Coating liquid for forming pressure measuring layer, method for producing pressure measuring layer, and article having non-planar portion and having pressure measuring layer

By using a pressure measurement layer coating liquid containing microcapsules of a chromogenic agent and an aromatic solvent, the problem of insufficient color distribution of pressure-sensitive chromogenic resin materials under low pressure and difficulty in measuring non-planar surfaces has been solved, achieving a temperature below 300MPa. Excellent color distribution and gradient, suitable for pressure measurement on complex surfaces.

CN115968390BActive Publication Date: 2024-10-18FUJIFILM CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202180052346.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-08-16
Publication Date
2024-10-18
Estimated Expiration
2041-08-16

AI Technical Summary

Technical Problem

It is difficult to measure the pressure of non-planar surfaces in the low pressure range with the existing technology. Especially at pressures below 300MPa, the color distribution of pressure-sensitive chromogenic resin materials is insufficient, and it is difficult to apply to complex surfaces such as curved surfaces and uneven surfaces. Pressure measurement.

Method used

A coating liquid for forming a pressure measuring layer using microcapsules containing a color-developing agent and an aromatic solvent, the average particle size of the microcapsules being 5 μm or more, the resin content being 17% or less relative to the total solid content, and the color-developing agent being activated clay. , acid clay and zinc salicylate derivatives, through specific coating amount and viscosity design, form a pressure measurement layer that can show good gradient properties under low pressure.

Benefits of technology

It achieves excellent color distribution and gradient under pressures below 300MPa, is suitable for pressure measurement on non-planar surfaces, and solves the problem in the prior art that the pressure measurement layer does not work well under low pressure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115968390B_ABST
    Figure CN115968390B_ABST
Patent Text Reader

Abstract

The first problem of the present invention is to provide a pressure measuring layer coating liquid for forming a pressure measuring layer, which can be applied to the measurement of pressure or pressure distribution in the non-planar portion of an article having a non-planar portion, and can form a pressure measuring layer showing a coloring portion with excellent gradation even when pressurized in a low pressure range of, for example, 300 MPa or less. In addition, the second problem of the present invention is to provide a pressure measuring layer manufacturing method, which can be applied to the measurement of pressure or pressure distribution in the non-planar portion of an article having a non-planar portion, and can obtain a coloring portion with excellent gradation even when pressurized in a low pressure range of, for example, 300 MPa or less. In addition, the third problem of the present invention is to provide a pressure measuring layer-containing article with a non-planar portion formed using the pressure measuring layer coating liquid, and a pressure measuring layer-containing article with a non-planar portion formed by the pressure measuring layer manufacturing method. The pressure measuring layer-forming coating liquid of the present invention contains: microcapsules containing a coloring agent and an aromatic solvent; a coloring agent not contained in the microcapsules; a resin; and a solvent, wherein the content of the resin is 17% by mass or less relative to the total solid content.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a coating liquid for forming a pressure measuring layer, a method for producing a pressure measuring layer, and an article having a non-planar portion and having a pressure measuring layer. Background Art

[0002] In recent years, as products have become more functional and sophisticated, the need to measure pressure distribution has tended to increase.

[0003] For example, Patent Document 1 proposes "a pressure-sensitive color-forming resin material characterized in that at least one of a color-forming agent and a color-developing agent that develops color upon contact is encapsulated in microcapsules and the two are blended in a resin composition serving as a matrix."

[0004] Previous technical literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2007-132756 Summary of the invention

[0007] Technical issues to be solved by the invention

[0008] As a result of studying the pressure-sensitive color-forming resin material described in Patent Document 1, the inventors have found that if the pressure is not applied at a relatively high pressure, the color-forming portion generated by the reaction between the color-forming agent and the color-developing agent in the pressurized area is insufficient to obtain a good color distribution (gradation) corresponding to the pressure difference. In other words, it has been found that there is room for further improvement in the pressure-sensitive color-forming resin material so that a color-forming portion having excellent gradation can be obtained even when the pressure is applied at a low pressure range (for example, 300 MPa or less).

[0009] Furthermore, the surface shape of the object to be measured by pressure includes not only a flat surface but also a curved surface and a concave-convex surface. Therefore, in the pressure measuring component in the form of a film or a sheet, for the object to be measured having a surface shape other than a flat surface, the pressure measuring component may not be able to follow the surface of the object to be measured, and the pressure or pressure distribution measurement becomes difficult. Therefore, a pressure measuring component that can be used for a non-planar portion of an object having a non-planar portion is desired.

[0010] Therefore, the object of the present invention is to provide a coating liquid for forming a pressure measuring layer, which can be used for measuring the pressure or pressure distribution in the above-mentioned non-planar portion of an article having a non-planar portion, and can form a pressure measuring layer showing a color-developing portion with excellent gradient even when pressurized in a low pressure range (for example, below 300 MPa).

[0011] Furthermore, the object of the present invention is to provide a method for manufacturing a pressure measuring layer, which can be applied to the measurement of pressure or pressure distribution in a non-planar portion of an article having a non-planar portion, and can obtain a color-developing portion with excellent gradient properties even when pressurized in a low pressure range (for example, below 300 MPa).

[0012] Furthermore, the present invention aims to provide an article with a pressure measuring layer and a non-planar portion formed using the pressure measuring layer-forming coating liquid and an article with a pressure measuring layer and a non-planar portion formed by the pressure measuring layer manufacturing method.

[0013] Means for solving technical problems

[0014] The present inventors have conducted intensive studies to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved by the following configuration.

[0015] [1] A coating liquid for forming a pressure measuring layer, comprising:

[0016] Microcapsules containing colorants and aromatic solvents;

[0017] Color developing agent not contained in microcapsules;

[0018] Resins; and

[0019] Solvents,

[0020] The content of the resin is 17% by mass or less based on the total solid content of the pressure measuring layer forming coating liquid.

[0021] [2] The coating liquid for forming a pressure measuring layer according to [1], wherein

[0022] The content of the resin is 13% by mass or less based on the total solid content of the pressure measuring layer forming coating liquid.

[0023] [3] The coating liquid for forming a pressure measuring layer according to [1] or [2], which has a viscosity at 25° C. of less than 5000 mPa·s.

[0024] [4] The coating liquid for forming a pressure measuring layer according to any one of [1] to [3], wherein

[0025] The microcapsules containing the color former and the aromatic solvent contain substantially no color developer.

[0026] [5] The coating liquid for forming a pressure measuring layer according to any one of [1] to [4], wherein

[0027] The average particle size of the microcapsules contained in the pressure measuring layer-forming coating liquid is 5 μm or more.

[0028] [6] The coating liquid for forming a pressure measuring layer according to any one of [1] to [5], wherein

[0029] The developer comprises a material selected from activated clay, acid clay and zinc salicylate derivatives.

[0030] [7] The coating liquid for forming a pressure measuring layer according to [6], wherein

[0031] The above-mentioned developer is 3,5-bis(α-methylbenzyl)zinc salicylate.

[0032] [8] The coating liquid for forming a pressure measuring layer according to any one of [1] to [7], wherein

[0033] The particle size distribution of the microcapsules contained in the pressure measuring layer-forming coating liquid is 15% or more.

[0034] [9] The coating liquid for forming a pressure measuring layer according to any one of [1] to [8], wherein

[0035] The total content of the microcapsules containing the color former and the aromatic solvent and the color developer is 50% by mass or more based on the total solid content of the pressure measuring layer forming coating liquid.

[0036]

[10] The coating liquid for forming a pressure measuring layer according to any one of [1] to [9], wherein

[0037] The coloring agent is selected from compounds represented by the general formula (1) described below and compounds having an indole structure.

[0038]

[11] A method for producing a pressure measuring layer, comprising the step of applying a coating liquid for forming a pressure measuring layer to a non-planar portion of an article including the non-planar portion to form the pressure measuring layer, wherein:

[0039] The pressure measuring layer forming coating liquid comprises: microcapsules containing a color former and an aromatic solvent; a color former not contained in the microcapsules; a resin; and a solvent.

[0040] The average particle size of the microcapsules containing the color former and the aromatic solvent is X μm, and the solid content coating amount of the pressure measuring layer forming coating liquid is Y g / m 2 When Y / X is used, the solid content coating amount is Yg / m 2 The ratio to the average particle size X μm is less than 1.

[0041]

[12] The method for manufacturing a pressure measuring layer according to

[11] , wherein:

[0042] The content of the resin is 17% by mass or less based on the total solid content of the pressure measuring layer forming coating liquid.

[0043]

[13] The method for producing a pressure measuring layer according to [1+] or

[12] , wherein:

[0044] The content of the resin is 13% by mass or less based on the total solid content of the pressure measuring layer forming coating liquid.

[0045]

[14] The method for producing a pressure measuring layer according to any one of

[11] to

[13] , wherein:

[0046] The pressure measuring layer-forming coating liquid has a viscosity at 25° C. of less than 5000 mPa·s.

[0047]

[15] The method for producing a pressure measuring layer according to any one of

[11] to

[14] , wherein:

[0048] The microcapsules containing the color former and the aromatic solvent contain substantially no color developer.

[0049]

[16] The method for producing a pressure measuring layer according to any one of

[11] to

[15] , wherein:

[0050] The average particle size of the microcapsules contained in the pressure measuring layer-forming coating liquid is 5 μm or more.

[0051]

[17] The method for producing a pressure measuring layer according to any one of

[11] to

[16] , wherein:

[0052] The developer comprises a material selected from activated clay, acid clay and zinc salicylate derivatives.

[0053]

[18] The method for producing a pressure measuring layer according to any one of

[11] to

[17] , wherein:

[0054] The above-mentioned developer is 3,5-bis(α-methylbenzyl)zinc salicylate.

[0055]

[19] The method for producing a pressure measuring layer according to any one of

[11] to

[18] , wherein:

[0056] The particle size distribution of the microcapsules contained in the pressure measuring layer-forming coating liquid is 15% or more.

[0057]

[20] The method for producing a pressure measuring layer according to any one of

[11] to

[19] , wherein:

[0058] The total content of the microcapsules containing the color former and the aromatic solvent and the color developer is 50% by mass or more based on the total solid content of the pressure measuring layer forming coating liquid.

[0059]

[21] The method for producing a pressure measuring layer according to any one of

[11] to

[20] , wherein:

[0060] The coloring agent is selected from compounds represented by the general formula (1) described below and compounds having an indole structure.

[0061]

[22] An article containing a non-planar portion and having a pressure measuring layer, comprising: an article including a non-planar portion; and a pressure measuring layer arranged on the non-planar portion and formed using the pressure measuring layer forming coating liquid described in any one of [1] to

[10] .

[0062]

[23] An article having a non-planar portion and having a pressure measuring layer, which is obtained by the method for producing a coating liquid for forming a pressure measuring layer according to any one of

[11] to

[21] .

[0063] Effects of the Invention

[0064] According to the present invention, a coating liquid for forming a pressure measuring layer can be provided, which can be suitable for measuring the pressure or pressure distribution in the above-mentioned non-planar portion of an article having a non-planar portion, and can form a pressure measuring layer showing a color-developing portion with excellent gradient even when pressurized in a low pressure range (for example, below 300 MPa).

[0065] Furthermore, according to the present invention, a method for manufacturing a pressure measuring layer can be provided, which can be applicable to the measurement of pressure or pressure distribution in a non-planar portion of an article having a non-planar portion, and can obtain a color-developing portion with excellent gradient properties even when pressurized in a low pressure range (for example, below 300 MPa).

[0066] Furthermore, according to the present invention, there can be provided an article with a pressure measuring layer and a non-planar portion formed using the pressure measuring layer forming coating liquid and an article with a pressure measuring layer and a non-planar portion formed by the pressure measuring layer manufacturing method. BRIEF DESCRIPTION OF THE DRAWINGS

[0067] Figure 1 It is a schematic cross-sectional view showing an example of a pressure measuring layer formed from the coating liquid of the present invention and is a schematic view for showing the relationship between specific microcapsules and a binder.

[0068] Figure 2 It is a schematic cross-sectional view showing an example of a pressure measuring layer formed from the coating liquid of the present invention and is a schematic view for showing the relationship between specific microcapsules and a binder.

[0069] Figure 3 This is a schematic cross-sectional view showing an example of the non-planar portion-containing article with a pressure measuring layer of the present invention.

[0070] Figure 4 This is a schematic cross-sectional view showing an example of the non-planar portion-containing article with a pressure measuring layer of the present invention. DETAILED DESCRIPTION

[0071] Hereinafter, the present invention will be described in detail.

[0072] Although the description of the constituent elements described below may be made based on representative embodiments of the present invention, the present invention is not limited to such embodiments.

[0073] In addition, in this specification, the numerical range expressed using "to" means a range including the numerical values ​​described before and after "to" as the lower limit and the upper limit.

[0074] Furthermore, in the numerical ranges recorded in stages in this specification, the upper limit or lower limit recorded in a certain numerical range can be replaced by the upper limit or lower limit of other numerical ranges recorded in stages. Furthermore, in the numerical ranges recorded in this specification, the upper limit or lower limit recorded in a certain numerical range can also be replaced by the value shown in the embodiment.

[0075] The various components described below may be used alone or in combination of two or more. For example, the polyisocyanate described below may be used alone or in combination of two or more.

[0076] In the present specification, when simply referred to as a substituent, examples of the substituent include the following substituent T.

[0077] (Substituent T)

[0078] Examples of the substituent T include a halogen atom (a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.), an alkyl group, a cycloalkyl group, an alkenyl group, a cycloalkenyl group, an alkynyl group, an aryl group, a heterocyclic group, a cyano group, a hydroxyl group, a nitro group, a carboxyl group, an alkoxy group, an aryloxy group, a silyloxy group, a heterocyclic group, an acyloxy group, a carbamoyloxy group, an amino group (including an alkylamino group and an anilino group), an acylamino group, an aminocarbonylamino group, an alkoxycarbonylamino group, an aryloxycarbonylamino group, a sulfamoylamino group, an alkyl or arylsulfonylamino group, a mercapto group, an alkylthio group, an arylthio group, a heterocyclicthio group, a sulfamoyl group, a sulfonic acid group, an alkyl or arylsulfinyl group, an alkyl or arylsulfonyl group, an acyl group, an aryloxycarbonyl group, an alkoxycarbonyl group, a carbamoyl group, an aryl or heterocyclic azo group, an imide group, a phosphinyl group, a phosphinyloxy group, a phosphinylamino group, a silyl group, and a group containing a polymerizable group.

[0079] Among the above-mentioned substituents, regarding a substituent having a hydrogen atom, the hydrogen atom part in the substituent may be further substituted with any of the above-mentioned substituents.

[0080] In this specification, unless otherwise specified, the weight average molecular weight (Mw) and the number average molecular weight (Mn) are values ​​calculated in terms of polystyrene by gel permeation chromatography (GPC).

[0081] In addition, in this specification, unless otherwise specified, the molecular weight of a compound having a molecular weight distribution is a weight average molecular weight (Mw).

[0082] In this specification, the "solid content" of the coating liquid for forming a pressure measuring layer refers to the components that form the pressure measuring layer formed using the coating liquid for forming a pressure measuring layer, and when the coating liquid for forming a pressure measuring layer contains a solvent (organic solvent, water, etc.), it refers to all components other than the solvent. In addition, if it is a component that forms the coating liquid for forming a pressure measuring layer, the liquid component is also regarded as a solid component.

[0083] [Pressure measurement layer forming coating liquid]

[0084] The coating liquid for forming a pressure measuring layer of the present invention (hereinafter, also referred to as "coating liquid" or "coating liquid A") contains microcapsules containing a coloring agent and an aromatic solvent (hereinafter, also referred to as "specific microcapsules"), a coloring agent not contained in the microcapsules (hereinafter, also referred to as "developer"), a resin and a solvent.

[0085] The content of the resin is 17% by mass or less based on the total solid content of the pressure measuring layer forming coating liquid.

[0086] The coating liquid of the present invention having the above-mentioned structure can be used for measuring the pressure or pressure distribution in the non-planar portion of an article having the non-planar portion, and can form a pressure measuring layer showing a color-developing portion with excellent gradation even when pressurized in a low pressure range (for example, below 300 MPa).

[0087] Although the mechanism of action of the above-mentioned configuration and effect is not clear, the present inventors speculate as follows.

[0088] The main characteristic point of the coating liquid of the present invention is that the content of the resin in the coating liquid is 17% by mass or less relative to the total solid content. In addition, it is believed that the above-mentioned resin acts as a resin binder that supports specific microcapsules and color developers in the pressure measurement layer formed by the coating liquid of the present invention. Since the content of the resin binder in the pressure measurement layer formed by the coating liquid of the present invention is set to be less than a specified amount, when the pressure measurement object is coated with the coating amount per unit area generally used in pressure measurement, the specific microcapsules are not easily buried in the resin binder. That is, it is believed that the pressure measurement layer formed by the coating liquid of the present invention is easy to take Figure 1 or Figure 2 Specifically, Figure 1 As shown in FIG. 1 , it is easy to adopt a mode in which a region of the specific microcapsule 14 completely protrudes from the film 12 of the resin binder that holds the specific microcapsule 14 and supports it on the coated surface of the measurement object 10. Figure 2 As shown in FIG. 1 , it is easy to adopt a mode in which a region of the specific microcapsule 14 protrudes from the film 12 of the resin binder that holds the specific microcapsule 14 and is supported on the coated surface of the measurement object 10, and a coating 15 that is a thin film of the above-mentioned resin binder is provided on the surface (a region of the surface or the entire region of the surface) of the region protruding from the film 12 of the specific microcapsule 14. That is, Figure 1 and Figure 2 As shown, the pressure measuring layer formed by the coating solution of the present invention is presumed to be easily destroyed when pressurized because the particle size D1 of the specific microcapsules 14 is larger than the thickness D2 of the film 12. As a result, even when pressurized at a pressure in a low pressure range (e.g., 300 MPa or less), good color development (color development density) and gradation can be easily obtained.

[0089] Furthermore, as described above, the coating liquid of the present invention can be applied to the measurement of pressure or pressure distribution in a non-planar portion of an object having a non-planar portion. That is, even for a measurement object that is difficult to measure in the form of a conventional film or sheet, a pressure measurement layer can be formed at a coating amount per unit area that is generally used in pressure measurement without being affected by the surface shape.

[0090] Hereinafter, the fact that the pressure measuring layer formed of the coating solution of the present invention has better color density, gradation and image quality and the coating properties of the coating solution of the present invention is also referred to as “the effect of the present invention is better”.

[0091] Hereinafter, first, various components contained in the coating liquid of the present invention will be described.

[0092] [Microcapsules containing a coloring agent and an aromatic solvent (specific microcapsules)]

[0093] The coating liquid of the present invention contains microcapsules (specific microcapsules) containing a coloring agent and an aromatic solvent.

[0094] Hereinafter, first, the materials constituting the specific microcapsules will be described in detail.

[0095] Microcapsules generally have a core and a capsule wall for enclosing a core material constituting the core (an enclosed component (also referred to as an included component)).

[0096] In the present invention, the specific microcapsules contain a coloring agent and an aromatic solvent as core materials (internal components). Since the coloring agent is contained in the microcapsules, the coloring agent can be stably present until the microcapsules are broken by applying pressure.

[0097] The capsule wall and core materials are described below.

[0098] <Capsule wall>

[0099] Examples of the wall material contained in the capsule wall of the specific microcapsule include polyethylene, polystyrene, polyvinyl, polyurethane, polyurea, and polyurethane polyurea.

[0100] The wall material included in the capsule wall preferably includes a polymer obtained using an isocyanate compound and an organic solvent, more preferably includes a polymer having at least one of an aminocaproate bond and a urea bond, and further preferably includes polyurethane polyurea.

[0101] <Core Material>

[0102] Certain microcapsules contain a chromogen as a core material.

[0103] (Coloring Agent)

[0104] The "color former" refers to a compound that develops color from a colorless state by contact with a color developer described later. As the color former, an electron donating dye precursor (a precursor of a color-developing dye) is preferred. That is, as the color former, an electron donating colorless dye is preferred.

[0105] As the electron-donating dye precursor, for example, compounds such as triarylmethanephthalide lactone compounds, fluorane compounds, phenothiazine compounds, indolylphthalide lactone compounds, colorless gold amine compounds, rhodamine lactam compounds, triarylmethane compounds, diphenylmethane compounds, triazene compounds, spiropyran compounds, fluorene compounds, pyridine compounds, and pyrazine compounds can be enumerated. In addition, for the details of these compounds, the record of Japanese Patent Laid-Open No. 5-257272 can be referenced.

[0106] Examples of the coloring agent include 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-n-octyl-2-methylindol-3-yl)phthalide, 3-[2,2-bis(1-ethyl-2-methylindol-3-yl)vinyl]-3-(4-diethylaminophenyl)-phthalide, 2-anilino-6-dibutylamino-3-methylfluoran, 6-diethylamino-3-methyl-2-(2,6-dimethylanilino)-fluoran, and 2-(2-chloroanilino)-6-dibutylaminofluoran. , 3,3-bis(4-dimethylaminophenyl)-6-dimethylaminophthalide, 2-anilino-6-diethylamino-3-methylfluoran, 9-[ethyl(3-methylbutyl)amino]spiro[12H-benzo[a]xanthene-12,1'(3'H)isobenzofuran]-3'-one and 2'-methyl-6'-(N-p-tolyl-Nethylamino)spiro[isobenzofuran-1(3H),9'-[9H]xanthene]-3-one, 3',6'-bis(diethylamino)-2-(4-nitrophenyl)spiro[isoindole-1,9'-xanthene]-3-one and 6'-(diethylamino)-1',3'-dimethylfluoran, etc. Furthermore, as the coloring agent, Pink-DCF and Orange-DCF (both manufactured by HODOGAYA CHEMICAL CO., LTD.) can also be used.

[0107] Furthermore, the electron donating dye precursor is preferably a compound represented by the following general formula (1) or a compound having an indole structure. The compound represented by the general formula (1) and the compound having an indole structure are described in detail below.

[0108] <<Compound represented by general formula (1)>>

[0109] [Chemical formula 1]

[0110]

[0111] In the general formula (1), R 1 and R 3 Each independently represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.

[0112] R 1 and R 3 The number of carbon atoms in the alkyl group is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, from the viewpoint of achieving more excellent effects of the present invention.

[0113] The type of the substituent that the alkyl group or the aryl group may have is not particularly limited, and the substituents exemplified in the substituent T described above may be mentioned.

[0114] Among them, from the viewpoint of more excellent effect of the present invention, as R 1 and R 3 , each independently preferably an alkyl group which may have a substituent or an aryl group which may have a substituent, more preferably an alkyl group which may have a substituent, and further preferably an unsubstituted alkyl group.

[0115] R 2 and R 4 Each independently represents an alkyl group which may have a substituent or an aryl group which may have a substituent.

[0116] R 2 and R 4 The number of carbon atoms in the alkyl group is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, from the viewpoint of achieving more excellent effects of the present invention.

[0117] R 2 and R 4 The aryl group represented may be a monocyclic structure or a polycyclic structure.

[0118] The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and the substituents exemplified in the substituent T described above may be mentioned.

[0119] Among them, from the viewpoint of more excellent effect of the present invention, as R 2 and R 4 , each independently preferably is an alkyl group which may have a substituent, and more preferably is an unsubstituted alkyl group.

[0120] Among them, R is preferred 1 ~R 4 All are unsubstituted alkyl groups, and more preferably are the same unsubstituted alkyl groups.

[0121] X 1 Indicates -O- or -NR 5 Among them, from the viewpoint of more excellent effect of the present invention, -NR 5 -.

[0122] R 5 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.

[0123] R 5 The number of carbon atoms in the alkyl group is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, from the viewpoint of achieving more excellent effects of the present invention.

[0124] R 5 The aryl group represented may be a monocyclic structure or a polycyclic structure.

[0125] The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and the substituents exemplified in the substituent T described above may be mentioned.

[0126] Among them, from the viewpoint of more excellent effect of the present invention, as R 5 , preferably an aryl group which may have a substituent, more preferably an aryl group substituted with a group selected from a halogen atom, a cyano group, a nitro group and a carboxyl group.

[0127] As the above-mentioned aryl group, a phenyl group is preferred.

[0128] Examples of the compound represented by the general formula (1) include 3',6'-bis(diethylamino)-2-(4-nitrophenyl)spiro[isoindol-1,9'-xanthene]-3-one and the like.

[0129] The molecular weight of the compound represented by the general formula (1) is not particularly limited, but is preferably 300 or more, more preferably 500 or more. The upper limit is not particularly limited, but is preferably 2000 or less, more preferably 1000 or less.

[0130] 《Compounds with indole structure》

[0131] The compound having an indole structure is a compound having an indole structure as a partial structure.

[0132] The number of indole structures in the compound having an indole structure is not particularly limited, and may be one or more. However, from the viewpoint of achieving a more excellent effect of the present invention, two or more indole structures are preferred, and two indole structures are more preferred.

[0133] As the compound having an indole structure, a compound represented by the general formula (2) or a compound represented by the general formula (3) is preferred, and a compound represented by the general formula (3) is more preferred.

[0134] [Chemical formula 2]

[0135]

[0136] In the general formula (2), R 6 and R 7 Each independently represents a hydrogen atom or an alkyl group which may have a substituent.

[0137] R 6 The number of carbon atoms in the alkyl group is not particularly limited, but is preferably 1 to 30, more preferably 1 to 20, further preferably 1 to 12, and particularly preferably 5 to 10 from the viewpoint of achieving more excellent effects of the present invention.

[0138] R 7The number of carbon atoms in the alkyl group is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, and even more preferably 1 to 3 from the viewpoint of achieving more excellent effects of the present invention.

[0139] The type of the substituent that the alkyl group may have is not particularly limited, and the substituents exemplified in the substituent T described above may be mentioned.

[0140] Among them, from the viewpoint of more excellent effect of the present invention, R 6 and R 7 It preferably represents an alkyl group which may have a substituent, and more preferably represents an unsubstituted alkyl group.

[0141] R 8 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.

[0142] R 8 The number of carbon atoms in the alkyl group is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, from the viewpoint of achieving more excellent effects of the present invention.

[0143] R 8 The aryl group represented may be a monocyclic structure or a polycyclic structure.

[0144] The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and the substituents exemplified in the substituent T described above may be mentioned.

[0145] Among them, from the viewpoint of more excellent effect of the present invention, as R 8 , preferably an aryl group which may have a substituent, more preferably an aryl group which has a substituent.

[0146] X 2 Indicates -O- or -NR 9 -.

[0147] Among them, from the viewpoint of more excellent effect of the present invention, as X 2 , preferably -O-.

[0148] R 9 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.

[0149] R 9 The number of carbon atoms in the alkyl group is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, from the viewpoint of achieving more excellent effects of the present invention.

[0150] R 9 The aryl group represented may be a monocyclic structure or a polycyclic structure.

[0151] The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and the substituents exemplified in the substituent T described above may be mentioned.

[0152] The molecular weight of the compound represented by the general formula (2) is not particularly limited, but is preferably 300 or more, more preferably 500 or more. The upper limit is not particularly limited, but is preferably 2000 or less, more preferably 1000 or less.

[0153] [Chemical formula 3]

[0154]

[0155] In the general formula (3), R 10 ~R 13 Each independently represents a hydrogen atom or an alkyl group which may have a substituent.

[0156] R 10 and R 12 The number of carbon atoms in the alkyl group is not particularly limited, but is preferably 1 to 30, more preferably 1 to 20, further preferably 1 to 12, and particularly preferably 5 to 10 from the viewpoint of achieving more excellent effects of the present invention.

[0157] R 11 and R 13 The number of carbon atoms in the alkyl group is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, and even more preferably 1 to 3 from the viewpoint of achieving more excellent effects of the present invention.

[0158] The type of the substituent that the alkyl group may have is not particularly limited, and the substituents exemplified in the substituent T described above may be mentioned.

[0159] Among them, from the viewpoint of more excellent effect of the present invention, as R 10 ~R 13 , preferably an alkyl group which may have a substituent, and more preferably an unsubstituted alkyl group.

[0160] X 3 Indicates -O- or -NR 14 -.

[0161] Among them, from the viewpoint of more excellent effect of the present invention, as X 3 , preferably -O-.

[0162] R 14 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.

[0163] R 14 The number of carbon atoms in the alkyl group is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, from the viewpoint of achieving more excellent effects of the present invention.

[0164] R 14 The aryl group represented may be a monocyclic structure or a polycyclic structure.

[0165] The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and the substituents exemplified in the substituent T described above may be mentioned.

[0166] Specific examples of the compound represented by the general formula (3) include 3,3-bis(2-methyl-1-octyl-3-indolyl)phthalidene.

[0167] The molecular weight of the compound represented by the general formula (3) is not particularly limited, but is preferably 300 or more, more preferably 500 or more. The upper limit is not particularly limited, but is preferably 2000 or less, more preferably 1000 or less.

[0168] As the coloring agent, from the viewpoint of achieving more excellent effects of the present invention, it is preferably selected from among compounds represented by the general formula (1) and compounds having an indole structure.

[0169] The coloring agent may be used alone or in combination of two or more.

[0170] The content of the coloring agent (the total content when two or more coloring agents are included) is not particularly limited, but is preferably 1 to 50% by mass, more preferably 3 to 35% by mass, and further preferably 5 to 25% by mass, based on the total mass of the core material.

[0171] The content of the coloring agent selected from the compound represented by the general formula (1) and the compound having an indole structure (the total content when two or more are included) is preferably 20 to 100% by mass, more preferably 40 to 100% by mass, based on the total mass of the coloring agent.

[0172] (Aromatic solvents)

[0173] The specific microcapsules contain an aromatic solvent as a core material.

[0174] The aromatic solvent is a solvent having an aromatic ring. The aromatic solvent is preferably liquid at 25°C.

[0175] The aromatic solvent is not particularly limited, but preferably contains a compound having at least one aromatic ring and no aromatic condensed ring (specific aromatic solvent).

[0176] The number of aromatic rings contained in the specific aromatic solvent is not particularly limited, but from the viewpoint of more excellent effects of the present invention, it is preferably 1 or more. The upper limit is not particularly limited, but is preferably 5 or less, more preferably 3 or less, and further preferably 1 or 2.

[0177] Furthermore, the aromatic ring may have a substituent. As the substituent that the aromatic ring may have, the groups exemplified as the substituent T described above can be mentioned.

[0178] Furthermore, the specific aromatic solvent does not have an aromatic condensed ring. An aromatic condensed ring refers to a ring formed by condensing two or more aromatic rings.

[0179] The aromatic solvent preferably contains a compound represented by the general formula (5).

[0180] [Chemical formula 4]

[0181]

[0182] In the general formula (5), R 20 ~R 24 Each independently represents a hydrogen atom, an alkyl group which may have a substituent, or a monocyclic aromatic group which may have a substituent.

[0183] R 20 ~R 24 The number of carbon atoms in the alkyl group is not particularly limited, but is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 5 from the viewpoint of achieving more excellent effects of the present invention.

[0184] R 20 ~R 24 The monocyclic aromatic group represented here means a monocyclic aromatic group, and examples thereof include a benzene ring group and a monocyclic aromatic heterocyclic group.

[0185] Among them, from the viewpoint of excellent effect of the present invention, as R 20 ~R 24 , preferably a hydrogen atom or an alkyl group which may have a substituent.

[0186] The type of the substituent that the alkyl group and the monocyclic aromatic group may have is not particularly limited, and the substituents exemplified in the substituent T described above may be mentioned.

[0187] L represents a single bond or an arylene group which may have a substituent.

[0188] The number of carbon atoms in the arylene group represented by L is not particularly limited, but is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 5 from the viewpoint of achieving more excellent effects of the present invention.

[0189] Among them, from the viewpoint of further excellent effects of the present invention, L is preferably an arylene group which may have a substituent.

[0190] The type of the substituent that the arylene group may have is not particularly limited, and the groups exemplified in the substituent T described above can be mentioned.

[0191] R 25 represents a hydrogen atom or a monocyclic aromatic group which may have a substituent.

[0192] R 25 The monocyclic aromatic group represented here means a monocyclic aromatic group, and examples thereof include a benzene ring group and a monocyclic aromatic heterocyclic group.

[0193] The type of the substituent that the monocyclic aromatic group may have is not particularly limited, and the substituents exemplified in the substituent T described above may be mentioned.

[0194] Among them, from the viewpoint of excellent effect of the present invention, as R 25 , preferably a monocyclic aromatic group which may have a substituent.

[0195] The specific aromatic solvents are not particularly limited, and examples thereof include alkylbenzene compounds such as linear alkylbenzene, diarylalkane compounds such as 1,1-diphenylethane and 1-phenyl-1-(2,3-xylyl)ethane, alkylbiphenyl compounds such as isopropylbiphenyl, triarylmethane compounds, diarylalkylene compounds, and aromatic hydrocarbons such as arylindan compounds.

[0196] Among them, the aromatic solvent is preferably an alkylbenzene compound or a diarylalkane compound from the viewpoint of excellent solubility of the compound having a benzotriazole structure.

[0197] The aromatic solvents may be used alone or in combination of two or more.

[0198] Among them, from the viewpoint of achieving more excellent effects of the present invention, it is preferred to use two or more aromatic solvents, and more preferably to use a mixture of 2 to 5 kinds.

[0199] Aromatic solvents other than the specific aromatic solvents may be used in combination.

[0200] The content of the aromatic solvent (the total content when multiple types are included) is not particularly limited, but is preferably 30 to 95% by mass, more preferably 40 to 90% by mass, and further preferably 50 to 80% by mass, relative to the total mass of the core material.

[0201] The content of the specific aromatic solvent is preferably 50 to 100% by mass, more preferably 75 to 100% by mass, based on the total mass of the aromatic solvent.

[0202] The content of the aromatic solvent in the specific microcapsule is not particularly limited, but is preferably 20 to 80% by mass, more preferably 30 to 70% by mass, based on the total mass of the specific microcapsule, from the viewpoint of achieving excellent desired effects of the present invention.

[0203] (Other ingredients)

[0204] The specific microcapsules may contain other components besides the above-mentioned coloring agent and aromatic solvent. Examples of other components include additives such as aliphatic solvents, ultraviolet absorbers, light stabilizers, antioxidants, paraffin wax, and odor suppressants.

[0205] The specific microcapsules also preferably contain an aliphatic solvent.

[0206] The aliphatic solvent refers to a solvent containing a compound having an aliphatic group, that is, a solvent containing a compound having no aromatic ring.

[0207] The aliphatic solvent is not particularly limited, and examples thereof include aliphatic hydrocarbons such as isoparaffin and dibutyl phthalate; natural animal and plant oils such as soybean oil, corn oil, cottonseed oil, rapeseed oil, olive oil, coconut oil, castor oil and fish oil; and high-boiling-point fractions of natural products such as mineral oil.

[0208] Among them, from the viewpoint of achieving more excellent effects of the present invention, the aliphatic solvent is preferably an aliphatic hydrocarbon, and more preferably an isoparaffin.

[0209] The aliphatic solvent may be used alone or in combination of two or more.

[0210] The content of the aliphatic solvent in the specific microcapsule is not particularly limited, but is preferably 5 to 40% by mass, more preferably 10 to 30% by mass, based on the total mass of the aromatic solvent, from the viewpoint of achieving excellent desired effects of the present invention.

[0211] The specific microcapsule preferably contains an ultraviolet absorber. The ultraviolet absorber is an organic compound having a function of absorbing ultraviolet rays irradiated from the outside.

[0212] As the ultraviolet absorber, a compound having a benzotriazole structure is preferred.

[0213] The number of benzotriazole structures in the compound having a benzotriazole structure is not particularly limited, and may be one or more.

[0214] As the compound having a benzotriazole structure, a compound represented by the general formula (4) is preferred.

[0215] [Chemical formula 5]

[0216]

[0217] In the general formula (4), R 15 ~R 18 Each independently represents a hydrogen atom or a substituent.

[0218] As R 15 ~R 18 The substituent represented is not particularly limited, and the groups exemplified in the substituent T described above can be mentioned.

[0219] Among them, when R 15 ~R 18 When R is a substituent, from the viewpoint of excellent effects of the present invention, it is preferred that 15 ~R 18 At least one of them is a halogen atom.

[0220] R 19 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.

[0221] R 19 The aryl group represented may be a monocyclic structure or a polycyclic structure.

[0222] The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and the substituents exemplified in the substituent T described above may be mentioned.

[0223] Among them, from the viewpoint of excellent effect of the present invention, as R 19 , the aryl group may have a substituent, and more preferably the aryl group is substituted with at least one hydroxyl group.

[0224] As the above-mentioned aryl group, a phenyl group is preferred.

[0225] The molecular weight of the compound having a benzotriazole structure is not particularly limited, but from the viewpoint of more excellent effects of the present invention, it is preferably 500 or less, more preferably 400 or less, and further preferably 350 or less. The lower limit is not particularly limited, but is often greater than 100. When the molecular weight of the compound having a benzotriazole structure is small, it is easily dissolved in the above-mentioned aromatic solvents, resulting in better storage stability.

[0226] The compound having a benzotriazole structure is not particularly limited, and examples thereof include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-5'-tert-butylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-tert-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-dodecyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3',5 '-di-tert-amylphenyl)benzotriazole, 2-(2'-hydroxy-5'-(1,1,3,3-tetramethylbutyl)phenyl)benzotriazole, 2-(2'-hydroxy-4'-octyloxyphenyl)benzotriazole, 2-(2'-hydroxy-3'-(3,4,5,6-tetrahydrophthalimidomethyl)-5'-methylbenzylphenyl)benzotriazole, 2-(3'-sec-butyl-5'-tert-butyl-2'-hydroxyphenyl)benzotriazole, 2-(3',5'-bis-(α,α-dimethylbenzyl)-2'-hydroxyphenyl)benzotriazole triazole, 2-(3'-tert-butyl-2'-hydroxy-5'-(2-octyloxycarbonylethyl)phenyl)-5-chloro-benzotriazole, 2-(3'-tert-butyl-5'-[2-(2-ethylhexyloxy)-carbonylethyl]-2'-hydroxyphenyl)-5-chloro-benzotriazole, 2-(3'-tert-butyl-2'-hydroxy-5'-(2-methoxycarbonylethyl)phenyl)-5-chloro-benzotriazole, 2-(3'-tert-butyl-2'-hydroxy-5'-(2-methoxycarbonylethyl)phenyl)benzotriazole, 2-(3'-tert-butyl phenyl)benzotriazole, 2-(3'-tert-butyl-2'-hydroxy-5'-(2-octyloxycarbonylethyl)phenyl)benzotriazole, 2-(3'-tert-butyl-5'-[2-(2-ethylhexyloxy)carbonylethyl]-2'-hydroxyphenyl)benzotriazole, 2-(3'-dodecyl-2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(3'-tert-butyl-2'-hydroxy-5'-(2-isooctyloxycarbonylethyl)phenyl)benzotriazole and 2,2'-methylene-bis[4-(1,1,3,3-tetramethylbutyl)-6-benzotriazol-2-ylphenol].

[0227] Among them, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole or 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole is preferred as the compound having a benzotriazole structure because the effects of the present invention are more excellent.

[0228] The compound having a benzotriazole structure may be used alone or in combination of two or more.

[0229] The content of the compound having a benzotriazole structure in the specific microcapsule is not particularly limited, but is preferably 10% by mass or more, more preferably 20% by mass or more, and further preferably 30% by mass or more relative to the coloring agent from the viewpoint of achieving better effects of the present invention.

[0230] The upper limit is not particularly limited, but is preferably 500% by mass or less, more preferably 300% by mass or less, and further preferably 100% by mass or less from the viewpoint of solubility of the compound having a benzotriazole structure.

[0231] As the ultraviolet absorber, ultraviolet absorbers other than the compound having a benzotriazole structure may be used.

[0232] The content of the ultraviolet absorber other than the compound having a benzotriazole structure is preferably 0 to 50% by mass, more preferably 0 to 25% by mass, based on the total mass of the compound having a benzotriazole structure.

[0233] The specific microcapsule preferably contains substantially no color developer. “Substantially contains” means that the content of the color developer is 1% by mass or less relative to the total mass of the core material of the specific microcapsule.

[0234] (Method for producing specific microcapsules)

[0235] The method for producing the specific microcapsules is not particularly limited, and a method having a step of forming the specific microcapsules using the above-mentioned coloring agent, the above-mentioned aromatic solvent and the capsule wall material can be cited. Specifically, known methods such as interfacial polymerization, internal polymerization, phase separation, external polymerization and gel method can be cited. Among them, interfacial polymerization is preferred.

[0236] Hereinafter, the interfacial polymerization method will be described as an example of a method for producing specific microcapsules whose capsule walls are polyurea or polyurethaneurea.

[0237] As the interfacial polymerization method, an interfacial polymerization method is preferably one that includes the following steps: a step of dispersing an oil phase containing a colorant, an aromatic solvent and a capsule wall material (for example, a raw material containing polyisocyanate and at least one selected from polyols and polyamines. In addition, when polyisocyanate is reacted with water to produce polyamines in the system, polyols and polyamines can be omitted) in an aqueous phase containing an emulsifier to prepare an emulsion (emulsification step); and a step of polymerizing the capsule wall material at the interface between the oil phase and the aqueous phase to form a capsule wall and form specific microcapsules containing the colorant (encapsulation step).

[0238] The mass ratio of the total amount of polyol and polyamine to the amount of polyisocyanate in the raw materials (total amount of polyol and polyamine / amount of polyisocyanate) is not particularly limited, but is preferably 0.1 / 99.9 to 30 / 70, more preferably 1 / 99 to 25 / 75.

[0239] Furthermore, the type of the emulsifier used in the emulsification step is not particularly limited, and examples thereof include a dispersant and a surfactant.

[0240] Examples of the dispersant include resins such as polyvinyl alcohol.

[0241] The number average wall thickness of the specific microcapsules is not particularly limited, but is preferably, for example, 10 to 1000 nm.

[0242] The wall thickness of a specific microcapsule refers to the thickness (μm) of the capsule wall of capsule particles constituting the specific microcapsule, and the number average wall thickness refers to the average value of the capsule wall thickness (μm) of five specific microcapsules measured using a scanning electron microscope (SEM).

[0243] Specifically, the number average wall thickness of the specific microcapsules is measured by the following method.

[0244] First, the coating liquid is applied to an arbitrary support to form a coating film. The obtained coating film is sliced, the formed cross section is observed using a SEM, and 5 arbitrary specific microcapsules are selected. The cross section of each selected specific microcapsule is observed, the thickness of the capsule wall is measured, and the average value is calculated.

[0245] As shown in the following formula, the wall thickness of a specific microcapsule (thickness of the capsule wall) depends on the relationship between the capsule wall and the contents and the particle size of the specific microcapsule, and can be adjusted according to the particle size of the specific microcapsule (average primary particle size), the density of the capsule wall (wall density), the amount of the solute, solvent and auxiliary solvent contained in the specific microcapsule, the density of the solute and solvent and auxiliary solvent contained in the specific microcapsule, the amount of wall material (wall material amount), etc.

[0246] Specifically, for example, by increasing the amount of the solute, solvent, and auxiliary solvent (ie, the inclusions) contained in a specific microcapsule, the capsule wall can be adjusted to a thin thickness.

[0247] [Formula 1]

[0248] δ=D×10 3 / 2×{[(S×ρ+W×γ×G) / (S×ρ)] 1 / 3 -1}

[0249] δ: Capsule wall thickness [nm]

[0250] D: Particle size of microcapsules [μm)

[0251] S: Amount of solute, solvent and auxiliary solvent contained in microcapsules [kg]

[0252] ρ: wall density [kg / L]

[0253] W: Material quantity [kg]

[0254] γ: reaction rate [-]

[0255] G: Density of solute, solvent and auxiliary solvent contained in microcapsule [kg / L]

[0256] The specific microcapsules may be used alone or in combination of two or more.

[0257] In the coating liquid of the present invention, the content of the specific microcapsules is preferably 10 to 70% by mass, more preferably 20 to 50% by mass, and even more preferably 20 to 45% by mass based on the total solid content of the coating liquid.

[0258] The contents of the specific macrocapsules, the color developer, and the resin in the coating liquid can be identified using various measuring devices, for example, after subjecting the coating liquid to centrifugal separation to separate the components.

[0259] 〔Other microcapsules〕

[0260] The coating liquid of the present invention may contain other microcapsules (hereinafter also referred to as "other microcapsules") other than the specific microcapsules within a range that does not hinder the effects of the present invention. The other microcapsules are not particularly limited, and examples thereof include macrocapsules that do not contain aromatic solvents and microcapsules that do not contain coloring agents.

[0261] In the macrocapsules (referring to the specific microcapsules and all other microcapsules that may be arbitrarily contained) contained in the coating liquid of the present invention, the content of the specific microcapsules is preferably 85 to 100 mass %, more preferably 95 to 100 mass %, further preferably 98 to 100 mass %, particularly preferably 99 to 100 mass %, and most preferably 100 mass %, relative to the total mass of the microcapsules.

[0262] [Average particle size and particle size distribution of microcapsules contained in the coating liquid of the present invention]

[0263] Next, preferred aspects of the average particle size and particle size distribution of the microcapsules (the "microcapsules" referred to herein refer to all of the specific microcapsules and other microcapsules that may be arbitrarily included) contained in the coating liquid of the present invention will be described.

[0264] The average particle size of the microcapsules contained in the coating solution of the present invention is not particularly limited, and is preferably 1 μm or more, more preferably 5 μm or more, based on the volume-based median particle size (D50), but from the perspective of the better effect of the present invention, it is further preferably 10 μm or more, and particularly preferably 15 μm or more. And, as its upper limit, it is preferably 200 μm or less, more preferably less than 100 μm, further preferably 80 μm or less, and particularly preferably 50 μm or less.

[0265] Here, the volume-based median diameter (D50) of the microcapsules refers to the diameter at which the volumes of the larger and smaller diameter particles are equal when the microcapsules are divided into two parts using the particle diameter at which the cumulative volume of the entire microcapsules is 50% as a threshold.

[0266] The particle size distribution of the microcapsules contained in the coating solution of the present invention is preferably 10% or more, more preferably 15% or more, and further preferably 20% or more from the viewpoint of achieving a more excellent effect of the present invention. In addition, the upper limit is not particularly limited, but is preferably 40% or less.

[0267] The volume-based median diameter and particle size distribution of the microcapsules can be controlled by adjusting the production conditions of the microcapsules and the like.

[0268] The volume-based particle size distribution and median diameter (D50) of the microcapsules contained in the coating solution of the present invention can be measured using a laser diffraction / scattering particle size distribution measuring apparatus (apparatus: for example, Microtrac MT3300EXII (manufactured by Nikkiso Co., Ltd.)) for the microcapsules dispersed in the solution.

[0269] When the volume-based median diameter (D50) of the microcapsules contained in the coating solution of the present invention is measured in a coating state, the surface of the coating is photographed at a magnification of 150 times using an optical microscope, and the sizes of all microcapsules within a randomly set range of 2 cm×2 cm are measured for calculation.

[0270] 〔Color developer〕

[0271] The coating liquid of the present invention contains a developer.

[0272] In addition, the "developer" mentioned here refers to a developer that exists outside the microcapsule (in other words, is not contained in the microcapsule). That is, the coating solution of the present invention contains specific microcapsules and may also contain other microcapsules other than the specific microcapsules, but the "developer" mentioned here refers to a developer that is not contained in any microcapsule but exists outside the microcapsule.

[0273] The color developer is a compound that has no color-developing function by itself but has the property of causing the color-developing agent to develop color when in contact with the color-developing agent. As the color developer, an electron-accepting compound (electron-accepting compound) is preferred.

[0274] Examples of the electron accepting compound include clay substances such as activated clay, acid clay, attapulgite, zeolite, bentonite, and kaolin, phenolic compounds, zinc salicylate derivatives, and hydroxybenzoic acid esters.

[0275] Specific examples of the electron accepting compound include 2,2-bis(4-hydroxyphenyl)propane [also known as bisphenol A], 2,2-bis(4-hydroxyphenyl)hexafluoropropane [also known as bisphenol AF], 2,2-bis(p-hydroxyphenyl)pentane, 2,2-bis(p-hydroxyphenyl)ethane, 2,2-bis(p-hydroxyphenyl)butane, 2,2-bis(4'-hydroxy-3',5'-dichlorophenyl)propane, 1,1-(p-hydroxyphenyl)cyclohexane, 1, 1-(p-hydroxyphenyl) propane, 1,1-(p-hydroxyphenyl) pentane, 1,1-(p-hydroxyphenyl)-2-ethylhexane, 3,5-bis(α-methylbenzyl) salicylic acid and its polyvalent metal salts, 3,5-di(tert-butyl) salicylic acid and its polyvalent metal salts, 3-α,α-dimethylbenzyl salicylic acid and its polyvalent metal salts, butyl p-hydroxybenzoate, benzyl p-hydroxybenzoate, 2-ethylhexyl p-hydroxybenzoate, p-phenylphenol and p-cumylphenol, etc. In addition, as the electron accepting compound, the compound represented by the general formula (1) described in paragraphs 0051 to 0060 of International Publication No. 2018 / 199044A1 can also be used.

[0276] As the electron accepting compound, from the viewpoint of more excellent effects of the present invention, it is preferred to select at least one of activated clay, acidic clay, kaolin, phenolic compounds (e.g., bisphenolic compounds), zinc salicylate derivatives and hydroxybenzoic acid esters, more preferably selected from at least one of activated clay, acidic clay and zinc salicylate derivatives, and further preferably 3,5-bis(α-methylbenzyl)zinc salicylate.

[0277] When the electron accepting compound is particulate, its shape is not particularly limited, and may be any of spherical, elliptical, cubic, needle-shaped, and irregular shapes, etc. The same applies when the electron accepting compound particles are aggregates of a plurality of particles.

[0278] The color developer may be used alone or in combination of two or more.

[0279] The color developer can be surface-modified with a dispersant such as sodium hexametaphosphate.

[0280] In the coating liquid of the present invention, the content of the colorant (when the colorant is surface-modified by a dispersant, it refers to the content of the colorant after surface modification. That is, the content of the colorant surface-modified by a dispersant) is not particularly limited, but is preferably 20 to 90% by mass, more preferably 50 to 80% by mass, relative to the total solid content of the coating liquid.

[0281] In the coating solution of the present invention, the mass content ratio (specific microcapsules / developer) of the specific microcapsules and the color developer (when the color developer is surface-modified by a dispersant, it is the surface-modified color developer) is preferably 1 / 9 to 9 / 1, more preferably 2 / 8 to 8 / 2, further preferably 3 / 7 to 7 / 3, and particularly preferably 3 / 7 to 5 / 5, from the viewpoint of better effect of the present invention.

[0282] In the coating of the present invention, the total content of the specific microcapsules and the color developer is preferably 50% by mass or more relative to the total solid content of the coating solution. The upper limit is not particularly limited, but is preferably 99.5% by mass or less.

[0283] 〔Resin〕

[0284] The coating liquid of the present invention contains a resin, which functions as a resin binder that supports specific microcapsules and a color developer.

[0285] As the above-mentioned resin, in addition to the resin that can be added when preparing the coating liquid of the present invention, there are resins that are brought into the coating liquid from the raw material components, such as emulsifiers such as polyvinyl alcohol used in the preparation of specific microcapsule dispersions and dispersants such as polyvinyl alcohol used in the preparation of colorant dispersions.

[0286] The type of resin is not particularly limited, and examples thereof include synthetic polymers and natural polymers such as styrene-butadiene copolymers, polyvinyl acetate, polyacrylates, polyvinyl alcohol, polyacrylic acid, maleic anhydride-styrene copolymers, olefin resins, modified acrylate copolymers, starch, casein, gum arabic, gelatin, carboxymethyl cellulose or its salts, and methyl cellulose.

[0287] In the coating liquid of the present invention, the content of the resin is 17% by mass or less relative to the total solid content of the coating liquid, and preferably 13% by mass or less from the viewpoint of the more excellent effect of the present invention. The lower limit of the content of the resin is not particularly limited, but is preferably 0.5% by mass or more, and more preferably 1% by mass or more.

[0288] The weight average molecular weight of the resin is not particularly limited, but is preferably 1,000 to 1,000,000.

[0289] 〔Solvent〕

[0290] The coating liquid of the present invention contains a solvent.

[0291] In addition, the "solvent" mentioned here refers to the solvent existing outside the microcapsule (in other words, not contained in the microcapsule). That is, the coating liquid of the present invention contains specific microcapsules and may also contain other microcapsules other than the specific microcapsules, but the "solvent" mentioned here refers to the solvent existing outside the microcapsule without being contained in any microcapsule.

[0292] The solvent is not particularly limited as long as it can disperse the microcapsules and dissolve or disperse the developer.

[0293] Among them, a solvent that does not swell the capsule wall of the specific microcapsule and does not cause the capsule content (core material) to seep out or release from the capsule is preferred, and a solvent having no aromatic group is more preferred.

[0294] Specifically, the solvent that can be used includes water (pure water, distilled water, ion-exchanged water, etc. can be used, and distilled water is preferred from the viewpoint of stability over time), ketone solvents such as methyl ethyl ketone, and ester solvents such as ethyl acetate.

[0295] In the coating liquid of the present invention, the content of the solvent is preferably 10 to 90% by mass, more preferably 20 to 80% by mass, and even more preferably 20 to 70% by mass, based on the total mass of the coating liquid.

[0296] And, when the coating liquid of the present invention includes water, the content of water is preferably 50 mass % or more, more preferably 70 mass % or more, relative to the gross mass of the solvent. In addition, as the upper limit value, it is not particularly limited, but preferably 100 mass % or less, more preferably 99.5 mass % or less, and further preferably 98 mass % or less.

[0297] [Other ingredients]

[0298] The coating liquid of the present invention may contain other components in addition to the above-mentioned components.

[0299] The other components are not particularly limited, and examples thereof include thickeners, pigments, surfactants, fluorescent whitening agents, defoaming agents, penetrants, ultraviolet absorbers, pH adjusters, and preservatives.

[0300] And, when the coating liquid of the present invention includes a surfactant, the content of the surfactant is preferably 10% by mass or less, more preferably 5% by mass or less, and further preferably 3% by mass or less relative to the total solid content of the coating liquid. In addition, the lower limit is not particularly limited, for example, 0.5% by mass or more.

[0301] As the surfactant, a low-molecular surfactant is preferred.

[0302] Furthermore, from the viewpoint of better coating properties in the non-planar portion and / or better applicability to spraying, the coating solution of the present invention preferably does not substantially contain inorganic particles other than the developer (e.g., pigments such as talc or titanium dioxide, silica particles, heavy calcium carbonate, and light calcium carbonate). "Substantially containing no inorganic particles other than the developer" means that the content of inorganic particles other than the developer is 3% by mass or less, preferably 1% by mass or less, more preferably 0.5% by mass or less, and further preferably 0% by mass relative to the total solid content of the coating solution.

[0303] [Method for producing coating liquid]

[0304] The method for producing the coating solution of the present invention is not particularly limited, but the coating solution is preferably produced by mixing a microcapsule dispersion containing specific microcapsules, a dispersion containing a developer, and optional components added as needed.

[0305] The coating liquid of the present invention must contain a resin. The resin may be contained in the microcapsule dispersion and / or the dispersion containing the developer, or may be further added when the microcapsule dispersion and the dispersion containing the developer are mixed.

[0306] Furthermore, the coating solution of the present invention must contain a solvent. The solvent may be a solvent contained in the microcapsule dispersion and the dispersion containing the developer, or may be further added when the microcapsule dispersion and the dispersion containing the developer are mixed.

[0307] The upper limit of the viscosity of the coating liquid of the present invention at 25°C is not particularly limited, but from the viewpoint of ensuring coating properties, it is preferably 100,000 mPa·s or less, and from the viewpoint of more excellent effects of the present invention, it is more preferably less than 5,000 mPa·s, further preferably 3,000 mPa·s or less, particularly preferably 2,000 mPa·s or less, and most preferably 1,000 mPa·s or less. And, as its lower limit, it is preferably 0.1 mPa·s or more, more preferably 0.5 mPa·s or more, and further preferably 1 mPa·s or more.

[0308] In this specification, "viscosity" means a value measured by an E-type viscometer at 25° C. As the E-type viscometer, for example, VISCOSITY METER TVB-10H (manufactured by TOKI SANGYO CO., LTD.) or the like can be used.

[0309] The viscosity of the coating liquid of the present invention can be adjusted according to the type and content of each component contained in the coating liquid of the present invention, for example.

[0310] The coating solution of the present invention preferably contains substantially no coarse particles from the viewpoint of better coating properties in non-planar portions and / or better applicability to spray coating. As a form of such a coating solution, a form in which the volume-based median particle size (D50) of the microcapsules contained in the coating solution is 1 to 50 μm and the color developer is an organic compound (as the organic compound, a metal salt of an aromatic carboxylic acid is preferred, a metal salicylate derivative is more preferred, and a zinc salicylate derivative is further preferred).

[0311] [Application of the coating liquid of the present invention]

[0312] By using the coating solution of the present invention, it is possible to measure the pressure or pressure distribution in the non-planar portion of an article having the non-planar portion.

[0313] Hereinafter, a method for measuring pressure using the coating liquid of the present invention will be described.

[0314] The pressure measurement method using the coating liquid of the present invention preferably includes the following steps: a step of applying the coating liquid of the present invention on the measurement surface of the measurement object as the measurement object of pressure or pressure distribution to form a coating film (pressure measurement layer); and a step of applying pressure to the obtained pressure measurement layer (pressure measurement step).

[0315] When pressure is applied to the pressure measuring layer, the specific microcapsules are broken, and the coloring agent contained in the specific microcapsules leaks out of the specific microcapsules, and undergoes a coloring reaction with the coloring agent. As a result, coloring occurs in the pressurized area.

[0316] As described above, the coating solution of the present invention can also be applied to a measurement object having a surface shape other than a flat surface.

[0317] The shape of the measurement surface in the measurement object is not particularly limited, and examples thereof include a flat surface, a curved surface, and a concave-convex surface. The measurement surface for pressure measurement may be a part of the surface of the measurement object or the entire surface.

[0318] The object to be measured preferably includes non-planar portions such as a curved surface and an uneven surface, and more preferably a part or all of the measurement surface includes non-planar portions.

[0319] The coating method of the coating liquid of the present invention is not particularly limited, and examples thereof include roll coating, spray coating, brush coating, and dip coating.

[0320] When applying the coating liquid of the present invention, the coating liquid of the present invention can be directly applied to the measurement surface of the measurement object, or an intervening object (for example, a film or paper) is arranged on the measurement surface of the measurement object and the coating liquid of the present invention is applied to the above-mentioned intervening object.

[0321] The coating amount of the coating liquid of the present invention can be set according to the purpose of measurement, but is preferably 2 to 40 g / m2 in terms of solid content from the viewpoint of obtaining good color development and color distribution. 2 , more preferably 2 to 30 g / m 2 , and more preferably 2 to 20 g / m 2 , especially preferably set to 2 to 15 g / m 2 .

[0322] Furthermore, the coating liquid of the present invention may be dried by heat treatment after being applied to the measurement surface of the measurement object. The drying temperature is not particularly limited, and is preferably 40 to 120° C., for example. The drying time is not particularly limited, and is preferably 5 to 600 seconds, for example.

[0323] When pressure is applied to the pressure measuring layer, the pressure may be any of point pressure, linear pressure, and surface pressure.

[0324] The pressure range that can be measured by the pressure measuring layer is not particularly limited, but is preferably 300 MPa or less, and more preferably 0.1 to 300 MPa, for example.

[0325] The pressure measuring layer exhibits a property that the color density increases with increasing pressure (in other words, color gradation) when a pressure of 300 MPa or less is applied. The color gradation of the pressure measuring layer is preferably a property that the color density increases with increasing pressure.

[0326] The pressure range measurable by the pressure measuring layer can be appropriately set according to the measurement purpose. The measurable pressure range can be adjusted by, for example, controlling the particle diameter, wall thickness and constituent materials of the specific microcapsules and the coating amount of the coating solution of the present invention.

[0327] The color development property (color development density) and gradation property of the color development portion generated in the pressurized region of the pressure measuring layer can be measured using a reflection densitometer (for example, RD-19I manufactured by GretagMacbeth).

[0328] The object to be measured is not particularly limited as long as it is an object having a shape that enables measurement of pressure or pressure distribution. Specifically, various molding dies including press dies, vacuum molding dies, and injection molding dies can be cited.

[0329] The use of the coating liquid of the present invention is not particularly limited, and examples thereof include confirmation of pressure distribution in the molding processing of various components, bodies, etc. and the assembly processing of components in the manufacture of vehicles such as automobiles and aircraft; confirmation of pressure distribution in the assembly processing of building materials; confirmation of pressure distribution in the process of curved surface processing of electronic products (such as bonding of curved displays); confirmation of impact force applied to goods during transportation; confirmation of mold contact in the manufacture of metal products; confirmation of mold contact during the molding processing of resin products; confirmation of pressure distribution in the tableting of pharmaceutical tablets; confirmation of pressure distribution on the surface of furniture such as the seats of chairs and sofas; confirmation of the close contact force applied to writing tools, etc.; confirmation of pressure on stationery such as; confirmation of impact force applied to sports equipment such as balls made of elastic materials; confirmation of the gap (space) between upper and lower teeth in dental products, etc.

[0330] Furthermore, the pressure measurement using the coating liquid of the present invention is also suitable for applications such as checking mold contact in metal processing and checking pressure distribution when bonding curved displays.

[0331] [Articles with non-planar parts and pressure measuring layer]

[0332] The invention also relates to an article comprising a non-planar portion and having a pressure-determining layer.

[0333] The non-planar portion-containing article with a pressure measuring layer of the present invention comprises an article including a non-planar portion and a pressure measuring layer formed using a coating solution A and disposed on the non-planar portion.

[0334] The article with a pressure measuring layer having a non-planar portion of the present invention can be obtained by the pressure measuring method using the coating liquid (coating liquid A) of the present invention. That is, the article with a pressure measuring layer having a non-planar portion of the present invention corresponds to a laminated body obtained by forming a pressure measuring layer on the non-planar portion of the article as a measurement object having a non-planar portion such as a curved surface and a concave-convex surface on a part or the whole of the measurement surface in the pressure measuring method using the coating liquid (coating liquid A) of the present invention.

[0335] In addition, as the measurement object, there can be mentioned an article having a shape that enables measurement of pressure or pressure distribution, and specific examples of the article are as described above.

[0336] exist Figure 3 and Figure 4 A specific example of an article having a non-planar portion and having a pressure measuring layer is shown in FIG.

[0337] Figure 3The illustrated article 31 having a non-planar portion with a pressure measuring layer includes an article 30 having a non-planar portion and a pressure measuring layer 33 disposed on the non-planar portion of the article 30 having a non-planar portion. The pressure measuring layer 33 includes specific microcapsules 34, a color developer 35, and a film 32 formed of a resin binder that holds and supports the specific microcapsules 34 and the color developer 35 on the article 30 having a non-planar portion. In the pressure measuring layer 33, a region of the specific microcapsules 34 completely protrudes from the film 32. In the pressure measuring layer 33, the particle size D31 of the specific microcapsules 34 is larger than the thickness D32 of the film 32.

[0338] Figure 4 The illustrated article 41 with a pressure measuring layer having a non-planar portion includes an article 40 having a non-planar portion and a pressure measuring layer 43 disposed on the non-planar portion of the article 40 having a non-planar portion. The pressure measuring layer 43 includes specific microcapsules 44, a color developer 45, a film 42 formed of a resin binder that holds and supports the specific microcapsules 44 and the color developer 45 on the article 40 having a non-planar portion, and a coating 46 formed of the same resin binder as the film 42. In the pressure measuring layer 43, a region of the specific microcapsules 44 protrudes from the film 42, and the surface (a region of the surface or the entire region of the surface) of the region of the specific microcapsules 44 protruding from the film 42 is covered with the coating 46 which is a thin film of the resin binder. In the pressure measuring layer 43, the particle size D41 of the specific microcapsules 44 is larger than the thickness D42 of the film 42.

[0339] [Method for producing pressure measuring layer]

[0340] The invention also relates to a method for producing a pressure measuring layer.

[0341] The method for producing a pressure measuring layer of the present invention comprises the step of applying a coating liquid for forming a pressure measuring layer (hereinafter also referred to as "coating liquid" or "coating liquid B") to the non-planar portion of an article including the non-planar portion to form the pressure measuring layer, wherein:

[0342] The pressure measuring layer forming coating liquid comprises: microcapsules containing a coloring agent and an aromatic solvent (hereinafter also referred to as "specific microcapsules"), a coloring agent not contained in the microcapsules (hereinafter also referred to as "coloring agent"), a resin and a solvent.

[0343] The average particle size of the specific microcapsules is X μm, and the solid content coating amount of the pressure measurement layer forming coating liquid is Y g / m 2 When Y / X is used, the solid content coating amount is Yg / m 2 The ratio to the average particle size X μm is less than 1.

[0344] When pressure is applied to the pressure measuring layer formed by the method for producing a pressure measuring layer of the present invention, the specific microcapsules are destroyed and the coloring agent contained in the specific microcapsules leaks out of the specific microcapsules and reacts with the coloring agent to develop color. As a result, color is developed in the pressurized area.

[0345] The method for manufacturing a pressure measuring layer of the present invention having the above-mentioned structure can be applied to the measurement of pressure or pressure distribution in a non-planar portion of an article having a non-planar portion. Furthermore, the pressure measuring layer obtained by the method for manufacturing a pressure measuring layer of the present invention has excellent gradation of the color developing portion even when pressurized in a low pressure range (for example, 300 MPa or less).

[0346] Although the mechanism of action of the above-mentioned configuration and effect is not clear, the present inventors speculate as follows.

[0347] The main features of the method for producing a pressure measuring layer of the present invention are as follows: the above-mentioned coating liquid for forming a pressure measuring layer (coating liquid B) is used, the average particle size of the specific microcapsules is set to X μm, and the solid content coating amount of the coating liquid B is set to Y g / m 2 When the solid content coating amount is expressed by Y / X, it is Yg / m 2 The pressure measuring layer is formed on the non-planar portion of the article including the non-planar portion in a manner that the ratio to the average particle size X μm is less than 1. The coating liquid B further contains a resin together with the specific microcapsules and the developer. It is believed that the resin acts as a resin binder that supports the specific microcapsules and the developer in the pressure measuring layer formed by the coating liquid B.

[0348] The present inventors have found that by setting the average particle size of the specific microcapsules to X μm and the solid content coating amount of the coating liquid B to Y g / m 2 When Y / X is less than 1, the pressure measuring layer is formed, and the obtained pressure measuring layer has a structure in which the specific microcapsules are not buried in the resin binder (specifically, it becomes as described above). Figure 1 and Figure 2 It is presumed that the specific microcapsules in such a pressure measuring layer are easily destroyed when pressurized, and as a result, even when pressurized at a pressure in a low pressure range (for example, 300 MPa or less), good color development (color development concentration) and gradation properties can be easily obtained.

[0349] Furthermore, as described above, the method for producing a pressure measuring layer of the present invention can be applied to the measurement of pressure or pressure distribution in a non-planar portion of an object having a non-planar portion. That is, even for a measurement object that is difficult to measure in the form of a conventional film or sheet, the pressure measuring layer can be formed at a coating amount per unit area generally used in pressure measurement without being affected by the surface shape.

[0350] Hereinafter, the fact that the pressure measuring layer formed by the method for producing a pressure measuring layer of the present invention is more excellent in one or more selected from the group consisting of color density, gradation, and image quality is also referred to as “the effect of the present invention is more excellent”.

[0351] [Coating liquid for forming pressure measuring layer (coating liquid B)]

[0352] The pressure measuring layer forming coating liquid (coating liquid B) used in the method for producing the pressure measuring layer of the present invention contains microcapsules (specific microcapsules) containing a color former and an aromatic solvent, a color developer (developer) not contained in the microcapsules, a resin and a solvent.

[0353] The coating liquid B used in the method for producing a pressure measuring layer of the present invention is the same as the coating liquid for forming a pressure measuring layer of the present invention (coating liquid A) except for the content of the resin, and the preferred aspects are also the same.

[0354] In the coating liquid used in the method for producing the pressure measuring layer of the present invention, the content of the resin is preferably 30% by mass or less relative to the total solid content, and is preferably 17% by mass or less, and more preferably 13% by mass or less, from the viewpoint that the specific microcapsules in the formed pressure measuring layer further protrude from the film and the effect of the present invention is more excellent. The lower limit of the content of the resin is not particularly limited, but is preferably 1% by mass or more, and more preferably 3% by mass or more.

[0355] In the method for manufacturing a pressure measuring layer of the present invention, the object to be measured is an object to be measured having a surface shape other than a plane. Specifically, there can be mentioned objects to be measured having a measuring surface such as a curved surface and a concave-convex surface. The measuring surface for pressure measurement can be a part of the surface of the object to be measured or the entire surface.

[0356] In the method for producing the pressure measuring layer of the present invention, the coating method of the coating liquid B is not particularly limited, and examples thereof include roll coating, spray coating, brush coating, and dip coating.

[0357] When applying the coating liquid B, the coating liquid B may be directly applied to the measurement surface of the measurement object, or an intervening object (e.g., a film or paper) may be disposed on the measurement surface of the measurement object and the coating liquid B may be applied to the intervening object.

[0358] The coating amount of the coating liquid B is set to be X μm, where the average particle size of the specific microcapsules is X μm, and the solid content coating amount of the coating liquid B is Y g / m 2 When Y / X is used, the solid content coating amount is Yg / m 2The ratio of the average particle size X μm (hereinafter abbreviated as "Y / X") is less than 1. That is, when the average particle size of the specific microcapsules is 3 μm, the solid content coating amount is less than 3 g / m 2 When the coating amount of the coating liquid B and the average particle size of the specific microcapsules satisfy the above relationship, a microcapsule can be formed as follows: Figure 1 and Figure 2 The pressure measuring layers of the structure are shown.

[0359] In order to achieve a better effect of the present invention, the average particle size (X) of the specific microcapsules is preferably 1 to 100 μm and Y / X is 0.8 or less, and the average particle size (X) of the specific microcapsules is more preferably 3 to 50 μm and Y / X is 0.6 or less. In addition, Y / X is preferably 0.1 or more in order to achieve a better color concentration of the color development portion generated in the pressurized region of the pressure measuring layer.

[0360] After the coating liquid B is applied to the measurement surface of the measurement object, it can be dried by heat treatment. The drying temperature is not particularly limited, and is preferably 40 to 120° C., for example. The drying time is not particularly limited, and is preferably 5 to 600 seconds, for example.

[0361] When pressure is applied to the pressure measuring layer, the pressure may be any of point pressure, linear pressure, and surface pressure.

[0362] The pressure range that can be measured by the pressure measuring layer is not particularly limited, but is, for example, preferably 300 MPa or less, more preferably 100 MPa or less, and more preferably 1 to 100 MPa.

[0363] The pressure measuring layer exhibits a property that the color density increases with increasing pressure (in other words, color gradation) when a pressure of 300 MPa or less is applied. The color gradation of the pressure measuring layer is preferably a property that the color density increases with increasing pressure.

[0364] The measurable pressure range can be appropriately set according to the measurement purpose. The measurable pressure range can be adjusted by, for example, controlling the particle diameter, wall thickness, and constituent materials of the specific microcapsules and the coating amount of the coating solution B.

[0365] The color development property (color development density) and gradation property of the color development portion generated in the pressurized region of the pressure measuring layer can be measured using a reflection densitometer (for example, RD-19I manufactured by GretagMacbeth).

[0366] The object to be measured is not particularly limited as long as it has a non-planar portion in at least one region of the measurement surface. Specifically, various molding dies including stamping dies, vacuum molding dies, and injection molding dies can be cited.

[0367] The use to which the method for producing a pressure measuring layer of the present invention can be applied is not particularly limited, and the various uses exemplified as the applicable uses of the coating liquid A described above can be cited.

[0368] Furthermore, the method for producing a pressure measuring layer according to the present invention is also suitable for applications such as checking mold contact in metal processing and checking pressure distribution during bonding of curved displays.

[0369] [Articles with non-planar parts and pressure measuring layer]

[0370] The invention also relates to an article comprising a non-planar portion and having a pressure-determining layer.

[0371] The article with a pressure measuring layer having a non-planar portion of the present invention is a laminate formed by the above-mentioned method for manufacturing a pressure measuring layer of the present invention. That is, the laminate formed by forming a pressure measuring layer on the above-mentioned non-planar portion of an article as a measurement object having a non-planar portion such as a curved surface and a concave-convex surface on a part or all of the measurement surface corresponds to this. As the article with a pressure measuring layer having a non-planar portion, specifically, the above-mentioned Figure 3 The article 31 having a non-planar portion and a pressure measuring layer is shown Figure 4 An article 41 having a non-planar portion and a pressure-measuring layer is shown.

[0372] Example

[0373] Below, the present invention is further described in detail according to the examples. The materials, usage, ratio, processing content and processing steps shown in the following examples can be appropriately changed as long as they do not depart from the purpose of the present invention. Therefore, the scope of the present invention should not be interpreted restrictively by the examples shown below. In addition, as long as there is no special specification below, "part" and "%" are mass references.

[0374] [Example 1]

[0375] [Preparation of microcapsule dispersion 1 containing a coloring agent]

[0376] In 50 parts of a mixture of 1,2-dimethyl-4-(1-phenylethyl)benzene, 1,3-dimethyl-4-(1-phenylethyl)benzene, 1,4-dimethyl-2-(1-phenylethyl)benzene and 1-(ethylphenyl)-1-phenylethane (SRS-101 manufactured by Yantai Jinzheng Fine Chemical Co., Ltd.), 3 parts of 3',6'-bis(diethylamino)-2-(4-nitrophenyl)spiro[isoindol-1,9'-xanthene]-3-one (Pink-DCF manufactured by HODOGAY A CHEMICAL CO., LTD.), 4 parts of 6'-(diethylamino)-1',3'-dimethylfluoran (Orange-DCF manufactured by HODOGAYA CHEMICAL CO., LTD.) and 2-(2'-hydroxy-5'-methylphenyl)benzotriazole (JOHOKU CHEMICAL CO., LTD.) as a UV absorber were dissolved. CO., LTD, JF-77-P) 3 parts to obtain solution A.

[0377] Next, 13 parts of synthetic isoparaffin (IP Solvent 1620 manufactured by Idemitsu Kosan Co., Ltd.) and 0.3 parts of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine (ADEKA Polyether EDP-300 manufactured by ADEKA Corporation) dissolved in 2.5 parts of methyl ethyl ketone were added to the stirred solution A to obtain a solution B. Furthermore, 2.5 parts of a trimethylolpropane adduct of toluene diisocyanate (BURNOCK D-750 manufactured by DIC Corporation, solid content 75% by mass, ethyl acetate solution) dissolved in 6 parts of ethyl acetate were added to the stirred solution B to obtain a solution C. Then, the above solution C was added to a solution prepared by dissolving 7 parts of polyvinyl alcohol (PVA-217E manufactured by KURARAY CO., LTD.) in 140 parts of water to emulsify and disperse the solution. 200 parts of water was added to the emulsified liquid, and the mixture was heated to 70°C with stirring, stirred for 1 hour, and then cooled. Furthermore, water was added to adjust the concentration to obtain a microcapsule dispersion containing a coloring agent having a solid content concentration of 20%.

[0378] The average particle size of the obtained microcapsules containing the coloring agent is 20 μm. The average particle size and particle size distribution are measured by laser scattering method using Microtrac MT3300EXII (Nikkiso Co., Ltd.), the average particle size is measured by the value of D50, and the particle size distribution is measured by the CV value (in addition, the average particle size and particle size distribution are both volume basis). Relative to the total solid content of the microcapsule dispersion, the content of the resin binder is 8.5% by mass, and the content of the microcapsules is 91.5% by mass. The contents of the resin binder and the microcapsules are separated by centrifugation.

[0379] [Preparation of developer dispersion 1]

[0380] 100 parts of activated clay (MIZUSAWA INDUSTRIAL CHEMICALS, LTD., Shilton F-242) as a developer, 0.5 parts of sodium hexametaphosphate (NIHON KAGAKU SANGYO CO., LTD., sodium hexametaphosphate), 15 parts of a 10% sodium hydroxide aqueous solution and 240 parts of water were added to obtain a dispersion containing a developer.

[0381] The microcapsule dispersion 1 containing a color former and the developer dispersion 1 are mixed to prepare a pressure measuring layer forming coating liquid 1. In the mixed pressure measuring layer forming coating liquid 1, the microcapsule dispersion 1 containing a color former and the developer dispersion 1 are each mixed at a ratio of 50 mass %.

[0382] 〔evaluate〕

[0383] <Pressure Measurement Layer Preparation>

[0384] The coating liquid 1 for forming a pressure measuring layer was sprayed onto a metal plate (concave mirror / convex mirror (R=100 mm) made of stainless steel (SUS304)) as a coated object in a coating amount described in Table 1. The same metal plate was placed from above the coated surface so as to cover the coated area, and pressurization was performed for 120 seconds at three-point pressures of 1 MPa, 5 MPa, and 10 MPa using a press machine (product name: H1F35-1, manufactured by Komatsu Ltd.).

[0385] After the pressing was completed, the metal plate placed above the coated surface was removed, the color development and color distribution of the coated area were visually confirmed, and sensory evaluation was performed according to the following evaluation criteria.

[0386] <Color Evaluation (Concentration)>

[0387] The color development state after applying pressure at 5 MPa was visually confirmed and evaluated according to the following evaluation criteria.

[0388] "A": Color is developed at a sufficient density to be visually recognized.

[0389] "B": The color development density is slightly low, but the color is developed to a level that is not a problem in practical use.

[0390] "C": no color development.

[0391] <Gradualness>

[0392] "AA": A 3-point difference can be clearly visually identified.

[0393] "A": Ability to visually recognize 3 points of difference.

[0394] "B": The difference between 1 MPa and 5 MPa or the difference between 5 MPa and 10 MPa can be visually recognized.

[0395] "C": Although the difference between 1 MPa and 5 MPa and the difference between 5 MPa and 10 MPa cannot be visually recognized, the difference between 1 MPa and 10 MPa can be visually recognized.

[0396] "D": No difference can be visually discerned.

[0397] <Color granularity (image quality)>

[0398] The color development surface state of the metal plate after the pressing was visually observed and evaluated according to the following evaluation criteria.

[0399] "A": The graininess in the color development portion is very small.

[0400] "B": The color part has a slight grainy feel, but it is not a problem in practical use.

[0401] "C": The graininess in the color development part is noticeably large.

[0402] <Spreadability Evaluation>

[0403] The coated metal plates were visually observed and evaluated according to the following evaluation criteria.

[0404] "A": Uneven application (thickness) cannot be visually recognized.

[0405] "B": Uneven application (thickness) can be visually recognized.

[0406] [Example 2]

[0407] A pressure measuring layer-forming coating liquid 2 was prepared by the same method as in Example 1, except that the developer dispersion liquid 1 was changed to the developer dispersion liquid 2, and the same evaluation as in Example 1 was performed.

[0408] <Developer Dispersion Liquid 2>

[0409] A dispersion was prepared by dispersing 35 parts of 3,5-di-α-methylbenzyl salicylic acid zinc (substituted salicylic acid metal salt, developer), 7 parts of sodium hexametaphosphate and 50 parts of water into an average particle diameter of 2 μm using a sand mill. A developer dispersion was prepared by adding 10 parts of a 10% aqueous solution of polyvinyl alcohol (PVA-203, manufactured by KURARAY CO., LTD.). The developer content was 98% by mass relative to the total solid content of the developer dispersion. The binder and developer content were determined by separation by centrifugation. Centrifugation was performed multiple times as needed.

[0410] [Examples 3 to 14, 16 to 22 (color developer type: zinc salicylate)]

[0411] As shown in Table 1, the pressure measuring layer forming coating liquids of Examples 3 to 14 and 16 to 22 (color developer type: zinc salicylate) were prepared in the same procedure as Example 2 except that various conditions such as the materials and the content of the materials were changed. In addition, in Examples 19 to 21, a resin binder dispersion was used in addition to the microcapsule dispersion and the color developer dispersion. In Example 22, a part of the water in the pressure measuring layer forming coating liquid was removed by heating to make it a high viscosity solution.

[0412] The same evaluation as in Example 1 was carried out using the obtained coating liquid for forming a pressure measuring layer.

[0413] [Example 15 and Comparative Example 1 (Type of developer: activated clay)]

[0414] As shown in Table 1, pressure measuring layer-forming coating solutions of Example 15 and Comparative Example 1 (developer type: activated clay) were prepared in the same manner as in Example 1 except that various conditions such as the materials and the contents of the materials were changed.

[0415] The same evaluation as in Example 1 was carried out using the obtained coating liquid for forming a pressure measuring layer.

[0416] [Reference Example 1 (Type of developer: activated clay)]

[0417] As shown in Table 1, a pressure measuring layer-forming coating liquid of Reference Example 1 (type of developer: activated clay) was prepared in the same procedure as in Example 1 except that various conditions such as the materials and the contents of the materials were changed.

[0418] The same evaluation as in Example 1 was carried out using the obtained coating liquid for forming a pressure measuring layer.

[0419] [Example 23]

[0420] A coating liquid for forming a pressure measuring layer was prepared in the same manner as in Example 1 except that the developer dispersion liquid 1 was changed to LR-220 (solid content concentration: 43%) manufactured by SANKO Inc.

[0421] In addition, in the pressure measuring layer forming coating liquid prepared in Example 23, the content of the resin was 17% by mass or less based on the total solid content of the pressure measuring layer forming coating liquid.

[0422] The same evaluation as in Example 1 was carried out using the obtained pressure measuring layer-forming coating liquid. As a result, the results were all A for "color development (density)", "gradation", "color development granularity (image quality)", and "spreadability".

[0423] [Comparative Example 2]

[0424] The double-sheet pressure measuring sheet set consisting of an electron-donating colorless dye sheet and a developer sheet disclosed in Example 1 of Japanese Patent Gazette No. 2009-019949 was used to perform pressure measurement on the concave and convex surface of the metal plate used in the above-mentioned [Example 1]. As a result, the thin sheet did not follow the concave and convex surface and measurement could not be performed.

[0425] Table 1 is shown below.

[0426] The various components shown in Table 1 are as follows.

[0427] <Microcapsule composition>

[0428] (Coloring Agent)

[0429] Orange-DCF: 6'-(diethylamino)-1',3'-dimethylfluoran, manufactured by HODOGAYA CHEM ICAL CO., LTD.

[0430] Pink-DCF: 3',6'-bis(diethylamino)-2-(4-nitrophenyl)spiro[isoindol-1,9'-xanthene]-3-one, manufactured by HODOGAYA CHEMICAL CO., LTD.

[0431] Coloring agent A: 3,3-bis(2-methyl-1-octyl-3-indolyl)phthalide

[0432] Colorant B: RED40, manufactured by Yamamoto Chemicals Inc.

[0433] (Aromatic solvents)

[0434] SAS-296: 1,1-Diphenylethane, manufactured by JXTG Energy

[0435] SRS-101: A mixture of 1,2-dimethyl-4-(1-phenylethyl)benzene, 1,3-dimethyl-4-(1-phenylethyl)benzene, 1,4-dimethyl-2-(1-phenylethyl)benzene and 1-(ethylphenyl)-1-phenylethane (manufactured by Yantai Jinzheng Fine Chemical Co., Ltd.)

[0436] Alkeno L: Linear alkylbenzene, manufactured by JXTG Energy

[0437] (Emulsifier (resin binder))

[0438] PVA (polyvinyl alcohol): PVA-217E, manufactured by KURARAY C0., LTD.

[0439] <Developer Dispersion Liquid>

[0440] (Developer)

[0441] Activated clay: Shilton F-242, manufactured by MIZUSAWA INDUSTRIAL CHEMICALS, LTD.

[0442] Zinc salicylate: 3,5-bis(α-methylbenzyl) zinc salicylate, solid content 43% aqueous dispersion, manufactured by SANKO Inc.

[0443] (Dispersant (resin binder))

[0444] PVA (polyvinyl alcohol): PVA-203, manufactured by KURARAY C0., LTD.

[0445] <Resin Binder (Dispersion Liquid)>

[0446] (resin adhesive)

[0447] NPL: modified acrylic ester copolymer (product name: Nipol LX814, manufactured by Zeon Corporation, solid content 47% by mass aqueous dispersion)

[0448] In the table, the values ​​in the column "Average particle size and particle size distribution of microcapsules" are the values ​​obtained by measuring the average particle size and particle size distribution of microcapsules in the microcapsule dispersion using Microtrac MT3300EXII (manufactured by Nikkiso Co., Ltd.) by laser scattering method. The average particle size was measured by the D50 value, and the particle size distribution was measured by the cV value (in addition, the average particle size and particle size distribution are both volume-based).

[0449] In addition, "viscosity" is a value measured at a temperature of 25°C using an E-type viscometer (VISCOSITY METER TVB-10H (manufactured by TOKISANGYO CO., LTD.)).

[0450] In addition, in the table, each resin of PVA (polyvinyl alcohol) recorded in the "Emulsifier (Resin Binder)" column, PVA (polyvinyl alcohol) recorded in the "Dispersant (Resin Binder)" column, and NPL (modified acrylate copolymer) recorded in the "Resin Binder (Dispersion Liquid)" column corresponds to the "resin" in the coating solution of the present invention.

[0451] In the table, "Pink-DCF" corresponds to the compound represented by the general formula (1), and the color former A corresponds to the compound having an indole structural part.

[0452] In the table, in each column of "Microcapsule dispersion", "Developer dispersion", and "Resin binder (dispersion)", "Mixing ratio (solution)" refers to the mixing ratio of the above-mentioned dispersions.

[0453] In addition, in the table, in the column "Total content of microcapsules and color developers relative to the total solid content of the coating liquid for forming the pressure measuring layer [mass %]", "P" indicates that the total content of microcapsules and color developers is 50 mass % or more relative to the total solid content of the coating liquid for forming the pressure measuring layer, and "N" indicates that the total content of microcapsules and color developers is less than 50 mass % relative to the total solid content of the coating liquid for forming the pressure measuring layer.

[0454] In the table, the "Y / X" column represents the ratio of the solid content coating amount Yg / m2 of the coating liquid to the average particle size Xμm of the microcapsules, "P" represents the case where the value of Y / X is less than 1, and "N" represents the case where the value of Y / X is greater than 1.

[0455] [Table 1]

[0456]

[0457] As shown in Table 1, it was confirmed that the desired effect can be obtained when the coating liquid for forming a pressure measuring layer of the present invention is used. In addition, it was confirmed that the desired effect can be obtained when the method for using the coating liquid for forming a pressure measuring layer of the present invention is used.

[0458] Furthermore, from the comparison between Examples 1 to 7 and Example 8, it was confirmed that when the particle size distribution of the microcapsules was 15% or more (preferably 30% or more), the gradation of the color development part was more excellent.

[0459] Furthermore, from the comparison between Example 2 and Examples 9 to 14, it was confirmed that when the average particle size of the microcapsules was 10 μm or more, the color development and gradation of the color development part were more excellent. In addition, it was confirmed that when the average particle size of the microcapsules was less than 100 μm, the image quality of the color development part was more excellent.

[0460] Furthermore, from the comparison between Example 2 and Example 18, it was confirmed that when the coloring agent contained in the microcapsule includes the compound represented by the above-mentioned general formula (1), the coloring property and gradation property of the coloring part are more excellent.

[0461] Furthermore, from the comparison of Examples 19 to 21, it was confirmed that when the content of the resin binder relative to the total solid content of the pressure measuring layer-forming coating liquid was 13 mass % or less, the color development property and gradation property of the color development portion were more excellent.

[0462] Furthermore, from the comparison between Example 2 and Example 22, it was confirmed that when the viscosity (25° C.) of the pressure measuring layer-forming coating liquid was less than 5000 mPa·s, the coating property was more excellent.

[0463] The pressure measuring layer forming coating liquid of the comparative example did not provide the expected effect. Also, the pressure measuring layer forming coating liquid of the comparative example did not provide the expected effect in the method of using the pressure measuring layer forming coating liquid of the comparative example.

[0464] Explanation of symbols

[0465] 10-measurement object (coated object), 12, 32, 42-film, 14, 34, 44-specific microcapsule, 15, 46-film, 35, 45-color developer, 30, 40-article containing non-planar portion, 31, 41-object containing non-planar portion with pressure measuring layer, 33, 43-pressure measuring layer, D1-particle size of specific microcapsule, D2-thickness of film 12, D31-particle size of specific microcapsule 34, D32-thickness of film 32, D41-particle size of specific microcapsule 44, D42-thickness of film 42.

Claims

1. A coating liquid for forming a pressure measuring layer, comprising: Microcapsules containing colorants and aromatic solvents; Color developing agent not contained in microcapsules; Resins; and Solvents, The content of the resin is 17% by mass or less based on the total solid content of the pressure measuring layer forming coating liquid, The coloring agent is selected from triarylmethanephthalide compounds, fluorane compounds, phenothiazine compounds, indolylphthalide compounds, colorless gold amine compounds, rhodamine lactam compounds, triarylmethane compounds, diphenylmethane compounds, triazene compounds, spiropyran compounds, fluorene compounds, pyridine compounds, pyrazine compounds, The aromatic solvent is a compound having at least one aromatic ring and no aromatic condensed ring. The developer is selected from activated clay, acid clay, attapulgite, zeolite, bentonite, kaolin, phenolic compounds, zinc salicylate derivatives, and hydroxybenzoic acid esters. The average particle size of the microcapsules contained in the pressure measuring layer forming coating liquid is 1 μm or more and 100 μm or less, The particle size distribution of the microcapsules contained in the pressure measuring layer forming coating liquid is 10% or more and 40% or less, The content of the microcapsules is 20% to 50% by mass relative to the total solid content of the pressure measuring layer forming coating liquid, the content of the color developer is 50% to 80% by mass relative to the total solid content of the pressure measuring layer forming coating liquid, and the total content of the microcapsules and the color developer is 50% to 99.5% by mass relative to the total solid content of the pressure measuring layer forming coating liquid. The pressure range that can be measured using the pressure measuring layer obtained from the pressure measuring layer-forming coating liquid is 1 to 10 MPa.

2. The coating liquid for forming a pressure measuring layer according to claim 1, wherein The content of the resin is 13% by mass or less based on the total solid content of the pressure measuring layer forming coating liquid. 3 . The coating liquid for forming a pressure measuring layer according to claim 1 , which has a viscosity at 25° C. of less than 5000 mPa·s.

4. The coating liquid for forming a pressure measuring layer according to claim 1 or 2, wherein The microcapsules containing the color former and the aromatic solvent contain substantially no color developer.

5. The coating liquid for forming a pressure measuring layer according to claim 1 or 2, wherein The average particle diameter of the microcapsules contained in the pressure measuring layer-forming coating liquid is 5 μm or more and 100 μm or less.

6. The coating liquid for forming a pressure measuring layer according to claim 1 or 2, wherein The developer comprises a material selected from activated clay, acid clay and zinc salicylate derivatives.

7. The coating liquid for forming a pressure measuring layer according to claim 6, wherein The developer is 3,5-bis(α-methylbenzyl) zinc salicylate.

8. The coating liquid for forming a pressure measuring layer according to claim 1 or 2, wherein The particle size distribution of the microcapsules contained in the pressure measuring layer-forming coating liquid is 15% or more and 40% or less.

9. The coating liquid for forming a pressure measuring layer according to claim 1 or 2, wherein The coloring agent is selected from the compounds represented by the general formula (1) and compounds having an indole structure, In the formula, R 1 and R 3 each independently represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent, R 2 and R 4 Each independently represents an alkyl group which may have a substituent or an aryl group which may have a substituent, X 1 Indicates -O- or -NR 5 -, R 5 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.

10. A method for producing a pressure measuring layer, comprising the step of applying a coating liquid for forming a pressure measuring layer to a non-planar portion of an article including the non-planar portion to form the pressure measuring layer, wherein: The pressure measuring layer forming coating liquid comprises: microcapsules containing a color former and an aromatic solvent; a color former not contained in the microcapsules; a resin; and a solvent. The coloring agent is selected from triarylmethanephthalide compounds, fluorane compounds, phenothiazine compounds, indolylphthalide compounds, colorless gold amine compounds, rhodamine lactam compounds, triarylmethane compounds, diphenylmethane compounds, triazene compounds, spiropyran compounds, fluorene compounds, pyridine compounds, pyrazine compounds, The aromatic solvent is a compound having at least one aromatic ring and no aromatic condensed ring. The developer is selected from activated clay, acid clay, attapulgite, zeolite, bentonite, kaolin, phenolic compounds, zinc salicylate derivatives, and hydroxybenzoic acid esters. The average particle size of the microcapsules contained in the pressure measuring layer forming coating liquid is 1 μm or more and 100 μm or less, The particle size distribution of the microcapsules contained in the pressure measuring layer forming coating liquid is 10% or more and 40% or less, The content of the microcapsules is 20% to 50% by mass relative to the total solid content of the pressure measuring layer forming coating liquid, the content of the color developer is 50% to 80% by mass relative to the total solid content of the pressure measuring layer forming coating liquid, and the total content of the microcapsules and the color developer is 50% to 99.5% by mass relative to the total solid content of the pressure measuring layer forming coating liquid. The average particle size of the microcapsules containing the color former and the aromatic solvent is X μm, and the solid content coating amount of the pressure measuring layer forming coating liquid is Y g / m 2 When Y / X is used, the solid content coating amount is Yg / m 2 The ratio to the average particle size X μm is 0.8 or less.

11. The method for manufacturing a pressure measuring layer according to claim 10, wherein: The content of the resin is 17% by mass or less based on the total solid content of the pressure measuring layer forming coating liquid.

12. The method for producing a pressure measuring layer according to claim 10 or 11, wherein: The content of the resin is 13% by mass or less based on the total solid content of the pressure measuring layer forming coating liquid.

13. The method for producing a pressure measuring layer according to claim 10 or 11, wherein: The pressure measuring layer-forming coating liquid has a viscosity at 25° C. of less than 5000 mPa·s.

14. The method for producing a pressure measuring layer according to claim 10 or 11, wherein: The microcapsules containing the color former and the aromatic solvent contain substantially no color developer.

15. The method for producing a pressure measuring layer according to claim 10 or 11, wherein: The average particle diameter of the microcapsules contained in the pressure measuring layer-forming coating liquid is 5 μm or more and 100 μm or less.

16. The method for producing a pressure measuring layer according to claim 10 or 11, wherein: The developer comprises a material selected from activated clay, acid clay and zinc salicylate derivatives.

17. The method for producing a pressure measuring layer according to claim 10 or 11, wherein: The developer is 3,5-bis(α-methylbenzyl) zinc salicylate.

18. The method for producing a pressure measuring layer according to claim 10 or 11, wherein: The particle size distribution of the microcapsules contained in the pressure measuring layer-forming coating liquid is 15% or more and 40% or less.

19. The method for producing a pressure measuring layer according to claim 10 or 11, wherein: The coloring agent is selected from the compounds represented by the general formula (1) and compounds having an indole structure, In the formula, R 1 and R 3 each independently represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent, R 2 and R 4 Each independently represents an alkyl group which may have a substituent or an aryl group which may have a substituent, X 1 Indicates -O- or -NR 5 -, R 5 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.

20. An article having a non-planar portion and a pressure-measuring layer, comprising: an article comprising a non-planar portion; and A pressure measuring layer is disposed on the non-planar portion and is formed using the pressure measuring layer forming coating liquid according to any one of claims 1 to 9.

21. An article having a non-planar portion and having a pressure-sensing layer, wherein the pressure-sensing layer is obtained by the method for producing a pressure-sensing layer according to any one of claims 10 to 19.

Citation Information

Patent Citations

  • Photosensitive-thermosensitive recording material

    JP1993257272A

  • Pressure-sensitive coloring resin material, pressure-sensitive member, and buffer material

    JP2007132756A

  • Stimuli-responsive composite particles and manufacturing method for same

    WO2018199044A1

  • Pressure measurement material

    CN110720031A

  • Microcapsule for pressure-sensitive recording material, its manufacturing method and pressure-sensitive recording material using it

    JP2007237696A