Preparation method of modified iron phosphate for high-rate lithium iron phosphate anode material
By using refined ammonium dihydrogen phosphate and ferrous sulfate solution to react and adding resol phenolic resin and cetyltrimethylammonium acetate in the preparation process of lithium iron phosphate anode material to form a uniform conductive carbon film, the problem was solved The problem of uneven conductivity and lithium ion insertion/extraction rate improves the high-rate charge and discharge performance of the battery.
Patent Information
- Application Number
- CN202211605830.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-14
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2042-12-14
AI Technical Summary
Existing lithium iron phosphate anode materials have inhomogeneities in their conductivity and lithium ion insertion/extraction rate during high-rate charge and discharge processes, which affects battery performance, and existing technology cannot effectively improve the formation and distribution consistency of conductive carbon films.
Refined ammonium dihydrogen phosphate solution and ferrous sulfate solution are continuously reacted to generate iron phosphate slurry, and after filtering and washing, resol phenolic resin and cetyltrimethylammonium acetate are added for slurry treatment to generate preliminary carbonization. And highly active magnesium oxide iron phosphate powder is spray dried and oxygen-isolated roasted to form a uniform conductive carbon film.
Significantly improves the formation and distribution consistency of the conductive carbon film, improves the conductivity of lithium iron phosphate powder and the high-rate charge and discharge performance of the battery, achieving a conductive effect similar to graphene or carbon nanotubes, and has a high cost-effectiveness Suitable for battery level production.
Smart Images

Figure BDA0003997783110000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium iron phosphate anode materials, and in particular relates to a method for preparing modified iron phosphate for high-rate lithium iron phosphate anode materials. Background Art
[0002] Lithium iron phosphate batteries have become the mainstream of power batteries and energy storage batteries due to their long cycle life, good safety, and improved design level. Their production capacity and output are showing a blowout trend. The output of lithium iron phosphate powder, the anode material used, has reached nearly 500,000 tons in 2021 and is expected to exceed 1 million tons in 2022. In some application scenarios of power batteries, it is sometimes necessary to charge more than 80% of the power in about half an hour, or sometimes it is necessary to output more than 20% of the power in about 3 minutes. High-rate lithium iron phosphate power batteries refer to batteries whose performance is basically unaffected during and after very frequent rapid charging and discharging processes. The most important condition for the production of high-rate lithium iron phosphate power batteries is high-rate lithium iron phosphate powder materials. In order to ensure the consistency of the performance of lithium iron phosphate power batteries, the performance of lithium iron phosphate powder materials should have higher consistency.
[0003] At present, the main production process of lithium iron phosphate powder, anode material, is the high-temperature solid phase synthesis method. The conventional operation process of producing lithium iron phosphate powder by the high-temperature solid phase synthesis method includes: firstly preparing battery-grade iron phosphate powder, lithium carbonate powder, carbon source such as sucrose, pure water or ethanol and a small amount of additives into slurry, grinding to a fine powder particle size of 0.1-0.5μm, spray drying to obtain a powder such as D 50 The spherical powder of 20-40μm is then reduced and sintered at 680-750℃ to obtain D 50 The spherical powder of 15-30μm is crushed by air flow to obtain D 50 1-2μm and lithium iron phosphate microsphere powder with appropriate particle size distribution. When preparing the slurry, a grinding dispersant can be added, and a doping element component that improves the intrinsic conductivity of lithium iron phosphate can be added; the D 50 The 1-2μm lithium iron phosphate microspheres are composed of dozens or hundreds of lithium iron phosphate primary crystals with an olivine structure, and the surface of the primary crystals is coated with a conductive carbon film. During the reduction sintering process, reducing components such as aldehydes and CO generated by thermal decomposition of sucrose reduce iron phosphate to ferrous phosphate, which then reacts with lithium ions in a solid phase to form lithium iron phosphate primary crystals with an olivine structure; a certain amount of carbon generated by thermal decomposition of sucrose forms a conductive coating thin layer on the surface of the lithium iron phosphate primary crystals, forms a conductive connecting carbon layer between the primary crystals, and also forms a conductive carbon film on the surface of the D 50The surface of the 15-30μm lithium iron phosphate spherical powder forms a conductive carbon-rich shell. The formation of the carbon-rich shell is due to the difference between the non-water-soluble properties of iron phosphate and lithium carbonate and the extremely high water-soluble properties of sucrose, which makes the spray-dried powder such as D 50 In the 20-40μm spherical powder, sucrose is enriched on the surface of the spherical powder particles; therefore, the D 50 There is a very significant and inevitable uneven distribution of the conductive carbon coating amount, thickness and density between 1-2μm lithium iron phosphate microspheres. In short, the conventional production process of lithium iron phosphate powder for anode materials, such as D 50 For 1-2μm lithium iron phosphate microsphere powder, there are very significant differences in the conductivity and the influence of the conductive carbon coating layer on the insertion / extraction rate of lithium ions, between the lithium iron phosphate microspheres and between the primary grains within the microspheres. This difference or inconsistency significantly affects the charge and discharge performance of the final lithium iron phosphate battery.
[0004] Therefore, it is necessary to improve the carbon film coating, element doping and distribution uniformity, which play an important role in the conductivity of lithium iron phosphate microspheres and the insertion / extraction rate of lithium ions. To achieve this goal, the slurry ratio, grinding depth, spray drying conditions, reduction sintering conditions, and air flow crushing intensity are generally comprehensively controlled. This is a matter that must be considered and optimized from beginning to end in the high-temperature solid-phase synthesis lithium iron phosphate test and production.
[0005] For example, CN109192953A provides a high-rate spherical lithium iron phosphate carbon composite positive electrode material and a preparation method thereof, wherein the positive electrode material comprises the following raw material components: iron phosphate, lithium source, carbon source A, metal oxide additive, dispersant and carbon source B; wherein: the Li element in the lithium source accounts for 6.0-8.0% of the mass of the iron phosphate; the carbon source A accounts for 0.3-12.5% of the mass of the iron phosphate; the metal oxide additive accounts for 0.5-5.0% of the mass of the iron phosphate; the dispersant accounts for 0.2-1.5% of the mass of the iron phosphate; and the carbon source B accounts for 1-15.0% of the mass of the iron phosphate. The preparation method comprises the following steps: (1) batching and grinding; (2) spray drying and granulation; (3) heat treatment, wherein the carbon source A and the metal oxide additive are added during the grinding process, and the carbon source B is added during the heat treatment process. The lithium iron phosphate positive electrode material prepared by the present invention is a spherical particle, the surface and the interior of which are uniformly coated with metal-doped carbon, with high conductivity, good crystallinity, and a tap density of 1.3-1.8 g / cm 3 , its 10C discharge capacity can reach 148mAh / g.
[0006] CN114314548A provides a titanium and zirconium co-doped carbon-coated lithium iron phosphate positive electrode material and its preparation method and application. The chemical expression of the material is Li 1-y Zr y Fe 1-xTi x PO4 / C, wherein titanium is doped to the Fe position, zirconium is doped to the Li position, and 0.001≤x≤0.05, 0.001≤y≤0.02; its preparation method is to mix iron phosphate, lithium carbonate, carbon source, titanium source and zirconium source in a liquid medium, and then the mixture is ball-milled and sand-milled to a certain slurry particle size, and then granulated by spray drying technology, and finally the dried spray material is sintered in an atmosphere furnace. The present invention effectively enhances the ion and electron transmission capacity of lithium iron phosphate by adding titanium and zirconium elements to carbon-coated lithium iron phosphate, improves the compaction density of the material, and is suitable for use as a positive electrode material for high-energy and high-power density lithium-ion power batteries.
[0007] The CN109192953A, CN114314548A or similar prior arts do not involve the modification of ferric phosphate during the preparation of ferric phosphate powder.
[0008] CN106185857A provides a battery-grade iron phosphate and a preparation method thereof, wherein the molar ratio of phosphorus to iron of the battery-grade iron phosphate is 1.03-1.05, the Ti content is 0.2-0.5%, and the Mn content is 0.02-0.05%. The preparation method is to first prepare a phosphoric acid or phosphate solution of a certain concentration and an iron salt solution of a certain concentration, and then prepare a dihydrate iron phosphate doped with titanium and manganese by adding titanium salt and manganese salt in liquid phase synthesis, and then washing and drying. The lithium iron phosphate further prepared by the battery-grade dihydrate iron phosphate synthesized by the present invention has high electronic conductivity, and its 0.2C specific capacity can reach 160mAh / g.
[0009] In the prior art, there are also attempts to prepare lithium iron phosphate containing graphene or carbon nanotubes by adding a small amount of graphene or carbon nanotubes to the grinding ingredients for preparing lithium iron phosphate from raw materials such as iron phosphate, lithium carbonate, and sucrose, and to add a small amount of graphene or carbon nanotubes to the grinding ingredients for preparing lithium iron phosphate anode slurry, thereby ultimately improving the conductivity of lithium iron phosphate anode materials. However, the effect on improving the high-rate performance of lithium iron phosphate batteries is limited, mainly because there is a certain contradiction between the conductivity and dispersion properties of graphene or carbon nanotubes.
[0010] None of the above-mentioned prior arts involve introducing or forming appropriate carbon-containing materials during the preparation process of lithium iron phosphate powder, which carbon-containing materials can generate partial conductive carbon film in lithium iron phosphate microspheres or significantly improve the generation of conductive carbon film, or can improve the consistency of conductive carbon film distribution, so that the prepared lithium iron phosphate anode material has better high-rate performance, and the further prepared lithium iron phosphate battery has high-rate charge and discharge performance that meets the latest technological requirements. Summary of the invention
[0011] In order to solve the above technical problems, the present invention provides a method for preparing modified iron phosphate for high-rate lithium iron phosphate anode materials, which comprises the following steps: continuously reacting a refined ammonium dihydrogen phosphate solution, a ferrous sulfate solution and hydrogen peroxide, filtering and washing the generated iron phosphate slurry after aging, and providing a slurry treatment step after washing the iron phosphate, coating a water-soluble resol phenolic resin and hexadecyltrimethylammonium acetate capable of generating a carbon-containing material, and magnesium acetate, a magnesium-doped raw material capable of improving the intrinsic conductivity of primary grains for further preparing lithium iron phosphate, and then spray drying and oxygen-isolated roasting to generate an iron phosphate powder containing an appropriate amount of preliminary carbon and highly active magnesium oxide. The 0.5-1.0wt% initial carbon contained in the iron phosphate powder is mostly dispersed into nano-thin sheets with an outer size of less than 30nm during the grinding of the ingredients in the process of producing lithium iron phosphate powder by high-temperature solid phase synthesis. It can generate a part of the conductive carbon film in the lithium iron phosphate and significantly improve the generation of the conductive carbon film and the distribution consistency of the conductive carbon film; the high-activity magnesium oxide containing 1.5-2.5mol% of the iron phosphate forms a good doping in the process of preparing lithium iron phosphate, which improves the intrinsic conductivity of the primary grains of lithium iron phosphate; therefore, the prepared lithium iron phosphate powder has good high-rate performance, and the further prepared lithium iron phosphate battery has a high-rate charge and discharge performance that meets the latest technical requirements. This method has a high cost-effectiveness ratio and is suitable for battery-grade iron phosphate manufacturers.
[0012] The present invention provides a method for preparing a modified iron phosphate for a high-rate lithium iron phosphate anode material, comprising the following steps:
[0013] (1) The slurry in the precipitation reaction tank is continuously stirred and the slurry temperature is controlled at 50-60°C; the circulating slurry in one channel of the precipitation reaction tank is continuously mixed with a 1.0-2.0 mol / L, 50-60°C refined ferrous sulfate aqueous solution at a required flow rate, respectively, at a volume flow rate ratio of 5-10:1, and then continuously mixed with a 50-60°C hydrogen peroxide aqueous solution at a required flow rate, and then continuously mixed with a 1.5-2.5 mol / L, 50-60°C refined ammonium dihydrogen phosphate aqueous solution at a required flow rate, and then injected into the slurry in the precipitation reaction tank; the other circulating slurry in the precipitation reaction tank is continuously mixed with a 4.0-8.0 mol / L, 50-60°C ammonia water at a volume flow rate ratio of 10- The volume flow ratio is 20:1, and after continuous mixing, it is injected into the slurry in the precipitation reaction tank, and the pH value of the slurry is controlled to be in the range of 2.0-2.3; the slurry in the precipitation reaction tank continuously flows into the aging treatment tank through the high-position discharge port, and the slurry temperature in the aging treatment tank is controlled to be 70-80°C for aging treatment; wherein, the feeding molar ratio of ferrous sulfate and diammonium phosphate is controlled to be 0.96-0.98:1, and the feeding molar ratio of H2O2 and ferrous sulfate is controlled to be 0.60-0.65; the average residence time of the slurry in the precipitation reaction tank is 0.5-1h, and the aging treatment time in the aging treatment tank is 8-12h. During the aging treatment process, only low-speed stirring is performed to ensure that the solid content is roughly evenly dispersed in the slurry;
[0014] (2) After the aging treatment in step (1), the slurry is filtered through a belt filter or a plate and frame filter, and washed with water at 70-80° C. until the effluent conductivity is ≤150 μS / cm. The filter cake is transferred into a slurry treatment tank, and magnesium acetate or its aqueous solution accounting for 1.5-2.5 mol% of iron phosphate is added, stirred evenly, and a resin aqueous solution is added for slurrying, and a slurry treatment is performed, and the slurry treatment time is 0.5-1 h. The slurry for slurry treatment is prepared according to the solid content concentration of iron phosphate dihydrate of 45-50 wt% and the solid content concentration of phenolic resin of 0.5-1.0 wt%; the resin aqueous solution contains phenolic resin with a weight average molecular weight of 2000-3000 and hexadecyltrimethylammonium acetate, wherein the weight percentage concentration ratio of the phenolic resin to the hexadecyltrimethylammonium acetate based on the solid content is 1:0.1-0.15;
[0015] (3) The slurry after the slurry treatment in step (2) is spray-dried at 200-250° C., and the dried material is roasted in an oxygen-proof furnace at 500-550° C. for 4-8 hours and crushed to obtain modified iron phosphate.
[0016] In the preparation method of the modified iron phosphate for high-rate lithium iron phosphate anode material of the present invention, according to the specific effects and comparisons in the operation process of the subsequent related embodiments and comparative examples, it can be inferred that the phenolic resin and hexadecyltrimethylammonium acetate introduced into the dihydrate iron phosphate slurry before spray drying can be roughly evenly distributed on the surface and between the grains of the iron phosphate grains of the spherical powder obtained by spray drying, and a certain amount of initial carbon, such as 40-50% of the amount of phenolic resin added, is formed between the anhydrous iron phosphate grains in the modified iron phosphate powder obtained by roasting at 500-550° C. in an oxygen-proof furnace, and the initial carbon formed is also roughly evenly distributed on the surface and between the anhydrous iron phosphate grains in the iron phosphate powder; the obtained modified iron phosphate powder, In the process of producing lithium iron phosphate powder by high temperature solid phase synthesis method, as the iron phosphate powder, lithium carbonate powder, sucrose and water slurry are ground to a fine powder particle size such as 0.2-0.5 μm, the 0.5-1.0wt% preliminary carbon contained in the iron phosphate powder is mostly dispersed into nano flakes with an outer size of less than 30nm. Although the weight content of the preliminary carbon is not high, the number of dispersed nano flakes is large, part of which adheres to the surface of lithium carbonate crystal grains, and part of which still adheres to the surface of anhydrous iron phosphate crystal grains, thereby improving the binding ability of sucrose liquid with the surface of lithium carbonate crystal grains and the surface of anhydrous iron phosphate crystal grains in the grinding slurry, and part of the nano flakes are dispersed into the sucrose liquid to reduce the fluidity of the sucrose liquid, so that the spray-dried product such as D 50 The distribution uniformity of sucrose in the 20-40μm spherical powder is significantly improved, and the surface enrichment of the spherical powder is significantly reduced. After reduction sintering at 680-750℃, the obtained D 50 The surface of the 15-30μm lithium iron phosphate spherical powder basically no longer forms a carbon-rich shell, so that the lithium iron phosphate spherical powder is neutralized by air flow pulverization, such as D 50 In the 1-2 μm lithium iron phosphate microspheres, the conductive carbon film generated by sucrose and the preliminary carbonized nanosheets has significantly improved coating and coating uniformity on the surface of the lithium iron phosphate primary crystal grains and between the primary crystal grains. Under the same conductive carbon coating amount conditions and the same sucrose carbon generation coating amount conditions, the charge and discharge performance of the lithium iron phosphate battery finally prepared is much better than when the phenolic resin and / or hexadecyltrimethylammonium acetate are not introduced in step (2). Therefore, the phenolic resin and hexadecyltrimethylammonium acetate introduced in step (2) are calcined in an oxygen-proof furnace at 500-550° C. in step (4) to generate preliminary carbon. In the process of using iron phosphate for high-temperature solid-phase synthesis to produce lithium iron phosphate powder, in addition to being basically converted into conductive carbon, it can also significantly improve the generation of conductive carbon film and improve the distribution consistency of conductive carbon film, thereby improving the electrical properties of lithium iron phosphate powder. The conductive effect is equivalent to or better than that of graphene and carbon nanotubes specially added with good conductivity and dispersibility.
[0017] In the method for preparing modified iron phosphate for high-rate lithium iron phosphate anode material of the present invention, the magnesium acetate accounting for 1.5-2.5 mol% of the iron phosphate added during the slurry treatment in step (2) can improve the intrinsic conductivity of primary grains for further preparing lithium iron phosphate. It can be seen from the relevant embodiments and comparative examples that the same amount of magnesium acetate is better when added in this step than when added during the grinding and mixing of iron phosphate powder with lithium carbonate powder, sucrose and water slurry. The reason is that, except for a small part of the added magnesium ions being adsorbed and combined with ferric phosphate dihydrate, most of the added magnesium ions are calcined at 500-550°C in the oxygen-tight furnace in step (4) to generate highly active and widely dispersed magnesium oxide. During the process of using iron phosphate powder for high-temperature solid phase synthesis to produce lithium iron phosphate powder, the magnesium oxide is ground into a fine powder such as 0.2-0.5 μm with the iron phosphate powder, lithium carbonate powder, sucrose and water slurry, and is further dispersed by hydrolysis into colloidal magnesium hydroxide. After further reduction sintering at 680-750°C, most of the magnesium oxide is doped and enters the lattice of lithium iron phosphate primary grains. If magnesium acetate is added during the grinding of iron phosphate powder with lithium carbonate powder, sucrose and water slurry, the presence of a large amount of lithium carbonate causes the magnesium ions to form magnesium carbonate which is not easy to gel and has a low dispersion. After further reduction sintering at 680-750°C, the magnesium ions that are doped and enter the lattice of the primary lithium iron phosphate grains are less or less uniform, resulting in an inconsistent effect on improving the intrinsic conductivity of the prepared primary lithium iron phosphate grains and a poor overall doping effect. At the same time, the lithium acetate generated by the reaction of magnesium acetate and lithium carbonate has a much higher solubility than lithium carbonate and is easily enriched on the surface of the spherical powder particles obtained by further spray drying, resulting in uneven quality and decreased performance of the final lithium iron phosphate powder.
[0018] The phenolic resin can be prepared by the following steps: using a stirred reactor with condensation reflux and vacuum distillation; after sealing and replacing air, adding water and a formaldehyde aqueous solution with a concentration of 37-40wt% and phenol under continuous stirring, sealing the reactor, heating to 60-70°C, adding ammonia water dropwise for reaction for 20-30min, heating to 70-75°C for reaction for 20-30min, heating to 85-90°C and maintaining the temperature for reaction for 2-3h, then performing vacuum distillation for 2-4h until the solid concentration in the feed liquid reaches 35-40wt%, cooling to room temperature, and obtaining the phenolic resin; wherein the ingredients are water, formaldehyde aqueous solution, phenol, and ammonia in a weight ratio of 0.5-1.0:1.3-1.6:1:0.03-0.05; the vacuum distillation conditions include: a reaction feed liquid temperature of 70-80°C, an exhaust vacuum absolute pressure of 30-45kPa, and a condensation temperature of 10-25°C. The obtained phenolic resin is a resol phenolic resin, containing formaldehyde ≤ 0.1wt%, phenol ≤ 0.1wt%, with little odor, no visible change after being stored in a dark place for 1 month, and the use effect is the same as that of the newly prepared one, and can be diluted with water for use. Its weight average molecular weight can be determined by viscosity and concentration.
[0019] The hexadecyl trimethyl ammonium acetate, as a cationic surfactant, can be used as a morphology regulator in the process of preparing ferric phosphate by precipitation method, but the concentration in the slurry is generally 5g / L or above 0.4wt%, which is much higher than the concentration of 0.05-0.15wt% used in the present invention, and there is no similar application as the phenolic resin coating auxiliary agent in the prior art. The advantage of using the hexadecyl trimethyl ammonium acetate is that it avoids the hazards of high temperature corrosion such as nitrogen oxides and chlorides generated by hexadecyl trimethyl ammonium nitrate and hexadecyl trimethyl ammonium chloride.
[0020] It is inferred that in the resin aqueous solution, a certain degree of complexation should occur between the phenolic resin and hexadecyltrimethylammonium acetate. The modified iron phosphate obtained in step (3) is gray, and the detection shows that 0.5-1.0wt% of residual carbon is generated, and the carbon deposition rate is relatively certain, which is convenient for subsequent accurate batching and formation of lithium iron phosphate powder with the required determined carbon content.
[0021] In the prior art of producing lithium iron phosphate powder by high-temperature solid phase synthesis, there are also records of adding polymers such as phenolic resin when grinding and preparing iron phosphate powder, lithium carbonate powder and water slurry. However, the subsequent related embodiments and comparative examples show that the effect of introducing phenolic resin and hexadecyltrimethylammonium acetate into the dihydrate iron phosphate slurry before spray drying is better in the present invention. The reason is inferred to be that when adding polymers such as phenolic resin when grinding and preparing iron phosphate powder, lithium carbonate powder, sucrose and water slurry, even if combined with sucrose and glucose, the dispersion effect of the present invention cannot be achieved under the condition of obtaining the same conductive carbon coating amount, and thus the overall conductive effect is worse.
[0022] In step (1), a circulating slurry of the precipitation reaction tank is continuously mixed with a refined ferrous sulfate aqueous solution at a volume flow ratio of 5-10:1, and then continuously mixed with a hydrogen peroxide aqueous solution, and further continuously mixed with a refined diammonium phosphate aqueous solution, and then injected into the precipitation reaction tank slurry. This is the key to completely oxidizing ferrous ions to generate trivalent iron ions when the feed molar ratio of H2O2 to ferrous sulfate is only 0.60-0.65. The circulating slurry provides the acidic conditions required for the oxidation reaction, and the rapid mixing and oxidation reaction reduce the concentration of H2O2 in the mixed slurry and the precipitation reaction tank slurry and the decomposition effect of the contained dihydrate ferric phosphate on H2O2; another circulating slurry of the precipitation reaction tank is continuously mixed with ammonia water at a volume flow ratio of 10-20:1 and then injected into the precipitation reaction tank slurry, and the slurry pH value is controlled to be in the range of 2.0-2.3, and the feed liquid temperature is controlled to be 50-60°C. This is the key to ensuring that the precipitation reaction is complete and the amount of iron hydroxide impurities generated is low. In the prior art, the refined ferrous sulfate aqueous solution, hydrogen peroxide aqueous solution, ammonium dihydrogen phosphate aqueous solution, and ammonia water as the raw materials of the precipitation reaction are generally injected into the slurry of the precipitation reaction tank respectively, and the mixing efficiency is low. Even if a precipitation reaction tank with a special structure is used, the precipitation reaction is not easy to be complete, and the amount of iron hydroxide impurities generated is large. The aging of the slurry cannot ensure that all iron hydroxides are converted into dihydrate iron phosphate, and additional phosphoric acid is often required to convert iron hydroxide into dihydrate iron phosphate. The iron hydroxide impurities are the main harmful components of iron phosphate, and will eventually generate metal iron dendrites in the anode sheet during the high-rate charge and discharge cycle of the lithium iron phosphate battery, causing serious harm, and significantly accelerating the rate of reduction of the cycle performance of the lithium iron phosphate battery. In step (1), since the precipitation reaction is complete and the amount of iron hydroxide impurities generated is low, the aging process not only causes the necessary recrystallization of dihydrate iron phosphate, but also generates dihydrate iron phosphate, which is convenient for the filtering and washing operations of step (2). The pH value of the precipitation reaction slurry in step (1) can be easily controlled within the range of 2.0-2.3, which can better control the amount of iron hydroxide impurity phase generated, and no phosphoric acid needs to be added during the aging treatment.
[0023] The continuous mixing of the solution and slurry in step (1) can be carried out by a static mixer or a venturi arranged in the pipeline, both of which have the advantages of high mixing efficiency and fast mixing rate, can avoid or reduce the occurrence of side reactions, and have a good reaction effect of producing ferric phosphate dihydrate.
[0024] After filtration in step (2), the filter cake is washed with water at 70-80° C. until the effluent conductivity is ≤150 μS / cm. At this time, the effluent is tested with a 0.5 mol / L barium chloride-1.0 mol / L hydrochloric acid solution and no barium sulfate turbidity is observed, indicating that the sulfate ions have been washed away. DETAILED DESCRIPTION
[0025] The technical solution of the present invention is specifically described and illustrated below in conjunction with embodiments, but does not constitute a limitation of the present invention.
[0026] Example 1
[0027] The resol phenolic resin was prepared according to the following steps: a 3L stirred reactor with condensation reflux and vacuum distillation was used; the reactor was evacuated to an absolute pressure of 10 kPa, filled with 99.9% nitrogen to 300 kPa, and the evacuation and nitrogen filling operations were repeated 3 times to test the tightness and replace the air; under continuous stirring, 800 g of water, 1500 g of 37 wt% formaldehyde aqueous solution, and 1000 g of phenol were added in sequence, the reactor was sealed, and heating was performed immediately. After 20 minutes, the feed liquid was heated to 65°C, and 400 ml of 6 mol% ammonia water was added dropwise. The reaction was continued for 20 minutes, the temperature was raised to 73°C for 30 minutes, the temperature was raised to 85°C and the temperature was maintained for 3 hours, and then vacuum distillation was performed for 1 hour until the solid concentration in the feed liquid reached 38wt%, and the mixture was cooled to room temperature to obtain a resol phenolic resin; the vacuum distillation conditions included: a reaction feed liquid temperature of 76-80°C, an absolute vacuum pressure of 35kPa, and a condensation temperature of 15°C; the obtained resol phenolic resin contained formaldehyde ≤0.1wt%, phenol ≤0.1wt%, had a small odor, and had no visible change after being stored in a dark place for 1 month. According to the test results of its viscosity and concentration at 25°C, its weight average molecular weight was estimated to be 2600.
[0028] Example 2
[0029] On a test line with an hourly production capacity of about 3 kg of iron phosphate, about 10 kg of modified iron phosphate of this embodiment was prepared according to the following steps:
[0030] (1) The slurry in the precipitation reaction tank is continuously stirred and the slurry temperature is controlled at 55°C; the circulating slurry in one channel of the precipitation reaction tank is continuously mixed with a 1.8 mol / L, 56°C refined ferrous sulfate aqueous solution at a required flow rate, respectively, at a volume flow rate ratio of 7.5:1, and then continuously mixed with a 2.0 mol / L, 52°C hydrogen peroxide aqueous solution at a required flow rate, and then continuously mixed with a 2.2 mol / L, 56°C refined ammonium dihydrogen phosphate aqueous solution at a required flow rate, and then injected into the slurry in the precipitation reaction tank; the other circulating slurry in the precipitation reaction tank is continuously mixed with a 5.0 mol / L, 52°C ammonia water at a volume flow rate ratio of 1:1. 5:1 volume flow ratio, continuously mixed and then injected into the slurry in the precipitation reaction tank, and the pH value of the slurry was controlled to be 2.15; the slurry in the precipitation reaction tank continuously flows into the aging treatment tank through the high-position discharge port, and the slurry temperature in the aging treatment tank is controlled to be 75°C for aging treatment; wherein, the feeding molar ratio of ferrous sulfate and diammonium phosphate is controlled to be 0.98:1, and the feeding molar ratio of H2O2 and ferrous sulfate is controlled to be 0.63; the average residence time of the slurry in the precipitation reaction tank is 0.75h, and the aging treatment time in the aging treatment tank is 10h. During the aging treatment process, only low-speed stirring is performed to ensure that the solid content is roughly evenly dispersed in the slurry;
[0031] (2) After the aging treatment in step (1), the slurry is filtered through a plate and frame filter and washed with water at 75° C. until the outlet water conductivity is ≤150 μS / cm. After the filter cake is squeezed, the material is moved into a slurry treatment tank, and magnesium acetate accounting for 2.0 mol% of iron phosphate (added in the form of a 0.30 mol / L aqueous solution) is added, slurried, and a resin aqueous solution is added, stirred, and slurry treatment is performed. The slurry treatment time is 0.5 h. The slurry is prepared according to the solid content concentration of 50 wt% of iron phosphate dihydrate and the solid content concentration of 1.0 wt% of phenolic resin. The resin aqueous solution contains 2.0 wt% of the phenolic resin prepared in Example 1 with a weight average molecular weight of 2600 and 0.25 wt% of hexadecyltrimethylammonium acetate in terms of solid content.
[0032] (3) The slurry after the slurry treatment in step (2) was spray-dried at 250°C to obtain D 50 The spherical powder of 34 μm was dried and calcined in an oxygen-tight furnace at 520°C for 6 h, and crushed to -200 mesh to obtain modified iron phosphate.
[0033] In step (1), the total content of metal ions other than iron in the refined ammonium dihydrogen phosphate aqueous solution is less than 0.0005 mol / L, and the total content of water + components other than ammonium dihydrogen phosphate is less than 0.1 wt%; the total content of metal ions other than iron in the refined ferrous sulfate aqueous solution is less than 0.0005 mol / L. The continuous mixing of the solution and slurry is carried out by a static mixer arranged in the pipeline; the pH value of the slurry in the precipitation reaction tank can be accurately and easily controlled within the range of 2.12-2.18.
[0034] After aging treatment, the mother liquor of the slurry was filtered by the plate and frame filter. After standing for 3 hours, the total phosphorus and total iron in the supernatant were both less than 0.0005 mol / L, indicating that the precipitation rate of phosphorus and iron was very high. After washing with water at 75°C until the conductivity of the effluent was ≤150μS / cm, the effluent was tested with 0.5mol / L barium chloride-1.0mol / L hydrochloric acid solution to find that there was no barium sulfate turbidity, and it was considered that the sulfate had been washed away. The filter cake was squeezed and the output was white, with a dihydrate iron phosphate content of 66wt%, free water of 34wt%, and a sulfate content of less than 0.002wt% on a dry basis, and no iron hydroxide or ferrous hydroxide impurities.
[0035] The modified iron phosphate obtained in step (3) is gray and contains 0.97 wt % carbon.
[0036] Example 3
[0037] The modified ferric phosphate of this embodiment is prepared basically according to the method of Example 2, except that in the slurry for the coating treatment in step (2), the solid content concentration of ferric phosphate dihydrate is 50wt% and the solid content concentration of phenolic resin is 0.5wt%; the concentration ratio of phenolic resin to hexadecyltrimethylammonium acetate in the added resin aqueous solution remains unchanged.
[0038] The modified iron phosphate obtained in step (3) is light gray and contains 0.51 wt% carbon. 50 35μm.
[0039] Comparative Example 1
[0040] The ferric phosphate of this comparative example was prepared basically according to the method of Example 2, except that in step (2), the filter cake after filtration and washing with a plate and frame filter was squeezed and then moved into a slurry treatment tank, and the slurry treatment time was 0.5 h. The ingredients were only prepared according to the solid content concentration of ferric phosphate dihydrate of 50 wt %, and magnesium acetate and the resin aqueous solution were not added. Then, step (3) was spray-dried, and the D of the spherical powder obtained by spray drying was controlled. 50 33μm.
[0041] The iron phosphate obtained in step (3) is white and does not contain carbon.
[0042] Comparative Example 2
[0043] The modified ferric phosphate of this comparative example was prepared basically according to the method of Example 2, except that in step (2), the coating treatment slurry was prepared according to the solid content concentration of ferric phosphate dihydrate of 50wt% and the solid content concentration of phenolic resin of 1.0wt%, and hexadecyltrimethylammonium acetate was not added; in step (3), the D of the spherical powder obtained by spray drying was controlled to be 50 33μm.
[0044] The modified iron phosphate obtained in step (3) is light grey and contains 0.56 wt % carbon.
[0045] Comparative Example 3
[0046] The modified ferric phosphate of this comparative example was prepared basically according to the method of Example 2, except that in step (2), the coating treatment slurry was prepared according to the solid content concentration of ferric phosphate dihydrate of 50wt% and the solid content concentration of hexadecyltrimethylammonium acetate of 0.15wt%, and no phenolic resin was added; in step (3), the D of the spherical powder obtained by spray drying was controlled to be 50 34μm.
[0047] The modified iron phosphate obtained in step (3) is white and contains 0.10 wt% carbon.
[0048] The carbon content of the modified ferric phosphate obtained in Example 2-3 and Comparative Example 2-3 indicates that there is a certain complexation between the phenolic resin and hexadecyltrimethylammonium acetate when the two are used together, so that the carbon content is higher than when they are used alone.
[0049] Example 4
[0050] In a test line capable of producing 25 kg of lithium iron phosphate per day, the modified iron phosphate prepared in the above Examples 2-3 and Comparative Examples 1-3 was used to prepare about 1 kg of lithium iron phosphate respectively according to the following steps: the required amount (the specific amount of sucrose was determined by repeated trial and error according to the carbon content of 2.0 wt% in the obtained lithium iron phosphate) of iron phosphate powder, lithium carbonate powder, sucrose and water were mixed into a slurry, and ground in a sand mill to a fineness of D 50 0.32-0.35μm; after grinding, the slurry was spray dried, and the obtained D 50 The 31-33μm spherical powder was put into a sagger and reduced and sintered in a 720℃ push plate furnace for 8h. The obtained lithium iron phosphate spherical powder (fineness range D 50 23-27μm) was crushed by air flow to obtain D 50 1.1-1.2μm lithium iron phosphate powder with good sphericity (carefully adjust the airflow crushing conditions to make the particle size distribution of each lithium iron phosphate powder basically consistent and comparable).
[0051] In the above preparation process of lithium iron phosphate, samples were taken from the slurry after grinding, and the slurry was tested by transmission electron microscopy (TEM). It was found that the slurry after grinding of the modified iron phosphate obtained by the above Examples 2-3 contained a large number of nanosheets with an outer size of less than 30 nm, part of which adhered to the surface of lithium carbonate grains, part of which still adhered to the surface of anhydrous iron phosphate grains, and part of which was dispersed in the sucrose solution. When the modified iron phosphate obtained by the above Comparative Examples 1-3 was used, the number of nanosheets with an outer size of less than 30 nm was much smaller and the dispersion was much lower; the D obtained by reduction sintering 50The 23-26μm lithium iron phosphate spherical powder was detected by scanning electron microscopy (SEM), and it was found that the carbon distribution uniformity in the spherical particles when the modified iron phosphate obtained in the above Examples 2-3 was higher, the enrichment on the surface of the spherical powder was lower, the carbon film coating and coating uniformity on the surface of the lithium iron phosphate primary grains and between the primary grains was also higher, and basically no carbon-rich shell was formed, which was better than the situation when the iron phosphate obtained in the above Comparative Examples 1-3 was used; the surface of the lithium iron phosphate spherical powder obtained by using the iron phosphate obtained in Comparative Examples 1 and 3 had an obvious carbon-rich shell.
[0052] Comparative Example 4
[0053] The modified ferric phosphate of this comparative example was prepared basically according to the method of Example 2, except that in step (2), when the filter cake was discharged after squeezing and moved into the slurry treatment tank, the magnesium acetate aqueous solution was not added, but the resin aqueous solution was added, and the water was supplemented to a solid content concentration of 50 wt% of ferric phosphate dihydrate and a solid content concentration of 1.0 wt% of phenolic resin for batching; in step (3), the D of the spherical powder obtained by spray drying was controlled to 50 35μm.
[0054] The modified iron phosphate obtained in step (3) is gray and contains 0.98 wt % carbon.
[0055] Comparative Example 5
[0056] The modified ferric phosphate of this comparative example was prepared basically according to the method of Example 2, except that in step (2), when the filter cake was discharged after pressing and moved into the slurry treatment tank, after adding the magnesium acetate aqueous solution, the resin aqueous solution was not added, and the water was supplemented to a solid content concentration of ferric phosphate dihydrate of 50wt% for batching; in step (3), the D of the spherical powder obtained by spray drying was controlled to 50 34μm.
[0057] The modified iron phosphate obtained in step (3) is white and does not contain carbon.
[0058] Comparative Example 6
[0059] The modified iron phosphate prepared in Comparative Example 4 was used as a raw material, and the lithium iron phosphate of this comparative example was prepared substantially according to the method of Example 4, except that magnesium acetate accounting for 2.0 mol % of the iron phosphate was added to the slurry ingredients before grinding in a sand mill for doping.
[0060] Comparative Example 7
[0061] The modified iron phosphate prepared in Comparative Example 5 was used as a raw material, and the lithium iron phosphate of this comparative example was prepared basically according to the method of Example 4, except that the phenolic resin with a weight average molecular weight of 2600 prepared in Example 1 was added to the slurry ingredients before grinding in the sand mill, and the solid content accounted for 1.24wt% of the iron phosphate ratio and 0.15wt% of hexadecyltrimethylammonium acetate (the same ratio as that of iron phosphate, phenolic resin and hexadecyltrimethylammonium acetate in step (2) of Example 2) were added. Through repeated trial and error, the specific amount of sucrose was determined according to the carbon content of 2.0wt% in the obtained lithium iron phosphate.
[0062] The surface of the prepared lithium iron phosphate spherical powder particles has an obvious carbon-rich shell.
[0063] Comparative Example 8
[0064] The lithium iron phosphate of this comparative example was prepared by using the iron phosphate prepared in comparative example 5 as a raw material, basically according to the method of embodiment 4, except that graphene oxide (sheet diameter D 50 0.5μm), and through repeated exploration, the specific feeding amount of sucrose was determined according to the carbon content of 2.0wt% in the obtained lithium iron phosphate.
[0065] The graphene oxide was well dispersed in the slurry after grinding and in the powder obtained by spray drying. The surface of the prepared lithium iron phosphate spherical powder particles was found to have an obvious carbon-rich shell.
[0066] Comparative Example 9
[0067] The modified ferric phosphate of this comparative example was prepared substantially according to the method of Example 2, except that in step (1), the circulating slurry was not used when mixing the raw material solution, but a 1.8 mol / L, 56° C. refined ferrous sulfate aqueous solution of each required flow rate was directly mixed with a 2.0 mol / L, 52° C. aqueous hydrogen peroxide solution, and then mixed with a 2.2 mol / L, 56° C. refined ammonium dihydrogen phosphate aqueous solution, and then injected into the slurry in the precipitation reaction tank. However, the mixing efficiency was ensured by using a small diameter pipeline and a static mixer; and a 5.0 mol / L, 52° C. ammonia water of the required flow rate was injected into the slurry in the precipitation reaction tank, and the pH value of the slurry was controlled to be around 2.15.
[0068] The results include: in step (1), it is much more difficult to control the pH value of the precipitation reaction slurry to about 2.15 than in Example 2, and it is barely controlled within the range of 2.05-2.23; the filter cake obtained in step (2) is light red, and contains 1.8wt% of ferric hydroxide impurity phase on a dry basis, and a small amount of ferrous hydroxide impurity phase can also be detected.
[0069] This comparative example illustrates that in step (1) of Example 2, the circulating slurry is used when mixing the raw material solution, which can ensure that all ferrous ions are oxidized to form trivalent ferrous ions and reduce the decomposition amount of H2O2, and can also more accurately control the pH value range of the slurry, so that the precipitation reaction is complete and the amount of iron hydroxide impurity phase generated is low. The generation and recrystallization of dihydrate ferric phosphate can be ensured through the aging treatment process, and there is no need to add phosphoric acid during the aging treatment process.
[0070] Test Example 1
[0071] The lithium iron phosphate prepared in Example 4 from the iron phosphate obtained in Examples 2-3 and Comparative Examples 1-3, and the lithium iron phosphate prepared in Comparative Examples 5-8 were sampled as anode materials to prepare 10 R2025 button batteries. The manufacturing process of the R2025 button battery includes: mixing the lithium iron phosphate with the PVDF binder at a mass ratio of 100:2.5, adding an appropriate amount of NMP to mix, and the obtained mixed slurry is evenly coated on the carbon-coated aluminum foil with a 250μm slit die, first coating one side, drying and then coating the other side, and rolling at a pressure of 10MPa after drying to obtain a rolled positive electrode sheet, using a metal lithium sheet as the negative electrode, using a Celgard2300 microporous membrane as a diaphragm, and 1.0mol / LLiPF6 ethylene carbonate (EC): dimethyl carbonate (DMC) = 1:3 (volume ratio) solution as an electrolyte, and assembling the R2025 button battery in a glove box.
[0072] The compaction density of the lithium iron phosphate in each rolled positive electrode sheet was measured, wherein the compaction density of the lithium iron phosphate prepared by the iron phosphate obtained in Examples 2-3 in Example 6 was 2.38 g / cm 3 and 2.41 g / cm 3 .
[0073] The electrochemical performance test of the above R2025 button battery was carried out, wherein the charge and discharge cut-off voltage was 2.5-3.8V and the constant temperature was 25°C; the batteries of Examples 2-3 and Comparative Example 8 were subjected to 5 charge and discharge cycles at a charge and discharge rate of 0.2C, and then 300 charge and discharge cycles at a charge and discharge rate of 3C, and finally 300 charge and discharge cycles at a charge and discharge rate of 6C. The batteries of the other comparative examples were first subjected to 5 charge and discharge cycles at a charge and discharge rate of 0.2C, and then 100 charge and discharge cycles at a charge and discharge rate of 3C. The main test results are listed in Table 1.
[0074] Table 1: Half-cell test results of lithium iron phosphate prepared from modified iron phosphate of Examples 2-3, Comparative Examples 1-3, and lithium iron phosphate of Comparative Examples 6-8, unit: mAh / g
[0075]
Claims
1. A method for preparing a modified iron phosphate for a high-rate lithium iron phosphate anode material, comprising the following steps: (1) The slurry in the precipitation reaction tank is continuously stirred and the slurry temperature is controlled at 50-60°C; the circulating slurry in one path of the precipitation reaction tank is mixed with a 1.0-2.0 mol / L, 50-60°C refined ferrous sulfate aqueous solution, respectively, at a volume flow ratio of 5-10:1, and then continuously mixed with a 50-60°C hydrogen peroxide aqueous solution at a required flow rate, and then continuously mixed with a 1.5-2.5 mol / L, 50-60°C refined ammonium dihydrogen phosphate aqueous solution at a required flow rate, and then injected into the slurry in the precipitation reaction tank; the other circulating slurry in the precipitation reaction tank is mixed with a 4.0-8.0 mol / L, 50-60°C ammonia water at a volume flow ratio of 10-20:1, and then injected into the slurry in the precipitation reaction tank, and the pH value of the slurry is controlled to be in the range of 2.0-2.3; the slurry in the precipitation reaction tank continuously flows into the aging treatment tank through the high-position discharge port, and the slurry temperature in the aging treatment tank is controlled to be 70-80°C for aging treatment; in, The molar ratio of ferrous sulfate to ammonium dihydrogen phosphate is controlled to be 0.96-0.98:1, and the molar ratio of H2O2 to ferrous sulfate is controlled to be 0.60-0.65; the average residence time of the slurry in the precipitation reaction tank is 0.5-1h, and the aging treatment time in the aging treatment tank is 8-12h; (2) After the aging treatment in step (1), the slurry is filtered through a belt filter or a plate and frame filter, and washed with water at 70-80° C. until the effluent conductivity is ≤150 μS / cm. The filter cake is transferred into a slurry treatment tank, and magnesium acetate or its aqueous solution accounting for 1.5-2.5 mol% of iron phosphate is added, stirred evenly, and a resin aqueous solution is added for slurrying, and a slurry treatment is performed, and the slurry treatment time is 0.5-1 h. The slurry for slurry treatment is prepared according to the solid content concentration of iron phosphate dihydrate of 45-50 wt% and the solid content concentration of phenolic resin of 0.5-1.0 wt%; the resin aqueous solution contains phenolic resin with a weight average molecular weight of 2000-3000 and hexadecyltrimethylammonium acetate, wherein the weight percentage concentration ratio of the phenolic resin to the hexadecyltrimethylammonium acetate based on the solid content is 1:0.1-0.15; (3) The slurry after the slurry treatment in step (2) is spray-dried at 200-250° C., and the dried material is roasted in an oxygen-proof furnace at 500-550° C. for 4-8 hours and crushed to obtain modified iron phosphate.
2. The method for preparing the modified iron phosphate for high-rate lithium iron phosphate anode material according to claim 1, It is characterized in that The phenolic resin is prepared by the following steps: using a stirred reactor with condensation reflux and vacuum distillation; after sealing and replacing air, adding water and a formaldehyde aqueous solution with a concentration of 37-40wt% and phenol under continuous stirring, sealing the reactor, heating to 60-70°C, then dripping ammonia water for reaction for 20-30min, heating to 70-75°C for reaction for 20-30min, heating to 85-90°C and maintaining the temperature for reaction for 2-3h, then performing vacuum distillation for 2-4h until the solid concentration in the feed liquid reaches 35-40wt%, cooling to room temperature, and obtaining the phenolic resin; wherein the ingredients are water, formaldehyde aqueous solution, phenol, and ammonia in a weight ratio of 0.5-1.0:1.3-1.6:1:0.03-0.05; the vacuum distillation conditions include: a reaction feed liquid temperature of 70-80°C, an exhaust vacuum absolute pressure of 30-45kPa, and a condensation temperature of 10-5°C.
3. The method for preparing the modified iron phosphate for high-rate lithium iron phosphate anode material according to claim 1, It is characterized in that The continuous mixing of the solution and slurry in step (1) is carried out by a static mixer arranged in the pipeline.
4. The method for preparing the modified iron phosphate for high-rate lithium iron phosphate anode material according to claim 1, It is characterized in that In step (1), the molar ratio of ferrous sulfate to ammonium dihydrogen phosphate is controlled to be 0.98:
1. In step (2), magnesium acetate or its aqueous solution accounting for 2.0 mol% of iron phosphate is added.
5. The method for preparing the modified iron phosphate for high-rate lithium iron phosphate anode material according to claim 4, It is characterized in that The coating treatment slurry in step (2) is prepared according to the following ingredients: 50 wt% of ferric phosphate dihydrate solid content, 1.0 wt% of phenolic resin solid content, and 0.125 wt% of hexadecyltrimethylammonium acetate.
Citation Information
Patent Citations
Battery-grade iron phosphate and preparation method thereof
CN106185857A
A high magnification spherical lithium iron phosphate carbon composite positive electrode material and a preparation method thereof
CN109192953A
Titanium and zirconium co-doped carbon-coated lithium iron phosphate material as well as preparation method and application thereof
CN114314548A
Preparation method of lithium iron phosphate oxide of cathode material of lithium ion battery
CN101638227A
Method for preparing lithium iron phosphate / carbon composite material
CN108183234A