Glass fiber preparation device and method, and quartz image transmission optical fiber preparation method
By designing glass wire preparation equipment, using wire drawing furnaces, diameter measuring instruments and wire drawing wheels, the problem that ordinary communication fiber optic equipment cannot draw thick-diameter glass wires is solved, and the preparation of multi-core quartz image-transfer fiber and its prefabricated rods is realized, improving the The operationality and stability of the preparation reduce the cost and break the monopoly of foreign suppliers.
Patent Information
- Application Number
- CN202211666925.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-22
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2042-12-22
AI Technical Summary
Existing ordinary communication fiber equipment cannot draw thick-diameter glass wire, which cannot meet the preparation requirements of multi-core quartz image transmission fiber and its prefabricated rods. Moreover, quartz image transmission fiber relies on foreign suppliers, resulting in high costs and unstable supply.
A glass wire preparation equipment is designed, including a wire drawing furnace, a diameter meter, a cooling tank and a wire drawing wheel. The glass wire is pulled out by heating the prefabricated rod, and the diameter and speed are adjusted through the diameter meter measurement and wire drawing wheel to achieve a single core or The preparation of multi-core glass wire is suitable for finished glass wires with an outer diameter of 1-3mm.
The unwinding and pulling of thick-diameter single-core and multi-core glass wire is realized, which meets the preparation requirements of multi-core quartz image-transport fiber and its preformed rod, improves the operationality and process stability of the preparation, reduces the cost, and Break the dependence on foreign suppliers.
Smart Images

Figure CN115959824B_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of optical fiber manufacturing, and more specifically, relates to a glass fiber preparation device and method, and a quartz image transmission optical fiber preparation method. Background Art
[0002] Image transmission fiber is a flexible multi-core optical fiber for transmitting images. It is mainly used for image transmission in endoscopes and is an important core optical component of various fiber endoscopes. Image transmission fiber has the advantages of small size, light weight, large degree of freedom in use, easy to realize image transmission of complex spatial structures, passive real-time image transmission, high temperature resistance, electromagnetic radiation resistance, and nuclear radiation resistance. It is widely used in medical, industrial, scientific research, aerospace and other fields.
[0003] Traditional image transmission fiber is a bundle-type optical fiber image transmission bundle made of multi-component glass. It is a bundle of tens of thousands of 10-20μm multi-component glass optical fibers arranged at both ends, glued and positioned, and scattered in the middle. Its disadvantages include the existence of glued boundaries, difficulty in production, complex process, high cost, and large absorption loss. Multi-core quartz image transmission fiber is a single multi-core quartz image transmission fiber that neatly arranges thousands of quartz optical fibers in a quartz sleeve and integrates them into one. It has the advantages of high resolution, long manufacturable length and low cost. Compared with multi-component glass optical fiber image transmission bundles, quartz image transmission fiber has the following advantages: 1) It can achieve ultra-fine diameter and is more suitable for medical endoscope applications; 2) Excellent optical transmission performance and higher image quality; 3) Higher resolution; 4) It can achieve long-distance optical transmission; 5) High chemical stability and high mechanical durability; 6) It has a wider application prospect in the fields of medicine and industry.
[0004] The existing preparation process of ordinary communication optical fiber is to prepare a single-core preform rod first, and then draw the single-core preform rod into a quartz glass optical fiber with an outer diameter of 125μm, and then wind it up through an automatic wire reel after coating and curing. The drawing speed is generally above 30m / s. The outer diameter of the optical fiber applicable to ordinary communication optical fiber drawing equipment is within 200μm. The diameters of the single-core glass filaments and multi-core glass filaments used in the preparation process of quartz image transmission optical fiber are large, and they cannot be bent and wound, and the drawing of single-core glass filaments and multi-core glass filaments requires manual cutting for wire collection, so the drawing speed cannot be too fast, generally 1-3m / s. Due to the great differences in the structure, geometric dimensions and preparation process of quartz image transmission optical fiber compared with ordinary communication optical fiber, the existing ordinary communication optical fiber preparation equipment cannot meet the use requirements of drawing single-core glass filaments and multi-core glass filaments in the preparation process of quartz image transmission optical fiber. In addition, the image transmission optical fiber currently relies on foreign suppliers for import, which is expensive and subject to others. Therefore, independent innovation and research and development of image transmission optical fiber is conducive to breaking the monopoly of foreign image transmission optical fiber suppliers and reducing domestic procurement costs. In summary, this field urgently needs to design a set of new manufacturing equipment and preparation methods to achieve the preparation of thick-diameter glass fibers and quartz image transmission optical fibers. Summary of the invention
[0005] The present invention solves the problem that existing common communication optical fiber drawing equipment cannot draw thick-diameter glass fibers and cannot meet the requirements for preparing multi-core quartz image transmission optical fibers and preforms thereof by providing a glass fiber preparation device and method and a quartz image transmission optical fiber preparation method.
[0006] In a first aspect, the present invention provides a glass fiber preparation device, comprising: a drawing furnace, a diameter gauge, a cooling tank and a drawing wheel arranged in sequence from top to bottom;
[0007] The wire drawing furnace is used to heat the preform rod to draw out glass filaments; the preform rod is a single-core preform rod or a multi-core preform rod, and the glass filaments are single-core glass filaments or multi-core glass filaments;
[0008] The caliper is used to measure the diameter of the glass filament;
[0009] The cooling tank is used to cool the glass filaments;
[0010] The drawing wheel is used to control the drawing speed and diameter of the glass filaments to obtain finished glass filaments; the finished glass filaments are single-core finished glass filaments or multi-core finished glass filaments, and the outer diameter of the finished glass filaments is 1-3 mm.
[0011] Preferably, the measuring range of the caliper is 0.5-5 mm.
[0012] Preferably, the cooling groove is arranged on one side of the wire drawing channel, and a plurality of air holes facing the glass filaments are arranged in the cooling groove, the air holes are connected with the cooling gas pipeline, and the cooling gas is blown vertically toward the glass filaments through the air holes.
[0013] Preferably, the cooling gas is compressed air or nitrogen, and the temperature of the cooling gas is room temperature or lower than room temperature; the flow rate of the cooling gas is adjusted by a valve on the cooling gas pipeline.
[0014] Preferably, the drawing wheel is two pairs of rollers, which are respectively located on both sides of the drawing channel, and the two pairs of rollers are closed towards each other to clamp the glass filaments; the outer periphery of the drawing wheel is wrapped with a high-temperature resistant and elastic rubber material, and the temperature resistance of the rubber material is not lower than 250°C.
[0015] Preferably, the drawing wheel includes a driving wheel and a driven wheel, and the driving wheel is connected to a motor; the motor drives the drawing wheel rollers to rotate, so that the glass filaments are automatically pulled downward; the drawing speed and diameter of the glass filaments are controlled by adjusting the rotation speed of the rollers, and the drawing speed is 1 to 3 m / s.
[0016] Preferably, the glass filament preparation equipment also includes: a first guide assembly arranged between the diameter gauge and the cooling trough, and a second guide assembly arranged between the cooling trough and the drawing wheel; the first guide assembly includes a first guide wheel and a second guide wheel respectively arranged on both sides of the drawing channel, and the second guide assembly includes a third guide wheel and a fourth guide wheel respectively arranged on both sides of the drawing channel; the tolerance temperature of the first guide wheel, the second guide wheel, the third guide wheel and the fourth guide wheel are not lower than 1300°C; the first guide assembly is used to ensure that the glass filaments are pulled downward along the drawing channel, and the second guide assembly is used to ensure that the cooled glass filaments are pulled downward along the drawing channel.
[0017] In a second aspect, the present invention provides a method for preparing glass filaments, which is implemented by using the above-mentioned glass filament preparation device. The method for preparing glass filaments comprises the following steps:
[0018] The preform rod is placed in a wire drawing furnace for heating, and the conical portion of the preform rod is melted and then a glass wire is drawn out;
[0019] The diameter of the glass fibers is measured by a caliper;
[0020] The glass fibers are cooled by a cooling tank;
[0021] The drawing speed and diameter of the glass filaments are adjusted by a drawing wheel, and the length of the drawn glass filaments is shortened as required to obtain finished glass filaments;
[0022] Wherein, when the preform rod is a single-core preform rod, the glass filaments drawn out after the cone portion of the preform rod is melted are single-core glass filaments, and the finished glass filaments are single-core glass filaments finished products; the outer diameter of the single-core preform rod is 10 to 50 mm, and the outer diameter of the finished single-core glass filaments is 1 to 3 mm;
[0023] When the preform rod is a multi-core preform rod, the glass fibers pulled out after the cone portion of the preform rod is melted are multi-core glass fibers, and the finished glass fibers are multi-core glass fibers; the outer diameter of the multi-core preform rod is 10 to 50 mm, the outer diameter of the multi-core glass fibers is 1 to 3 mm, and the number of cores of the multi-core glass fibers is 100 to 300.
[0024] In a third aspect, the present invention provides a method for preparing a quartz image transmission optical fiber, comprising the following steps:
[0025] A single-core preform rod is used as a preform rod for preparation, and a single-core glass fiber finished product is prepared by the above-mentioned glass fiber preparation method;
[0026] After cleaning and drying, a plurality of the single-core glass filament finished products are stacked and filled into a quartz glass tube to obtain a multi-core preform rod; using the multi-core preform rod as a preform rod for preparation, and using the above-mentioned glass filament preparation method to prepare a multi-core glass filament finished product;
[0027] cleaning and drying a plurality of the multi-core glass filament products, and then piling and filling them into another quartz glass tube to obtain a composite multi-core preform;
[0028] The composite multi-core preform rod is placed on a common communication optical fiber drawing tower to be drawn into a fiber, and the quartz image transmission optical fiber prepared after coating and curing is bent and wound on a fiber receiving drum.
[0029] Preferably, the outer diameter of the quartz image transmission optical fiber is 300-1000 μm, and the number of pixels of the quartz image transmission optical fiber is 10000-90000.
[0030] One or more technical solutions provided in the present invention have at least the following technical effects or advantages:
[0031] The present invention firstly uses a wire drawing furnace to heat a preform rod to draw out glass filaments, the preform rod is a single-core or multi-core preform rod, and the glass filaments are single-core or multi-core glass filaments; then a diameter gauge is used to measure the diameter of the glass filaments, a cooling tank is used to cool the glass filaments, and finally a drawing wheel is used to control the drawing speed and diameter of the glass filaments to obtain a finished glass filament with an outer diameter of 1-3 mm. The equipment and preparation method provided by the present invention have strong operability and stable process, and can draw single-core glass filaments and multi-core glass filaments with an outer diameter of 1-3 mm, realize the non-winding drawing of thick-diameter glass filaments, can solve the problem that the preparation of quartz image transmission optical fiber and its preform rods is not compatible with the existing ordinary communication optical fiber drawing equipment, and can realize and meet the preparation requirements of multi-core quartz image transmission optical fiber and its preform rods. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 A schematic structural diagram of a glass fiber preparation device provided in Example 1 of the present invention;
[0033] Figure 2 A microscopic image of the end face of a quartz image transmitting optical fiber prepared by a method for preparing a quartz image transmitting optical fiber provided in Example 3 of the present invention;
[0034] Figure 3 A local microscopic image of the end face of a quartz image transmitting optical fiber prepared by the method for preparing a quartz image transmitting optical fiber provided in Example 3 of the present invention. DETAILED DESCRIPTION
[0035] The preparation process of the quartz image transmission optical fiber includes sequentially preparing a single-core glass fiber with an outer diameter of 1-3 mm, filling the drawn single-core glass fiber into a glass tube to form a multi-core preform rod (primary multifilament), drawing the multi-core preform rod into a multi-core glass fiber with an outer diameter of 1-3 mm, and then filling the multi-core glass fiber into a glass tube to form a composite multi-core preform rod (secondary multifilament), and finally drawing the composite multi-core preform rod into an image transmission optical fiber with an outer diameter of 300-1000 μm. In order to realize the preparation of the quartz image transmission optical fiber, the present invention first provides a glass fiber preparation device to realize the preparation of single-core glass fibers and multi-core glass fibers with thick diameters, and then realizes the preparation of composite multi-core image transmission optical fiber preform rods and multi-core quartz image transmission optical fibers on the basis of the above.
[0036] In order to better understand the above technical solution, the above technical solution will be described in detail below in conjunction with the accompanying drawings and specific implementation methods.
[0037] Embodiment 1:
[0038] Embodiment 1 provides a glass fiber preparation device, see Figure 1 , including a wire drawing furnace 1, a diameter gauge 3, a first guide assembly, a cooling trough 6, a second guide assembly and a wire drawing wheel 9 which are arranged in sequence from top to bottom.
[0039] The wire drawing furnace 1 is used to heat the preform rod 2 to draw out the glass filament 10. The preform rod 2 is a single-core preform rod or a multi-core preform rod, and correspondingly, the glass filament 10 is a single-core glass filament or a multi-core glass filament.
[0040] The diameter gauge 3 is used to measure the diameter of the glass filament 10 .
[0041] The first guide assembly is used to ensure that the glass filament 10 is pulled downward along the drawing channel.
[0042] The cooling tank 6 is used to cool the glass filaments 10 .
[0043] The second guide assembly is used to ensure that the cooled glass filaments 10 are pulled downward along the drawing channel.
[0044] The spinning wheel 9 is used to control the drawing speed and diameter of the glass filament 10 to obtain a finished glass filament, wherein the finished glass filament is a single-core glass filament or a multi-core glass filament, and the outer diameter of the finished glass filament is 1-3 mm.
[0045] Specifically, the measuring range of the caliper 3 is 0.5-5 mm.
[0046] The first guide assembly includes a first guide wheel 4 and a second guide wheel 5 respectively arranged on both sides of the wire drawing channel. The first guide wheel 4 and the second guide wheel 5 are both made of high temperature resistant materials, and the withstanding temperature is not less than 1300°C.
[0047] The cooling tank 6 is arranged at one side of the drawing channel, and a plurality of air holes facing the glass filaments 10 are arranged in the cooling tank 6, and the air holes are connected to the cooling gas pipeline, and the cooling gas is blown vertically to the glass filaments 10 through the air holes to cool down the glass filaments 10. The cooling gas is compressed air or nitrogen, and the temperature of the cooling gas is room temperature or lower than room temperature after pre-cooling; the flow rate of the cooling gas can be adjusted by the valve on the cooling gas pipeline as needed.
[0048] The second guide assembly includes a third guide wheel 7 and a fourth guide wheel 8 respectively arranged on both sides of the wire drawing channel. The third guide wheel 7 and the fourth guide wheel 8 are both made of high temperature resistant materials, and the withstanding temperature is not less than 1300°C.
[0049] The drawing wheel 9 is composed of two pairs of rollers, which are respectively located on both sides of the drawing channel, and the two pairs of rollers are closed towards each other to clamp the glass filament 10; the outer periphery of the drawing wheel 9 is wrapped with a high temperature resistant and elastic rubber material, and the temperature resistance of the rubber material is not less than 250°C, and the temperature resistance in the preferred embodiment is not less than 300°C. The opening and closing and rotation speed of the drawing wheel 9 can be adjusted as needed. Specifically, the drawing wheel 9 includes a driving wheel and a driven wheel, and the driving wheel is connected to a motor; the motor drives the drawing wheel 9 to rotate the rollers, so that the glass filament 10 is automatically pulled downward; the drawing speed and diameter of the glass filament 10 are controlled by adjusting the rotation speed of the rollers, and the drawing speed is 1 to 3 m / s.
[0050] Embodiment 2:
[0051] Embodiment 2 provides a method for preparing glass filaments, which is implemented by using the glass filament preparation device as described in Embodiment 1. The method for preparing glass filaments comprises the following steps:
[0052] The preform rod is placed in a wire drawing furnace for heating, and the conical portion of the preform rod is melted and then a glass wire is drawn out;
[0053] The diameter of the glass fibers is measured by a caliper;
[0054] The drawing direction of the glass filaments is limited by the first guide assembly to ensure that the glass filaments are drawn downward along the drawing channel;
[0055] The glass fibers are cooled by a cooling tank;
[0056] The second guide assembly is used to limit the pulling direction of the cooled glass filaments, so as to ensure that the cooled glass filaments are pulled downward along the drawing channel;
[0057] The drawing speed and diameter of the glass filaments are adjusted by a drawing wheel, and the length of the drawn glass filaments is shortened as required to obtain finished glass filaments.
[0058] Among them, when the preform rod is a single-core preform rod, the glass fiber pulled out after the cone portion of the preform rod is melted is a single-core glass fiber, and the finished glass fiber product is a single-core glass fiber finished product; the outer diameter of the single-core preform rod is 10 to 50 mm, and the outer diameter of the single-core glass fiber finished product is 1-3 mm.
[0059] When the preform rod is a multi-core preform rod, the glass fibers pulled out after the cone portion of the preform rod is melted are multi-core glass fibers, and the finished glass fibers are multi-core glass fibers; the outer diameter of the multi-core preform rod is 10 to 50 mm, the outer diameter of the multi-core glass fibers is 1 to 3 mm, and the number of cores of the multi-core glass fibers is 100 to 300.
[0060] The glass fiber preparation method provided in Example 2 corresponds to the function of the glass fiber preparation equipment provided in Example 1, and thus will not be described in detail.
[0061] Embodiment 3:
[0062] Embodiment 3 provides a method for preparing a quartz image transmission optical fiber, comprising the following steps:
[0063] A single-core preform rod is used as the preform rod for preparation, and a single-core glass fiber finished product is prepared by the glass fiber preparation method described in Example 2;
[0064] After cleaning and drying, a plurality of the single-core glass filament finished products are stacked and filled into a quartz glass tube to obtain a multi-core preform rod; using the multi-core preform rod as a preform rod for preparation, and using the glass filament preparation method described in Example 2 to prepare a multi-core glass filament finished product;
[0065] cleaning and drying a plurality of the multi-core glass filament products, and then piling and filling them into another quartz glass tube to obtain a composite multi-core preform;
[0066] The composite multi-core preform rod is placed on a common communication optical fiber drawing tower to be drawn into a fiber, and the quartz image transmission optical fiber prepared after coating and curing is bent and wound on a fiber receiving drum.
[0067] The preparation of each stage is further described below.
[0068] (1) Preparation of single-core glass fiber.
[0069] A designed and prepared single-core core rod (i.e., single-core preform rod) with a diameter of 10 to 50 mm is placed in a wire drawing furnace for heating. After the cone of the core rod is melted at high temperature, a glass filament is pulled out from under the wire drawing furnace. The diameter of the glass filament is measured by a diameter gauge. The glass filament passes through the first guide wheel and the second guide wheel in sequence. Since the first guide wheel and the second guide wheel are located on both sides of the glass filament, the glass filament can be prevented from deviating from the wire drawing channel. The first guide wheel and the second guide wheel are made of high-temperature resistant materials. The glass filament continues to be pulled downward and then passes through a cooling trough for cooling. The cooling trough is vertically placed on one side of the glass filament. A row of air holes facing the glass filament is designed in the cooling trough. The air holes are connected to a compressed air pipeline. Compressed air passes through the air holes of the cooling trough and blows vertically toward the glass filament to cool the glass filament. The flow rate of the compressed air can be adjusted as needed by a valve. After cooling, the glass filament continues to pass through the third guide wheel and the fourth guide wheel downward. The third guide wheel and the fourth guide wheel are located on both sides of the glass filament, so as to prevent the glass filament from deviating from the drawing channel due to the blowing of compressed air. The third guide wheel and the fourth guide wheel are made of high temperature resistant materials. After cooling, the glass filament continues to be pulled downward through the drawing wheel; the drawing wheel is two pairs of rollers, which are located on both sides of the glass filament respectively. The drawing wheel on one side is the active wheel driven by a motor, and the drawing wheel on the other side is the driven wheel. The opening and closing and rotation speed of the drawing wheel can be adjusted as needed. The outer periphery of the drawing wheel is wrapped with high temperature resistant rubber material, which is both high temperature resistant and elastic. The two pairs of rollers are closed towards each other to clamp the glass filament. The driving motor of the drawing wheel is turned on to rotate the rollers, and the glass filament is automatically pulled downward. The drawing speed and diameter of the glass filament can be controlled by adjusting the rotation speed of the drawing wheel. The drawn glass filament is shortened to the required length to finally obtain a single-core glass filament finished product with an outer diameter of 1-3mm.
[0070] (2) Preparation of multi-core glass fibers.
[0071] The finished single-core glass filaments drawn are cleaned, dried, and then piled and filled into a quartz glass tube until the inner hole of the quartz glass tube is filled (100-300 filaments). The outer diameter of the quartz glass tube is 10-50 mm. The quartz glass tube filled with single-core glass filaments is then placed in a drawing furnace in the glass filament preparation device provided by the present invention for heating. After the cone of the quartz glass tube is melted at high temperature, multi-core glass filaments are pulled out from under the drawing furnace. The diameter of the multi-core glass filaments is measured by a diameter gauge. The multi-core glass filaments pass through a first guide wheel and a second guide wheel in sequence. Since the first guide wheel and the second guide wheel are located on both sides of the multi-core glass filaments, the multi-core glass filaments can be prevented from deviating from the drawing channel, and the multi-core glass filaments continue to be pulled downward. Compressed air passes through a cooling groove. The air holes of the multi-core glass filaments are blown vertically to the multi-core glass filaments to cool the multi-core glass filaments. After cooling, the multi-core glass filaments continue to pass through the third guide wheel and the fourth guide wheel downward; since the third guide wheel and the fourth guide wheel are located on both sides of the multi-core glass filaments, the multi-core glass filaments can be prevented from deviating from the drawing channel due to the blowing of compressed air, and the multi-core glass filaments after cooling continue to be pulled downward through the drawing wheel; the drawing wheels are closed towards each other to clamp the multi-core glass filaments, and the drawing wheel rollers rotate to automatically draw the multi-core glass filaments downward, and the drawing speed and diameter of the multi-core glass filaments can be controlled by adjusting the rotation speed of the drawing wheel; the drawn multi-core glass filaments are shortened according to the required length, and finally a multi-core glass filament finished product with an outer diameter of 1-3mm and 100-300 cores is obtained.
[0072] (3) Preparation of composite multi-core preform rods.
[0073] The multi-core glass fiber products drawn above are cleaned, dried, and then piled up and filled into a quartz glass tube until the inner hole of the quartz glass tube is filled (100-300 strands) to obtain a composite multi-core preform rod (i.e., a composite multi-core image transmission optical fiber preform rod), wherein the number of cores of the composite multi-core preform rod is 10,000-90,000 cores.
[0074] (4) Preparation of quartz image transmitting optical fiber.
[0075] Finally, the composite multi-core preform prepared above is placed on a drawing tower of a common communication optical fiber drawing equipment (for example, a drawing tower for drawing common G.652 communication optical fiber) to draw into a fiber. The outer diameter of the obtained quartz image transmission optical fiber is 300-1000μm, and the number of pixels is 10000-90000. After coating and curing, the multi-core quartz image transmission optical fiber is bent and wound on the wire collection drum of the common communication optical fiber drawing equipment. The end face micrograph of the prepared quartz image transmission optical fiber is shown in FIG. Figure 2 , Figure 3 shown.
[0076] In summary, the present invention can draw single-core glass fibers and multi-core glass fibers with an outer diameter of 1-3 mm, realize the non-winding drawing of thick-diameter glass fibers, and thus meet the preparation requirements of multi-core quartz image transmission optical fibers and preforms thereof, with strong operability and stable process. In addition, the preparation process of the present invention does not have a melting and shrinking link, the process is simpler, and costs can be saved.
[0077] Finally, it should be noted that the above specific implementation methods are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A glass fiber preparation device, It is characterized in that include: The wire drawing furnace, diameter gauge, cooling tank and wire drawing wheel are arranged in sequence from top to bottom; The wire drawing furnace is used to heat the preform rod to draw out glass wire; The preform rod is a single-core preform rod or a multi-core preform rod, and the glass yarn is a single-core glass yarn or a multi-core glass yarn; The caliper is used to measure the diameter of the glass filament; The cooling tank is used to cool the glass filaments; The drawing wheel is used to control the drawing speed and diameter of the glass filament to obtain a finished glass filament and realize the non-winding drawing of thick-diameter glass filament; the drawing speed is 1 to 3 m / s; the finished glass filament is a single-core glass filament finished product or a multi-core glass filament finished product, and the outer diameter of the finished glass filament is 1-3 mm.
2. The glass fiber preparation device according to claim 1, It is characterized in that The measuring range of the caliper is 0.5-5 mm.
3. The glass fiber preparation device according to claim 1, It is characterized in that The cooling groove is arranged at one side of the wire drawing channel, and a plurality of air holes facing the glass filaments are arranged in the cooling groove. The air holes are connected with the cooling gas pipeline, and the cooling gas is blown vertically toward the glass filaments through the air holes.
4. The glass fiber preparation device according to claim 3, It is characterized in that The cooling gas is compressed air or nitrogen, and the temperature of the cooling gas is room temperature or lower than room temperature; the flow rate of the cooling gas is adjusted by a valve on the cooling gas pipeline.
5. The glass fiber production equipment according to claim 1, It is characterized in that The drawing wheel is composed of two pairs of rollers, which are respectively located on both sides of the drawing channel and closed towards each other to clamp the glass filaments. The outer periphery of the drawing wheel is wrapped with a high-temperature resistant and elastic rubber material, and the temperature resistance of the rubber material is not lower than 250°C.
6. The glass fiber preparation device according to claim 5, It is characterized in that The drawing wheel includes a driving wheel and a driven wheel, and the driving wheel is connected to a motor; the motor drives the drawing wheel roller to rotate, so that the glass filament is automatically pulled downward; the drawing speed and diameter of the glass filament are controlled by adjusting the rotation speed of the roller.
7. The glass fiber production equipment according to claim 1, It is characterized in that Also includes: A first guide assembly is arranged between the diameter gauge and the cooling trough, and a second guide assembly is arranged between the cooling trough and the drawing wheel; the first guide assembly includes a first guide wheel and a second guide wheel respectively arranged on both sides of the drawing channel, and the second guide assembly includes a third guide wheel and a fourth guide wheel respectively arranged on both sides of the drawing channel; the first guide wheel, the second guide wheel, the third guide wheel and the fourth guide wheel have a tolerance temperature of not less than 1300°C; the first guide assembly is used to ensure that the glass filaments are pulled downward along the drawing channel, and the second guide assembly is used to ensure that the cooled glass filaments are pulled downward along the drawing channel.
8. A method for preparing glass fibers, It is characterized in that The glass filament preparation method is implemented by using the glass filament preparation device according to any one of claims 1 to 7, and the glass filament preparation method comprises the following steps: The preform rod is placed in a wire drawing furnace for heating, and the conical portion of the preform rod is melted and then a glass wire is drawn out; The diameter of the glass fibers is measured by a caliper; The glass fibers are cooled by a cooling tank; The drawing speed and diameter of the glass filaments are adjusted by a drawing wheel, and the length of the drawn glass filaments is shortened as required to obtain finished glass filaments; Wherein, when the preform rod is a single-core preform rod, the glass filaments drawn out after the cone portion of the preform rod is melted are single-core glass filaments, and the finished glass filaments are single-core glass filaments finished products; the outer diameter of the single-core preform rod is 10 to 50 mm, and the outer diameter of the finished single-core glass filaments is 1 to 3 mm; When the preform rod is a multi-core preform rod, the glass fibers pulled out after the cone portion of the preform rod is melted are multi-core glass fibers, and the finished glass fibers are multi-core glass fibers. The outer diameter of the multi-core preform rod is 10 to 50 mm, the outer diameter of the multi-core glass fibers is 1 to 3 mm, and the number of cores of the multi-core glass fibers is 100 to 300.
9. A method for preparing a quartz image transmission optical fiber, It is characterized in that The following steps are involved: A single-core preform rod is used as the preform rod for preparation, and a single-core glass fiber finished product is prepared by the glass fiber preparation method as claimed in claim 8; After cleaning and drying, a plurality of the single-core glass filament finished products are stacked and filled into a quartz glass tube to obtain a multi-core preform rod; using the multi-core preform rod as a preform rod for preparation, and using the glass filament preparation method as claimed in claim 8 to prepare a multi-core glass filament finished product; cleaning and drying a plurality of the multi-core glass filament products, and then piling and filling them into another quartz glass tube to obtain a composite multi-core preform; The composite multi-core preform rod is placed on a common communication optical fiber drawing tower to be drawn into a fiber, and the quartz image transmission optical fiber prepared after coating and curing is bent and wound on a fiber receiving drum.
10. The method for preparing the quartz image transmission optical fiber according to claim 9, It is characterized in that The outer diameter of the quartz image transmission optical fiber is 300-1000 μm, and the number of pixels of the quartz image transmission optical fiber is 10000-90000.