A method for improving intergranular corrosion of the weld overlay layer on the inner wall of nickel-based weld overlay composite bends
By optimizing the welding and heat treatment processes of nickel-based weld overlay composite bends, the problem of intergranular corrosion in high-sulfur media environments was solved, thereby improving the corrosion resistance of nickel-based weld overlay composite bends and making them suitable for conveying high-sulfur media.
Patent Information
- Application Number
- CN202211054718.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-08-31
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-08-31
AI Technical Summary
Existing nickel-based weld overlay composite bends cannot achieve an intergranular corrosion rate of ≤1 mm/year in high sulfur-containing media environments, affecting their service life.
The surfacing layer is constructed using a single-gun welding method, combined with a specific cooling method (water cooling with a water pressure of 0.13 MPa ± 0.003 MPa and a temperature of 1020℃ ± 25℃) and heat treatment (quenching at 1030℃ + tempering at 530℃). The bending and heat treatment processes are optimized to ensure that the surfacing layer is flat, smooth, and has good mechanical properties.
The corrosion rate of the weld overlay layer on the inner wall of the nickel-based weld overlay composite bend is ≤1 mm/year, which improves the corrosion resistance and makes it suitable for harsh working conditions, especially for conveying high sulfur content media.
Smart Images

Figure CN115945865B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of natural gas pipeline technology, specifically to a method for improving intergranular corrosion of the weld overlay layer on the inner wall of a nickel-based weld overlay composite bend. Background Technology
[0002] Nickel-based weld overlay composite elbows consist of a carbon steel substrate with an inner wall weld overlay. The weld overlay material is Inconel 625, which has good corrosion resistance. However, its service life is shortened due to intergranular corrosion of the inner wall weld overlay. Before this invention, the corrosion rate of nickel-based weld overlay composite elbows was generally controlled to ≤5 mm / year according to the ASTM G28-02 test method. With this invention, the corrosion rate can be controlled to ≤1 mm / year.
[0003] The Sichuan Basin Dishanpo Gas Field Feixianguan Formation Gas Reservoir Development and Production Capacity Construction Project uses corrosion-resistant alloy composite bends with nominal DN150~DN300 and bending radius R≥5D. The main transport medium is sulfur-containing natural gas with a hydrogen sulfide content of approximately 15.5%. Under this medium environment, if the intergranular corrosion rate of the inner wall of the weld overlay cannot be ≤1 mm / year, its service life will be severely affected.
[0004] The weld overlay composite bends manufactured using existing technology, when subjected to intergranular corrosion tests according to ASTM G28-02, have an average corrosion rate of 3.53 mm, which cannot achieve ≤1 mm / year, thus failing to meet the requirements for intergranular corrosion in the transportation of high sulfur-containing media.
[0005] Through the improvements of this invention, the corrosion rate of the weld overlay layer on the inner wall of the manufactured weld overlay composite bend is only about 0.5 mm / year, achieving the requirement of ≤1 mm / year, and successfully solving the problem of intergranular corrosion in oil and gas transportation in high sulfur gas fields. Summary of the Invention
[0006] (a) Technical problems to be solved
[0007] To address the shortcomings of existing technologies, this invention provides a method for improving intergranular corrosion of the weld overlay layer on the inner wall of a nickel-based weld overlay composite bend. The corrosion rate of the weld overlay layer on the inner wall of the manufactured weld overlay composite bend is only about 0.5 mm / year, achieving the requirement of ≤1 mm / year, and successfully solving the problem of intergranular corrosion in oil and gas transportation in high-sulfur gas fields.
[0008] (II) Technical Solution
[0009] To address the problem of intergranular corrosion during oil and gas transportation in high-sulfur gas fields, this invention provides the following technical solution, comprising the following steps:
[0010] 1) Pre-bending welding: Under the premise that the raw materials have passed the re-inspection, the inner wall of the pipe is sandblasted and polished, and then a stainless steel alloy layer of specified length and thickness is welded using a hot wire TIG intelligent welding equipment with a single gun. The resulting weld layer is smoother and less prone to cracking during the bending process.
[0011] 2) Hot bending of composite straight pipe: After the weld overlay layer meets the standard, no solution treatment is performed. The pipe flows directly into the bending process. The bending temperature is 1020℃±25℃. The inner wall temperature at this temperature is measured to be about 940℃, which just meets the heat sensitization temperature of the nickel-based weld overlay layer. The pipe advances at a speed of 27mm±1.35mm per minute. The advancement is maintained at a constant speed and is not allowed to be interrupted. The heated forming area is water-cooled during bending. The cooling water pressure is 0.13Mpa±0.003Mpa and the cooling water temperature is 30℃±15℃.
[0012] 3) After the bending process is completed, the weld overlay is first subjected to non-destructive testing. If it passes the test, it is subjected to quenching (1030℃) + tempering (530℃) heat treatment. Quenching at 1030℃ can improve the intergranular corrosion resistance of the weld overlay. Tempering at 530℃ maintains the good strength, plasticity and toughness of the carbon steel substrate, and has good comprehensive mechanical properties. Physical and chemical tests are conducted according to relevant standards.
[0013] Preferably, before sandblasting the inner wall of the pipe, the inner wall needs to be cleaned to remove impurities and oil stains, remove rust, and expose the metallic color of the inner wall. Stainless steel wire brushes or special stainless steel wire wheels are used for cleaning during the welding process and between layers.
[0014] Preferably, the metal material and thickness for the pipe overlay welding are UNS N06625 / ≥3.6mm, the welding material for the pipe overlay welding is ERNiCrMo-3, the diameter of the welding material is 1.2mm, the arc voltage is 12-17V, the welding speed is 270mm / min, the backstep distance is 3.2mm, the swing width is 0mm, the pipe welding equipment is a hot wire TIG double gun overlay welding machine, and the bending equipment is a YWG-I-426 pipe bending machine.
[0015] Preferably, the pipe is hot-bent using a medium-frequency induction heating method.
[0016] Preferably, after the pipe cools, the surface of the bend is cleaned to remove welding slag, dirt and impurities.
[0017] Preferably, after the pipe is hot-burned, cooled, and its surface is cleaned, a post-hot-burning inspection is performed. The inspection includes visual inspection, dimensional and penetrant testing, ultrasonic testing, and magnetic particle testing. The visual inspection is performed according to NB / T 47013.7 standard, the penetrant testing is performed according to ASTM E165-2012 standard, the ultrasonic testing is performed according to ASTM A578-2017 standard, and the magnetic particle testing is performed according to ASTM A578-2015 standard.
[0018] The existing technical solutions mainly consist of the following three steps:
[0019] ① Pre-bending welding: After the raw materials have passed the re-inspection, the inner wall of the pipe is sandblasted and polished, and then a hot wire TIG intelligent welding equipment with two guns is used to weld a stainless steel alloy layer of a specified length and thickness.
[0020] ② Normalizing treatment before bending: The composite straight pipe after welding is placed in a heat treatment furnace for normalizing at 920℃.
[0021] ③ Hot bending of weld overlay composite straight pipe: After the weld overlay layer meets the standards, it enters the bending process. The bending temperature is 930℃±25℃, and the advance rate is 15mm±2.5mm per minute. The advance rate must be kept uniform and not interrupted. During bending, the heated forming area is water-cooled. The cooling water pressure is 0.25Mpa±0.025Mpa, and the cooling water temperature is 25℃±15℃.
[0022] ④ After the bending process is completed, the weld overlay is first subjected to non-destructive testing. If it passes the test, it is subjected to quenching (920℃) + tempering (530℃) heat treatment, and physical and chemical tests are conducted according to the phase observation standard.
[0023] (III) Beneficial Effects
[0024] Compared with the prior art, the present invention provides a method for improving intergranular corrosion of the weld overlay layer on the inner wall of a nickel-based weld overlay composite bend, which has the following beneficial effects:
[0025] 1. This method for improving intergranular corrosion of the weld overlay layer on the inner wall of nickel-based weld overlay composite bends improves upon existing technologies. The key points of this method are: single-gun welding during welding; cooling during bending (water cooling of the heated forming area during bending, with a water pressure of 0.13 MPa ± 0.003 MPa and a cooling water temperature of 30℃ ± 15℃); bending temperature (1020℃ ± 25℃, at which the inner wall temperature was measured to be 940℃, precisely meeting the heat sensitization temperature of the nickel-based weld overlay layer); and heat treatment (quenching (1030℃) + tempering (530℃) heat treatment after passing inspection, with quenching at 1030℃). Bends produced using this method have a smoother, more aesthetically pleasing inner wall weld overlay layer, are less prone to cracking, and exhibit ASTM G28-02 intergranular corrosion test results of ≤1 mm / year, demonstrating stronger corrosion resistance. They can be used in more demanding special working conditions, especially for transporting high-sulfur media.
[0026] 2. This method improves the intergranular corrosion of the weld overlay layer on the inner wall of nickel-based weld overlay composite bends. The core of this method lies in the following: cooling water pressure (0.13Mpa±0.003Mpa), bending temperature (1020℃±25℃), pushing speed (27mm±1.35mm per minute), and heat treatment temperature (quenching (1030℃) + tempering (530℃)). Bends made using this method have a smoother and more aesthetically pleasing weld overlay layer on the inner wall, are less prone to cracking, and the quenching at 1030℃ enhances the intergranular corrosion resistance of the weld overlay layer. The tempering treatment at 530℃ maintains the good strength, plasticity, and toughness of the carbon steel substrate, resulting in good comprehensive mechanical properties. The ASTM G28-02 intergranular corrosion test result is ≤1mm / year, indicating stronger corrosion resistance. It can be used in more demanding special working conditions, especially for the transportation of high sulfur-containing media. Attached Figure Description
[0027] Figure 1 This is a flowchart of a method for improving intergranular corrosion of the weld overlay layer on the inner wall of a nickel-based weld overlay composite bend, as proposed in this invention. Detailed Implementation
[0028] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0029] Please see Figure 1 A method for improving intergranular corrosion of the weld overlay layer on the inner wall of a nickel-based weld overlay composite bend, comprising the following steps:
[0030] 1) Pre-bending welding: Under the premise that the raw materials have passed the re-inspection, the inner wall of the pipe is sandblasted and polished, and then a stainless steel alloy layer of specified length and thickness is welded using a hot wire TIG intelligent welding equipment with a single gun. The resulting weld layer is smoother and less prone to cracking during the bending process.
[0031] 2) Hot bending of composite straight pipe: After the weld overlay layer meets the standard, no solution treatment is performed. The pipe flows directly into the bending process. The bending temperature is 1020℃±25℃. The inner wall temperature at this temperature is measured to be about 940℃, which just meets the heat sensitization temperature of the nickel-based weld overlay layer. The pipe advances at a speed of 27mm±1.35mm per minute. The advancement is maintained at a constant speed and is not allowed to be interrupted. The heated forming area is water-cooled during bending. The cooling water pressure is 0.13Mpa±0.003Mpa and the cooling water temperature is 30℃±15℃.
[0032] 3) After the bending process is completed, the weld overlay is first subjected to non-destructive testing. If it passes the test, it is subjected to quenching (1030℃) + tempering (530℃) heat treatment. Quenching at 1030℃ can improve the intergranular corrosion resistance of the weld overlay. Tempering at 530℃ maintains the good strength, plasticity and toughness of the carbon steel substrate, and has good comprehensive mechanical properties. Physical and chemical tests are conducted according to relevant standards.
[0033] Example 1: Before sandblasting the inner wall of the pipe, it is necessary to clean the inner wall of the pipe to remove impurities, oil stains and rust, so that the inner wall of the pipe is exposed to the metal color. Stainless steel wire brush or stainless steel wire wheel is used for cleaning during welding process and interlayer cleaning.
[0034] Example 2: The metal material and thickness used for pipe surfacing are UNS N06625 / ≥3.6mm, the welding material is ERNiCrMo-3, the diameter is 1.2mm, the arc voltage is 12-17V, the welding speed is 270mm / min, the backstep distance is 3.2mm, the swing width is 0mm, the pipe welding equipment is a hot wire TIG double gun surfacing machine, and the bending equipment is a YWG-I-426 pipe bending machine.
[0035] Example 3: Medium-frequency induction heating is used for hot bending of the pipe. After cooling, the surface of the bent pipe is cleaned to remove welding slag, dirt, and impurities. Following hot bending, cooling, and surface cleaning, post-hot bending inspection is performed, including visual inspection, dimensional and penetrant testing, ultrasonic testing, and magnetic particle testing. Visual inspection is conducted according to NB / T47013.7 standard; penetrant testing according to ASTM E165-2012 standard; ultrasonic testing according to ASTM A578-2017 standard; and magnetic particle testing according to ASTM A578-2015 standard.
[0036] Example 4:
[0037] A comparative test of intergranular corrosion was conducted on the composite bend produced by this method and the composite bend produced by existing methods:
[0038] The experimental data for this method are as follows:
[0039]
[0040] The test conditions and results for intergranular corrosion of the composite bend fabricated using this method are as follows:
[0041]
[0042] Therefore, it can be concluded that the average corrosion rate of the composite bend made by the method of the present invention, tested according to ASTM G28-2 (2015), is 0.34 mm / a, which meets the target that the corrosion rate should not exceed 1 mm / a.
[0043] The experimental data for the existing technical methods are as follows:
[0044]
[0045] The test conditions and results for intergranular corrosion of composite bends manufactured using existing techniques are as follows:
[0046]
[0047] Therefore, it can be concluded that the average corrosion rate of composite bends manufactured using existing techniques, tested according to ASTM G28-2 (2015), is 3.53 mm / a, which does not meet the target of a corrosion rate not exceeding 1 mm / a. The above two tests demonstrate the superiority of this method.
[0048] Example 5: Two types of weld overlay composite bends have been successfully trial-produced using this process and delivered in the Feixianguan Formation gas reservoir development capacity construction project of the Dishanpo gas field in the Sichuan Basin.
[0049] The materials and specifications of the weld overlay composite bend are as follows:
[0050] L360QS+inconel625 323.9×(15+3)㎜ R=6D.
[0051] In summary, this method for improving intergranular corrosion of the weld overlay layer on the inner wall of nickel-based weld overlay composite bends improves upon existing technologies. The key points of this method are: single-gun welding during welding; cooling during bending (water cooling of the heated forming area during bending, with a water pressure of 0.13 MPa ± 0.003 MPa and a cooling water temperature of 30℃ ± 15℃); bending temperature (1020℃ ± 25℃, at which the inner wall temperature was measured to be 940℃, precisely meeting the heat sensitization temperature of the nickel-based weld overlay layer); and heat treatment (quenching (1030℃) + tempering (530℃) heat treatment after passing inspection, with quenching at 1030℃). Bends produced using this method have a smoother, more aesthetically pleasing inner wall weld overlay layer, are less prone to cracking, and exhibit ASTM G28-02 intergranular corrosion test results of ≤1 mm / year, demonstrating stronger corrosion resistance. They can be used in more demanding special working conditions, especially for transporting high-sulfur media.
[0052] 2. The core of this method lies in the cooling water pressure (0.13Mpa±0.003Mpa), bending temperature (1020℃±25℃), pushing speed (27mm±1.35mm per minute), and heat treatment temperature (quenching (1030℃) + tempering (530℃)). Bending pipes produced using this method have a smoother and more aesthetically pleasing inner wall weld overlay, are less prone to cracking, and the 1030℃ quenching enhances the intergranular corrosion resistance of the weld overlay. The subsequent tempering at 530℃ maintains the good strength, plasticity, and toughness of the carbon steel substrate, resulting in excellent comprehensive mechanical properties. The ASTM G28-02 intergranular corrosion test result is ≤1mm / year, indicating stronger corrosion resistance. This allows the pipe to be used in more demanding special working conditions, especially for transporting high-sulfur media.
[0053] It should be noted that, in this document, relational terms such as "first" and "second" are used merely to distinguish one entity or operation from another, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Furthermore, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Without further limitations, an element defined by the phrase "comprising one" does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes said element.
[0054] Although embodiments of the invention have been shown and described, it will be understood by those skilled in the art that various changes, modifications, substitutions and alterations can be made to these embodiments without departing from the principles and spirit of the invention, the scope of which is defined by the appended claims and their equivalents.
Claims
1. A method for improving intergranular corrosion of the weld overlay layer on the inner wall of a nickel-based weld overlay composite bend, characterized in that, Includes the following steps: 1) Pre-bending welding: After inspecting the raw materials and ensuring they pass the re-inspection, the inner wall of the pipe is sandblasted and ground. Then, a stainless steel alloy layer of specified length and thickness is welded using a hot-wire TIG intelligent welding machine with a single gun. The metal material and thickness used for pipe welding are UNS N06625 / ≥3.6mm, the welding material is ERNiCrMo-3, the diameter is 1.2mm, the arc voltage is 12-17V, the welding speed is 270mm / min, the backstep distance is 3.2mm, the swing width is 0mm, the pipe welding equipment is a hot-wire TIG double-gun welding machine, and the bending equipment is a YWG-I-426 pipe bending machine. 2) Hot bending of composite straight pipe: The weld overlay is inspected. If the weld overlay meets the standard, no solution treatment is performed. The pipe is directly fed into the bending process. The bending temperature is 1020℃±25℃. The inner wall temperature at this temperature is measured to be 940℃, which just meets the heat sensitization temperature of the nickel-based weld overlay. The pipe is advanced at a speed of 27mm±1.35mm per minute. The advancement is kept at a constant speed and is not allowed to be interrupted. The heated forming area is water-cooled during bending. The cooling water pressure is 0.13Mpa±0.003Mpa and the cooling water temperature is 30℃±15℃. 3) After the bending process is completed, the weld overlay is subjected to non-destructive testing. If it passes the test, it is subjected to quenching and tempering heat treatment, quenching at 1030℃ and tempering at 530℃.
2. The method for improving intergranular corrosion of the weld overlay layer on the inner wall of a nickel-based weld overlay composite bend according to claim 1, characterized in that: Before sandblasting the inner wall of the pipe, it is necessary to clean the inner wall to remove impurities, oil stains, and rust, so that the inner wall of the pipe is exposed to a metallic color. Stainless steel wire brushes or special stainless steel wire wheels are used for cleaning during the welding process and between layers.
3. The method for improving intergranular corrosion of the weld overlay layer on the inner wall of a nickel-based weld overlay composite bend according to claim 1, characterized in that: The pipe is hot-bent using a medium-frequency induction heating method.
4. The method for improving intergranular corrosion of the weld overlay layer on the inner wall of a nickel-based weld overlay composite bend according to claim 1, characterized in that: After the pipe cools down, the surface of the bend is cleaned to remove welding slag, dirt and impurities.
5. The method for improving intergranular corrosion of the weld overlay layer on the inner wall of a nickel-based weld overlay composite bend according to claim 1, characterized in that: After the pipe is hot-bent, cooled, and its surface is cleaned, it undergoes post-hot-bent inspection. Visual inspection, dimensional and penetrant testing, ultrasonic testing, and magnetic particle testing are performed first. Visual inspection is conducted according to NB / T 47013.7 standard, penetrant testing is conducted according to ASTM E165-2012 standard, ultrasonic testing is conducted according to ASTM A578-2017 standard, and magnetic particle testing is conducted according to ASTM A578-2015 standard.
Citation Information
Patent Citations
Low temperature-resistant K60 pipe line steel, bent pipe made by same and manufacturing method of bent pipe
CN102383057A
Method for processing bent pipe with inner wall subjected to surfacing welding
CN102950427A
High steel grade bend pipe and preparation method
CN108048747A