230 min or 240 min, etc.
[0044] In the present invention, the temperature and time of the reaction process of step (2) are regulated, and the amount of the etchant, buffer and manganese salt added is coordinated, so that the precursor is affected by the pressure difference between the internal and external metal ions and the nano effect, and the effect gradually increases during the etching and reaction process, and finally the original precursor structure collapses to form nickel-manganese-zinc trimetallic nanosheets; if a hydrothermal reaction is used, it will lead to a violent reaction, structural collapse, and inability to achieve recombination.
[0045] Preferably, the sintering temperature in step (3) is 450-700°C, for example, 450°C, 475°C, 500°C, 525°C, 550°C, 575°C, 600°C, 625°C, 650°C, 675°C or 700°C.
[0046] If the sintering temperature provided by the present invention is too high, zinc will volatilize too quickly, resulting in too large pores. In addition, too high a temperature will also destroy the two-dimensional layer structure, while too low a temperature will affect the reaction rate, resulting in too small pores.
[0047] Preferably, the sintering time in step (3) is 3 to 10 hours, for example, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours or 10 hours.
[0048] As a preferred technical solution, the preparation method comprises the following steps:
[0049] (1) mixing a nickel salt, a zinc salt, an organic ligand and a solvent, and performing a heating reaction in an oil bath at 85 to 120° C. to obtain a nickel-zinc precursor;
[0050] (2) mixing the nickel-zinc precursor, manganese salt, acid, buffer and solvent described in step (1), wherein the mass ratio of the nickel-zinc precursor to the manganese salt is (2-10):1, the mass volume ratio of the nickel-zinc precursor to the acid is 25:(5-25) mg / mL, and the mass ratio of the buffer to the nickel-zinc precursor is (2-6):1, and heating the mixture in an oil bath at 80-110° C. for 90-180 min to obtain nickel-manganese-zinc-based nanosheets;
[0051] (3) Sintering the nickel-manganese-zinc-based nanosheets in step (2) at 450-700° C. for 3-10 hours to obtain the nickel-manganese oxide positive electrode material.
[0052] In a third aspect, the present invention provides a positive electrode material, which is obtained by compounding the nickel manganese oxide positive electrode material as described in the first aspect with a lithium source.
[0053] The nickel-manganese oxide material provided by the present invention can be further mixed with a lithium source and sintered to obtain a nickel-manganese-oxide lithium positive electrode material.
[0054] In a fourth aspect, the present invention further provides a lithium-ion battery, wherein the lithium-ion battery comprises the nickel-manganese oxide positive electrode material as described in the first aspect or the positive electrode material as described in the third aspect.
[0055] When the lithium-ion battery provided by the present invention uses nickel manganese oxide as the positive electrode material, lithium metal is correspondingly selected as the negative electrode.
[0056] Compared with the prior art, the present invention has the following beneficial effects:
[0057] In the preparation process of the present invention, after obtaining the nickel-zinc precursor (nickel-zinc organic skeleton, spindle-like structure), under the action of the etchant and the manganese salt, the etchant attacks the surface of the nickel-zinc precursor, the surface is etched and hydrolyzed, and due to the presence of the manganese salt, the inside and outside of the precursor are affected by the metal ion pressure difference and the nano effect, Mn 2+Penetrate into the precursor skeleton, under the dual effects of etching and manganese ions, the original nickel-zinc precursor structure collapses, the structure is reorganized, and a nickel-manganese-zinc trimetallic nanosheet structure is formed. After further sintering, the zinc element volatilizes, forming a cavity on the surface of the nanosheet, and finally a nickel-manganese oxide nanosheet structure with a porous structure is obtained. After being used as a positive electrode material, the structure is stable and has excellent lithium storage performance, thereby improving the battery cycle and rate performance. The button battery obtained by the nickel-manganese oxide provided by the present invention has a capacity retention rate of more than 87.48% after 500 cycles at 0.1C, a capacity retention rate of more than 76.70% after 1000 cycles, and a capacity retention rate of more than 62.58% after 2000 cycles, and a rate performance of more than 68.05% at 0.5C / 1C, a rate performance of more than 57.91% at 0.5C / 3C, and a rate performance of more than 51.23% at 0.5C / 4C. DETAILED DESCRIPTION
[0058] The technical scheme of the present invention is further illustrated by specific examples below. Those skilled in the art should understand that the examples are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0059] Example 1
[0060] This embodiment provides a nickel manganese oxide positive electrode material, and the morphology of the positive electrode material is a nanosheet with a porous structure.
[0061] The preparation method of the positive electrode material is as follows:
[0062] (1) 116 mg of fumaric acid (organic ligand), 214 mg of nickel chloride hexahydrate and 40.9 mg of zinc chloride were dispersed in 15 ml of N,N-dimethylformamide (DMF), and ultrasonic treatment was performed at room temperature for at least 30 min to make the solution uniformly dispersed. Then, the mixed solution was placed in a three-necked flask, and the flask was heated in an oil bath at 120° C. for 3 hours. After cooling to room temperature, the mixture was centrifuged and washed three times with DMF to obtain a light green precipitate, which is a nickel-zinc precursor with a spindle-like structure;
[0063] (2) Take 25 mg of the nickel-zinc precursor obtained above and disperse it in 12 ml of 0.1 mmol hydrochloric acid (commercially available concentrated hydrochloric acid) as solution A, disperse 5 mg of manganese nitrate hexahydrate and 100 mg of urea in 10 ml of distilled water as solution B; slowly introduce solution A into solution B, stir evenly to obtain solution C, seal solution C in a round-bottom flask, keep the flask in a 90° C. oil bath for 150 minutes, wash the product obtained after the reaction conventionally, and obtain a nickel-manganese-zinc-based nanosheet compound (the molar ratio of nickel: manganese: zinc is 7:1:2);
[0064] (3) The trimetallic nickel-manganese-zinc-based nanosheets obtained in (2) were placed in a tube furnace and maintained in a nitrogen atmosphere at 650° C. for 5 hours to obtain a nickel-manganese oxide nanosheet structure with a porous structure (porous biscuit-like thin sheet, NiMn 0.4 O 2 ).
[0065] Example 2
[0066] This embodiment provides a nickel manganese oxide positive electrode material, and the morphology of the positive electrode material is a nanosheet with a porous structure.
[0067] The preparation method of the positive electrode material is as follows:
[0068] (1) 11m6g of fumaric acid (organic ligand), 214mg of nickel chloride hexahydrate and 40.9mg of zinc chloride were dispersed in 15ml of N,N-dimethylformamide (DMF), and ultrasonic treatment was performed at room temperature for at least 30min to make the solution uniformly dispersed. Then, the mixed solution was placed in a three-necked flask, and the flask was heated in an oil bath at 120°C for 3 hours. After cooling to room temperature, the mixture was centrifuged and washed three times with DMF to obtain a light green precipitate, which is a nickel-zinc precursor with a spindle-like structure;
[0069] (2) Take 25 mg of the nickel-zinc precursor obtained above and disperse it in 25 ml of 0.1 mmol hydrochloric acid (commercially available concentrated hydrochloric acid) as solution A, disperse 12.5 mg of manganese nitrate hexahydrate and 150 mg of urea in 10 ml of distilled water as solution B; slowly introduce solution A into solution B, stir evenly to obtain solution C, seal solution C in a round-bottom flask, keep the flask in an 80° C. oil bath for 180 minutes, wash the product obtained after the reaction conventionally, and obtain a nickel-manganese-zinc-based nanosheet compound (the molar ratio of nickel: manganese: zinc is 6:3:1);
[0070] (3) The trimetallic nickel-manganese-zinc-based nanosheets obtained in (2) were placed in a tube furnace and kept in a nitrogen atmosphere at 450° C. for 10 hours to obtain a nickel-manganese oxide nanosheet structure with a porous structure (porous biscuits similar to thin sheets, Ni 0.5 Mn 0.4 O 2 ).
[0071] Example 3
[0072] This embodiment provides a nickel manganese oxide positive electrode material, and the morphology of the positive electrode material is a nanosheet with a porous structure.
[0073] The preparation method of the positive electrode material is as follows:
[0074] (1) 116 mg of fumaric acid, 214 mg of nickel sulfate and 40.9 mg of zinc chloride were dispersed in 15 ml of N,N-dimethylformamide (DMF), and ultrasonic treatment was performed at room temperature for at least 30 min to make the solution uniformly dispersed. Then, the mixed solution was placed in a three-necked flask, and the flask was heated in an oil bath at 90° C. for 5 hours. After cooling to room temperature, the mixture was centrifuged and washed three times with DMF to obtain a light green precipitate, which is a nickel-zinc precursor with a spindle-like structure;
[0075] (2) Take 25 mg of the nickel-zinc precursor obtained above and disperse it in 5 ml of 0.1 mmol hydrochloric acid (commercially available concentrated hydrochloric acid) as solution A, disperse 2.5 mg of manganese nitrate hexahydrate and 500 mg of urea in 10 ml of distilled water as solution B; slowly introduce solution A into solution B, stir evenly to obtain solution C, seal solution C in a round-bottom flask, keep the flask in a 90° C. water bath for 130 minutes, wash the product obtained after the reaction conventionally, and obtain a nickel-manganese-zinc-based nanosheet compound (the molar ratio of nickel: manganese: zinc is 8:1:1);
[0076] (3) The trimetallic nickel-manganese-zinc-based nanosheets obtained in (2) were placed in a tube furnace and maintained at 700° C. in a nitrogen atmosphere for 3 hours to obtain a nickel-manganese oxide nanosheet structure with a porous structure (porous biscuit-like thin sheet, NiMn 0.1 O 2 ).
[0077] Example 4
[0078] The difference between this embodiment and embodiment 1 is that the amount of hydrochloric acid added in step (2) of this embodiment is 30 mL (the mass volume ratio of the precursor to the acid is 25:30 mg / mL).
[0079] The rest of the preparation methods and parameters were the same as those in Example 1.
[0080] Example 5
[0081] The difference between this embodiment and embodiment 1 is that the mass of manganese nitrate hexahydrate in step (2) of this embodiment is 15 mg (the mass ratio of the precursor to the manganese salt is 25:15).
[0082] The rest of the preparation methods and parameters were the same as those in Example 1.
[0083] Example 6
[0084] The difference between this embodiment and embodiment 1 is that urea is not added in step (2) of this embodiment.
[0085] The rest of the preparation methods and parameters were the same as those in Example 1.
[0086] Example 7
[0087] The difference between this embodiment and embodiment 1 is that the sintering temperature in step (3) of this embodiment is 750°C.
[0088] The rest of the preparation methods and parameters were the same as those in Example 1.
[0089] Example 8
[0090] The difference between this embodiment and embodiment 1 is that the sintering temperature in step (3) of this embodiment is 400°C.
[0091] The rest of the preparation methods and parameters were the same as those in Example 1.
[0092] Comparative Example 1
[0093] The difference between this comparative example and Example 1 is that no etching agent (hydrochloric acid) is added in step (2) of this comparative example.
[0094] The rest of the preparation methods and parameters were the same as those in Example 1.
[0095] Comparative Example 2
[0096] The difference between this comparative example and Example 1 is that this comparative example does not include the calcination process in step (3), and in the preparation process of step (1), no zinc salt is added, thereby obtaining nickel manganese oxide without nanosheets having a porous structure.
[0097] The nickel manganese oxide provided in Example 1-8 and Comparative Example 1-2 was used as the positive electrode material. The positive electrode material, 10 wt% PVDF binder, and acetylene black were fully ground in a mortar at a mass ratio of 7:2:1 for at least 20 minutes. N-methylpyrrolidone (NMP) was added to the electrode material mixed with the conductive agent and the binder, and stirred at a speed of 800 r / min for 5 hours to form a uniform slurry. The slurry was evenly coated on an aluminum foil, and the aluminum foil was placed in a vacuum drying oven at 80°C for overnight drying. The aluminum foil coated with the active material was cut into 1.131 cm 2 The active material content of the circular electrode is about 0.9 mg cm -2 , and obtain the positive electrode sheet;
[0098] The positive electrode sheets provided in Examples 1-8 and Comparative Examples 1-2 were assembled into 2032 button cells in a glove box. -1 Bisfluoromethanesulfonimide (LiTFSI), 1.0wt% LiNO 3, a commercial electrolyte of 1,3-dioxane (DOL) and 1,2-dimethoxyethane (DME) (volume ratio of 1:1) was used as the lithium battery electrolyte, the counter electrode and the reference electrode were both lithium foil, and the separator was Celgard 2400 membrane. Before the test, the assembled battery was placed in an oven at 30°C for 6 hours to allow the electrolyte to completely wet the electrode material to obtain the battery to be tested.
[0099] The electrochemical performance test was performed on the batteries to be tested provided by Examples 1-8 and Comparative Examples 1-2. The test conditions were: the battery test system was Wuhan LAND, the test temperature was 25°C, the voltage window was set to 1.5-3.2V, and the charge and discharge cycle test was performed at 0.1C. The test results are shown in Table 1.
[0100] Table 1
[0101]
[0102] Rate performance test: The test conditions are 25°C, 0.5C charging, and 0.5C discharging. The test results are shown in Table 2.
[0103] Table 2
[0104]
[0105]
[0106] Combining Table 1 and Table 2:
[0107] From the data results of Example 1 and Example 4, it can be seen that adding too much etchant (acid) in step (2) is not conducive to the hydrolysis of the organic precursor and the reorganization of the nanosheets. Too much acid leads to too fast hydrolysis and the breakage of the nanosheets.
[0108] From the data results of Example 1 and Example 5, it can be seen that if the amount of manganese salt added in step (2) is too much, the ion osmotic pressure inside and outside the precursor will be too large, the manganese ions will penetrate too quickly and too much, and the nanosheet structure will be loose.
[0109] From the data results of Example 1 and Example 6, it can be seen that if no buffer is added in step (2), the thickness and integrity of the nanosheets will be affected.
[0110] From the data results of Example 1 and Examples 7 and 8, it can be seen that in step (3), the sintering temperature is too high, resulting in too fast sublimation of the zinc element and increase in pore diameter, while the sintering temperature is too low and complete sublimation of the zinc element cannot be achieved.
[0111] It can be seen from the data results of Example 1 and Comparative Example 1 that a porous thin sheet structure cannot be obtained without adding an etchant during the preparation process.
[0112] From the data results of Example 1 and Comparative Example 2, it can be seen that there is no porous structure in the nickel-manganese two-dimensional structure, and there is a problem of poor conductivity.
[0113] In summary, in the preparation process of the present invention, after obtaining the nickel-zinc precursor (nickel-zinc organic skeleton, spindle-like structure), under the action of the etchant and the manganese salt, the etchant attacks the surface of the nickel-zinc precursor, the surface is etched and hydrolyzed, and due to the presence of the manganese salt, the inside and outside of the precursor are affected by the metal ion pressure difference and the nano effect, Mn 2+ Penetrate into the precursor skeleton, under the dual effects of etching and manganese ions, the original nickel-zinc precursor structure collapses, the structure is reorganized, and a nickel-manganese-zinc trimetallic nanosheet structure is formed. After further sintering, the zinc element volatilizes, forming a cavity on the surface of the nanosheet, and finally a nickel-manganese oxide nanosheet structure with a porous structure is obtained. After being used as a positive electrode material, the structure is stable and has excellent lithium storage performance, thereby improving the battery cycle and rate performance. The button battery obtained by the nickel-manganese oxide provided by the present invention has a capacity retention rate of more than 87.48% after 500 cycles at 0.1C, a capacity retention rate of more than 76.70% after 1000 cycles, and a capacity retention rate of more than 62.58% after 2000 cycles, and a rate performance of more than 68.05% at 0.5C / 1C, a rate performance of more than 57.91% at 0.5C / 3C, and a rate performance of more than 51.23% at 0.5C / 4C.
[0114] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a positive electrode material for a lithium ion battery, characterized in that: The positive electrode material is nickel manganese oxide or the positive electrode material is obtained by mixing nickel manganese oxide and a lithium source and sintering them, and the morphology of the nickel manganese oxide is a porous nanosheet structure; The nickel manganese oxide is prepared by the following preparation method, which comprises the following steps: (1) mixing a nickel salt, a zinc salt, an organic ligand and a solvent to react to obtain a nickel-zinc precursor; (2) mixing the nickel-zinc precursor, manganese salt, buffer, etchant and solvent described in step (1) to obtain nickel-manganese-zinc-based nanosheets, wherein the etchant comprises an acid, and the buffer comprises urea and / or ammonia water; (3) Sintering the nickel-manganese-zinc-based nanosheets described in step (2) to obtain the nickel-manganese oxide positive electrode material.
2. The preparation method according to claim 1, characterized in that: The nickel salt in step (1) includes any one of nickel chloride hexahydrate, nickel nitrate or nickel acetate, or a combination of at least two of them.
3. The preparation method according to claim 1, characterized in that: The zinc salt in step (1) includes any one of zinc chloride, zinc nitrate or zinc acetate, or a combination of at least two of them.
4. The preparation method according to claim 1, characterized in that: The organic ligand in step (1) comprises fumaric acid.
5. The preparation method according to claim 1, characterized in that: The solvent in step (1) includes N,N-dimethylformamide.
6. The preparation method according to claim 1, characterized in that: The reaction in step (1) comprises an oil bath heating reaction.
7. The preparation method according to claim 6, characterized in that: The temperature of the oil bath heating reaction is 85-120°C.
8. The preparation method according to claim 1, characterized in that: After the reaction in step (1) is completed, centrifugation and washing are performed in sequence.
9. The preparation method according to claim 1, characterized in that: In step (2), the mass ratio of the nickel-zinc precursor to the manganese salt is (2-10):
1.
10. The preparation method according to claim 1, characterized in that: The mass volume ratio of the nickel zinc precursor to the acid is 25:(5-25) mg / mL.
11. The preparation method according to claim 1, characterized in that: The acid includes hydrochloric acid.
12. The preparation method according to claim 1, characterized in that: The mass ratio of the buffer to the nickel-zinc precursor is (2-6):
1.
13. The preparation method according to claim 1, characterized in that: The reaction in step (2) includes an oil bath heating reaction and / or a water bath heating reaction.
14. The preparation method according to claim 13, characterized in that: The reaction temperature of the oil bath heating reaction is 80-110°C.
15. The preparation method according to claim 13, characterized in that: The reaction time of the oil bath heating is 90 to 180 minutes.
16. The preparation method according to claim 13, characterized in that: The temperature of the water bath heating reaction is ≥80°C.
17. The preparation method according to claim 13, characterized in that: The reaction time of the water bath heating reaction is 90 to 240 minutes.
18. The preparation method according to claim 1, characterized in that: The sintering temperature in step (3) is 450-700°C.
19. The preparation method according to claim 1, characterized in that: The sintering time in step (3) is 3 to 10 hours.
20. The preparation method according to claim 1, characterized in that: The preparation method comprises the following steps: (1) mixing a nickel salt, a zinc salt, an organic ligand and a solvent, and performing a heating reaction in an oil bath at 85 to 120° C. to obtain a nickel-zinc precursor; (2) mixing the nickel-zinc precursor, manganese salt, acid, buffer and solvent described in step (1), wherein the mass ratio of the nickel-zinc precursor to the manganese salt is (2-10):1, the mass volume ratio of the nickel-zinc precursor to the acid is 25:(5-25) mg / mL, and the mass ratio of the buffer to the nickel-zinc precursor is (2-6):1, and heating the mixture in an oil bath at 80-110° C. for 90-180 min to obtain nickel-manganese-zinc-based nanosheets; (3) Sintering the nickel-manganese-zinc-based nanosheets in step (2) at 450-700° C. for 3-10 hours to obtain the nickel-manganese oxide positive electrode material; the buffer comprises urea and / or ammonia water.
21. A positive electrode material, characterized in that The positive electrode material is prepared by the preparation method according to any one of claims 1 to 20.
22. A lithium ion battery, characterized in that: The lithium-ion battery comprises the nickel manganese oxide positive electrode material as claimed in claim 1 or the positive electrode material as claimed in claim 9.