Preparation of a hollow nanocage electrocatalyst and its application in electrocatalytic oxygen evolution reaction

By introducing Fe into Co LDH hollow nanocages and selenizing them, Fe-CoSe2 hollow nanocages are formed, which solves the problems of poor conductivity and poor stability of layered double hydroxides in the oxygen evolution reaction, and improves the catalytic activity and Stable and suitable for industrial applications in electrocatalytic oxygen evolution reactions.

CN115976537BInactive Publication Date: 2024-10-15JILIN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211429267.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-11-15
Publication Date
2024-10-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing layered double hydroxides have problems such as poor conductivity, low catalytic activity, and poor stability in oxygen evolution reactions, which limits the improvement of their electrocatalytic performance in electrolyzing water.

Method used

By introducing Fe as a transition metal source into Co LDH hollow nanocages, Fe-Co LDH hollow nanocages are formed, and Fe-CoSe2 hollow nanocages are obtained through selenization treatment, which increases the coordination between the specific surface area and electronic structure and improves catalytic activity. and stability.

Benefits of technology

The catalytic activity and stability of the catalyst are significantly improved, the performance of the electrocatalytic oxygen evolution reaction is enhanced, and it is suitable for industrial catalytic applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN115976537B_ABST
    Figure CN115976537B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of preparation of electrode materials for lithium-ion batteries, and specifically relates to the preparation of a hollow nanocage electrocatalyst and its application in electrocatalytic oxygen evolution reaction. The present invention synthesizes Fe‑Co LDH hollow nanocages through the co-action of multiple components, and can further obtain Fe‑CoSe2 on this basis through selenization treatment, both of which are suitable for electrocatalytic oxygen evolution reaction. In terms of catalytic activity, a large number of defects are generated in the Co LDH hollow nanocages due to the doping of transition metal sources. This new structure has obvious catalytic advantages in both morphology and electronic structure: first, the hollow nanocage increases the specific surface area and accelerates the mass transfer process; second, the transition metal source has a coordinating effect on the electronic structure of the Co atom, which reduces the adsorption barrier of the catalyst material to the reaction intermediates during the OER process, improves the intrinsic activity of the catalyst, and enhances the catalytic activity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of catalysts, and particularly relates to the preparation of a hollow nanocage electrocatalyst and its application in an electrocatalytic oxygen evolution reaction. Background Art

[0002] With the development of society, people's demand for energy is growing. The over-exploitation and use of fossil fuels has led to a series of energy and environmental problems. It is urgent to develop green, clean and renewable energy. Compared with traditional fossil energy, hydrogen has ultra-high energy density and zero carbon dioxide emissions, and has been considered the most ideal clean energy. In the large-scale production of high-purity hydrogen, water electrolysis is the most feasible method. There are two half reactions involved in water electrolysis, namely the oxygen evolution reaction (OER) on the anode and the hydrogen evolution reaction (HER) on the cathode. OER is a four-electron process with slow reaction kinetics, so the kinetics of OER need to be improved.

[0003] At present, noble metals Ru and Ir have the best performance in OER electrocatalysts. However, the high cost and low stability of noble metals limit their application in the field of catalysis. Therefore, the development of cheap, highly active and highly stable OER catalysts is the key to improving the performance of water electrolysis. Two-dimensional transition metal materials have high catalytic activity and stability in the field of electrocatalysis and have a wide range of applications. The application of two-dimensional transition metal materials in the field of catalysis can be divided into three aspects: the first is the large surface area; the second is the excellent thermal conductivity; the third is the mechanical properties. Through the unremitting efforts of scientific researchers, a variety of two-dimensional nanomaterials have been developed, including transition metal layered double hydroxides, phosphides, sulfides, nitrides, carbides and selenides.

[0004] Among them, transition metal layered double hydroxides are applied to water electrolysis due to their unique electronic structure and large specific surface area. Among the hydroxides that have been reported, NiFe LDH, CoNi LDH, etc. all show good catalytic activity in oxygen evolution reaction. In order to further improve the performance of transition metal layered double hydroxides in OER, various methods such as doping and heterogeneous structures have been proposed to promote the catalytic process.

[0005] At present, layered double hydroxides have certain shortcomings in oxygen evolution reaction, such as poor conductivity, low catalytic activity and poor stability. Summary of the invention

[0006] The purpose of the present invention is to overcome the above-mentioned problems existing in the traditional technology, provide a preparation method of a hollow nanocage electrocatalyst and its application in the electrocatalytic oxygen evolution reaction, and greatly improve the performance of Co LDH in the electrocatalytic oxygen evolution reaction through the synergistic effect between metals from the aspects of the morphology and intrinsic activity of the catalyst, so as to promote the application of Co LDH series materials in industrial catalysis.

[0007] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0008] The invention provides a hollow nanocage electrocatalyst, which is composed of two-dimensional nanosheets. The electrocatalyst uses Fe as a transition metal source, and introduces the transition metal source into a Co LDH hollow nanocage to replace the position of Co, thereby obtaining a Fe-Co LDH hollow nanocage.

[0009] The present invention also provides a hollow nanocage electrocatalyst, which is composed of a combination of two-dimensional nanosheets. The electrocatalyst uses Fe as a transition metal source, and introduces a transition metal source into a Co LDH hollow nanocage to replace the position of Co, thereby obtaining a Fe-Co LDH hollow nanocage; the Fe-Co LDH hollow nanocage is then subjected to high-temperature calcination reaction with selenium powder, and a Fe-CoSe2 hollow nanocage with a hollow porous structure is obtained after selenization.

[0010] Furthermore, in the hollow nanocage electrocatalyst, the content of the transition metal source is 5-15%.

[0011] Furthermore, in the above hollow nanocage electrocatalyst, the wall thickness of the hollow nanocage electrocatalyst is 600-800 nm.

[0012] The present invention provides a method for preparing a hollow nanocage electrocatalyst, comprising the following steps:

[0013] 1) Synthesis of ZIF-67

[0014] Dissolve Co(NO3)2·6H2O and 2-MeIM in appropriate amount of methanol respectively, stir evenly, then quickly add 2-MeIM solution into Co(NO3)2·6H2O solution, mix evenly to obtain a purple solution; stir at room temperature for a period of time to obtain a purple product, collect the product by centrifugation; and dry to obtain ZIF-67;

[0015] 2) Synthesis of Co LDH hollow nanocages

[0016] Co(NO3)2·6H2O and ZIF-67 were dissolved in ethanol according to the ratio, and then stirred after ultrasonic homogenization; then refluxed at 90°C for a period of time, and the product was collected by centrifugation to obtain Co LDH hollow nanocages;

[0017] 3) Synthesis of Fe-Co LDH hollow nanocages

[0018] The Co LDH hollow nanocages and the transition metal source Fe are dissolved in deionized water, and then stirred after ultrasonic homogenization; then the mixture is allowed to stand for a period of time at room temperature, and the product is collected by centrifugation to obtain the Fe-Co LDH hollow nanocages.

[0019] The present invention also provides a method for preparing a hollow nanocage electrocatalyst, comprising the following steps:

[0020] 1) Synthesis of ZIF-67

[0021] Dissolve Co(NO3)2·6H2O and 2-MeIM in appropriate amount of methanol respectively, stir evenly, then quickly add 2-MeIM solution into Co(NO3)2·6H2O solution, mix evenly to obtain a purple solution; stir at room temperature for a period of time to obtain a purple product, collect the product by centrifugation; and dry to obtain ZIF-67;

[0022] 2) Synthesis of Co LDH hollow nanocages

[0023] Co(NO3)2·6H2O and ZIF-67 were dissolved in ethanol according to the ratio, and then stirred after ultrasonic homogenization; then refluxed at 90°C for a period of time, and the product was collected by centrifugation to obtain Co LDH hollow nanocages;

[0024] 3) Synthesis of Fe-Co LDH hollow nanocages

[0025] The Co LDH hollow nanocage and the transition metal source Fe are dissolved in deionized water, and then stirred after ultrasonic homogenization; then the mixture is allowed to stand at room temperature for a period of time, and the product is collected by centrifugation to obtain the Fe-Co LDH hollow nanocage;

[0026] 4) Synthesis of Fe-CoSe2 hollow nanocages

[0027] The Fe-Co LDH hollow nanocage and selenium powder were placed in the downstream and upstream of the tube furnace respectively, and the temperature was raised to 380-420°C at 1-3°C / min under argon protection, and kept warm for 1-3h; the product was collected to obtain Fe-CoSe2 hollow nanocage.

[0028] Further, in the preparation method as described above, in step 1), the molar ratio of Co(NO3)2·6H2O and 2-MeIM is 1:4;

[0029] In step 2), the mass ratio of Co(NO3)2·6H2O and ZIF-67 is 8:2-4;

[0030] In step 3), the mass ratio of Co LDH hollow nanocages to transition metal source Fe is 20:3.

[0031] Furthermore, in the preparation method as described above, in step 4), the selenium powder is sufficient.

[0032] Furthermore, in the preparation method as described above, in step 4), the temperature is raised to 400° C. at 2° C. / min under argon protection and kept at this temperature for 2 h.

[0033] The present invention also provides an application of a hollow nano cage electrocatalyst in an electrocatalytic oxygen evolution reaction.

[0034] The beneficial effects of the present invention are:

[0035] The present invention synthesizes Fe-Co LDH hollow nanocages through the co-action of multiple components, and can further obtain Fe-CoSe2 on this basis through selenization treatment, both of which are suitable for electrocatalytic oxygen evolution reaction. In terms of catalytic activity, a large number of defects are generated in the Co LDH hollow nanocages due to the doping of transition metal sources. This new structure has obvious catalytic advantages in both morphology and electronic structure: first, the hollow nanocage increases the specific surface area and accelerates the mass transfer process; second, the transition metal source has a coordinating effect on the electronic structure of Co atoms, so that the catalyst material reduces the adsorption barrier of the reaction intermediates during the OER process, improves the intrinsic activity of the catalyst, and enhances the catalytic activity. This synthesis method is of great significance to the synthesis of selenides and the research of catalysts.

[0036] Of course, any product implementing the present invention does not necessarily need to achieve all of the above advantages at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0038] Figure 1 It is the X-ray diffraction spectra of Fe-CoSe2 prepared by the present invention (Example 2) and the comparative example CoSe2 (Comparative Example 2);

[0039] Figure 2 is a morphology diagram of the Fe-CoSe2 material prepared by the present invention;

[0040] in, Figure 2 a is a scanning electron microscope image, Figure 2 b is a transmission electron microscopy image, and Figures cf are EDS images;

[0041] Figure 3 It is a performance comparison diagram of the Fe-Co LDH (Example 1) catalyst prepared by the present invention and the Co LDH (Comparative Example 1) catalyst;

[0042] Figure 4 It is a performance comparison diagram of the Fe-CoSe2 (Example 2) catalyst prepared by the present invention and the Fe-Co LDH (Example 1) catalyst;

[0043] Figure 5 It is a Tafel diagram comparing the Fe-Co LDH (Example 1) catalyst prepared by the present invention with the Co LDH (Comparative Example 1) and the Fe-CoSe2 (Example 2) catalyst;

[0044] Figure 6 is the LSV diagram of different Fe addition amounts of the Fe-Co LDH material prepared by the present invention;

[0045] Figure 7 is the CV diagram of the Fe-CoSe2 (Example 2) catalyst prepared by the present invention;

[0046] Figure 8 It is the LSV diagram of different Fe addition amounts in Fe-CoSe2 prepared by the present invention. DETAILED DESCRIPTION

[0047] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0048] The specific embodiments of the present invention are as follows:

[0049] Example 1

[0050] 1) Synthesis of ZIF-67: Dissolve 0.249 g (1 mmol) Co(NO3)2·6H2O and 0.328 g (4 mmol) 2-MeIM in 25 mL methanol, stir evenly, then quickly add 2-MeIM solution to Co(NO3)2·6H2O solution, mix evenly to obtain a purple solution; stir at room temperature for 24 h to obtain a purple product, collect the product by centrifugation; dry to obtain ZIF-67;

[0051] 2) Synthesis of Co LDH hollow nanocages: 800 mg Co(NO3)2·6H2O and 320 mg ZIF-67 were dissolved in 200 mL ethanol, homogenized by ultrasound and stirred for 15 min; then refluxed at 90 °C for 3 h in a round-bottom flask with a stirring rate of 900 r; the product was collected by centrifugation and washed three times with ethanol.

[0052] 3) Synthesis of Fe-Co LDH hollow nanocages: 40 mg Co LDH and 6 mg FeCl2·4H2O were dissolved in 40 mL deionized water, and stirred for 30 min after ultrasonic homogenization. The product was collected by centrifugation after standing at room temperature for 3 h.

[0053] The size of the obtained catalyst material is 600-800nm, and the Fe content is about 15wt%. The successful synthesis of the structure of "hollow nanocages composed of Fe-Co LDH nanosheets" can be observed by scanning electron microscopy and transmission electron microscopy. The catalytic activity exhibited by this defect-rich structure in the electrocatalytic process far exceeds that of the comparison material Co LDH nanosheets and other embodiment materials without obvious defects.

[0054] Example 2

[0055] 1) Synthesis of ZIF-67: Dissolve 0.249 g (1 mmol) Co(NO3)2·6H2O and 0.328 g (4 mmol) 2-MeIM in 25 mL methanol, stir evenly, then quickly add 2-MeIM solution to Co(NO3)2·6H2O solution, mix evenly to obtain a purple solution; stir at room temperature for 24 h to obtain a purple product, collect the product by centrifugation; dry to obtain ZIF-67;

[0056] 2) Synthesis of Co LDH hollow nanocages: 800 mg Co(NO3)2·6H2O and 320 mg ZIF-67 were dissolved in 200 mL ethanol, homogenized by ultrasound and stirred for 15 min; then refluxed at 90 °C for 3 h in a round-bottom flask with a stirring rate of 900 r; the product was collected by centrifugation and washed three times with ethanol.

[0057] 3) Synthesis of Fe-Co LDH hollow nanocages: 40 mg Co LDH and 6 mg FeCl2·4H2O were dissolved in 40 mL deionized water, and stirred for 30 min after ultrasonic homogenization. The product was collected by centrifugation after standing at room temperature for 3 h.

[0058] 4) Synthesis of Fe-CoSe2 hollow nanocages: Fe-Co LDH and selenium powder were placed in the downstream and upstream of a tube furnace, respectively. The temperature was raised to 400°C at 2°C / min under argon protection and kept at this temperature for 2 h. A black product was obtained and collected.

[0059] The catalyst prepared in this example was used as the anode and 1M KOH was used as the electrolyte to test the electrocatalytic oxygen evolution reaction. 2 At a current density of 1.3 Å, the overpotential is 302 mV. The results show that the material also has high electrocatalytic oxygen evolution activity and stability.

[0060] Example 3

[0061] 1) Synthesis of ZIF-67: Dissolve 0.249 g (1 mmol) Co(NO3)2·6H2O and 0.328 g (4 mmol) 2-MeIM in 25 mL methanol, stir evenly, then quickly add 2-MeIM solution to Co(NO3)2·6H2O solution, mix evenly to obtain a purple solution; stir at room temperature for 24 h to obtain a purple product, collect the product by centrifugation; dry to obtain ZIF-67;

[0062] 2) Synthesis of Co LDH hollow nanocages: 800 mg Co(NO3)2·6H2O and 320 mg ZIF-67 were dissolved in 200 mL ethanol, homogenized by ultrasound and stirred for 15 min; then refluxed at 90 °C for 3 h in a round-bottom flask with a stirring rate of 900 r; the product was collected by centrifugation and washed three times with ethanol.

[0063] 3) Synthesis of Fe-Co LDH hollow nanocages: 40 mg Co LDH and 2 mg FeCl2·4H2O were dissolved in 40 mL deionized water, and stirred for 30 min after ultrasonic homogenization. The product was collected by centrifugation after standing at room temperature for 3 h.

[0064] The catalyst prepared in this example was used as the anode and 1M KOH was used as the electrolyte to test the electrocatalytic oxygen evolution reaction. 2 At a current density of 1.3 Å, the overpotential is 326 mV. The results show that the material also has high electrocatalytic oxygen evolution activity and stability.

[0065] Example 4

[0066] 1) Synthesis of ZIF-67: Dissolve 0.249 g (1 mmol) Co(NO3)2·6H2O and 0.328 g (4 mmol) 2-MeIM in 25 mL methanol, stir evenly, then quickly add 2-MeIM solution to Co(NO3)2·6H2O solution, mix evenly to obtain a purple solution; stir at room temperature for 24 h to obtain a purple product, collect the product by centrifugation; dry to obtain ZIF-67;

[0067] 2) Synthesis of Co LDH hollow nanocages: 800 mg Co(NO3)2·6H2O and 320 mg ZIF-67 were dissolved in 200 mL ethanol, homogenized by ultrasound and stirred for 15 min; then refluxed at 90 °C for 3 h in a round-bottom flask with a stirring rate of 900 r; the product was collected by centrifugation and washed three times with ethanol.

[0068] 3) Synthesis of Fe-Co LDH hollow nanocages: 40 mg Co LDH and 4 mg FeCl2·4H2O were dissolved in 40 mL deionized water, and stirred for 30 min after ultrasonic homogenization. The product was collected by centrifugation after standing at room temperature for 3 h.

[0069] The catalyst prepared in this example was used as the anode and 1M KOH was used as the electrolyte to test the electrocatalytic oxygen evolution reaction. 2 At a current density of 1.3 Å, the overpotential is 336 mV. The results show that the material also has high electrocatalytic oxygen evolution activity and stability.

[0070] Example 5

[0071] 1) Synthesis of ZIF-67: Dissolve 0.249 g (1 mmol) Co(NO3)2·6H2O and 0.328 g (4 mmol) 2-MeIM in 25 mL methanol, stir evenly, then quickly add 2-MeIM solution to Co(NO3)2·6H2O solution, mix evenly to obtain a purple solution; stir at room temperature for 24 h to obtain a purple product, collect the product by centrifugation; dry to obtain ZIF-67;

[0072] 2) Synthesis of Co LDH hollow nanocages: 800 mg Co(NO3)2·6H2O and 320 mg ZIF-67 were dissolved in 200 mL ethanol, homogenized by ultrasound and stirred for 15 min; then refluxed at 90 °C for 3 h in a round-bottom flask with a stirring rate of 900 r; the product was collected by centrifugation and washed three times with ethanol.

[0073] 3) Synthesis of Fe-Co LDH hollow nanocages: 40 mg Co LDH and 12 mg FeCl2·4H2O were dissolved in 40 mL deionized water, and stirred for 30 min after ultrasonic homogenization. The product was collected by centrifugation after standing at room temperature for 3 h.

[0074] The catalyst prepared in this example was used as the anode and 1M KOH was used as the electrolyte to test the electrocatalytic oxygen evolution reaction. 2 The overpotential is 313 mV at a current density of 1.3 %. The results show that the material also has high electrocatalytic oxygen evolution activity and stability.

[0075] Example 6

[0076] 1) Synthesis of ZIF-67: Dissolve 0.249 g (1 mmol) Co(NO3)2·6H2O and 0.328 g (4 mmol) 2-MeIM in 25 mL methanol, stir evenly, then quickly add 2-MeIM solution to Co(NO3)2·6H2O solution, mix evenly to obtain a purple solution; stir at room temperature for 24 h to obtain a purple product, collect the product by centrifugation; dry to obtain ZIF-67;

[0077] 2) Synthesis of Co LDH hollow nanocages: 800 mg Co(NO3)2·6H2O and 320 mg ZIF-67 were dissolved in 200 mL ethanol, homogenized by ultrasound and stirred for 15 min; then refluxed at 90 °C for 3 h in a round-bottom flask with a stirring rate of 900 r; the product was collected by centrifugation and washed three times with ethanol.

[0078] 3) Synthesis of Fe-Co LDH hollow nanocages: 40 mg Co LDH and 2 mg FeCl2·4H2O were dissolved in 40 mL deionized water, and stirred for 30 min after ultrasonic homogenization. The product was collected by centrifugation after standing at room temperature for 3 h.

[0079] 4) Synthesis of Fe-CoSe2 hollow nanocages: Fe-Co LDH and selenium powder were placed in the downstream and upstream of a tube furnace, respectively. The temperature was raised to 400°C at 2°C / min under argon protection and kept at this temperature for 2 h. A black product was obtained and collected.

[0080] The catalyst prepared in this example was used as the anode and 1M KOH was used as the electrolyte to test the electrocatalytic oxygen evolution reaction. 2 The overpotential is 318 mV at a current density of 1.3 %. The results show that the material also has high electrocatalytic oxygen evolution activity and stability.

[0081] Example 7

[0082] 1) Synthesis of ZIF-67: Dissolve 0.249 g (1 mmol) Co(NO3)2·6H2O and 0.328 g (4 mmol) 2-MeIM in 25 mL methanol, stir evenly, then quickly add 2-MeIM solution to Co(NO3)2·6H2O solution, mix evenly to obtain a purple solution; stir at room temperature for 24 h to obtain a purple product, collect the product by centrifugation; dry to obtain ZIF-67;

[0083] 2) Synthesis of Co LDH hollow nanocages: 800 mg Co(NO3)2·6H2O and 320 mg ZIF-67 were dissolved in 200 mL ethanol, homogenized by ultrasound and stirred for 15 min; then refluxed at 90 °C for 3 h in a round-bottom flask with a stirring rate of 900 r; the product was collected by centrifugation and washed three times with ethanol.

[0084] 3) Synthesis of Fe-Co LDH hollow nanocages: 40 mg Co LDH and 4 mg FeCl2·4H2O were dissolved in 40 mL deionized water, and stirred for 30 min after ultrasonic homogenization. The product was collected by centrifugation after standing at room temperature for 3 h.

[0085] 4) Synthesis of Fe-CoSe2 hollow nanocages: Fe-Co LDH and selenium powder were placed in the downstream and upstream of a tube furnace, respectively. The temperature was raised to 400°C at 2°C / min under argon protection and kept at this temperature for 2 h. A black product was obtained and collected.

[0086] The catalyst prepared in this example was used as the anode and 1M KOH was used as the electrolyte to test the electrocatalytic oxygen evolution reaction. 2 The overpotential is 323mV at a current density of 1.38kV. The results show that the material also has high electrocatalytic oxygen evolution activity and stability.

[0087] Comparative Example 1

[0088] 1) Synthesis of ZIF-67: Dissolve 0.249 g (1 mmol) Co(NO3)2·6H2O and 0.328 g (4 mmol) 2-MeIM in 25 mL methanol, stir evenly, then quickly add 2-MeIM solution to Co(NO3)2·6H2O solution, mix evenly to obtain a purple solution; stir at room temperature for 24 h to obtain a purple product, collect the product by centrifugation; dry to obtain ZIF-67;

[0089] 2) Synthesis of Co LDH hollow nanocages: 800 mg Co(NO3)2·6H2O and 320 mg ZIF-67 were dissolved in 200 mL ethanol, homogenized by ultrasound and stirred for 15 min; then refluxed at 90 °C for 3 h in a round-bottom flask with a stirring rate of 900 r; the product was collected by centrifugation and washed three times with ethanol.

[0090] The catalyst prepared in this comparative example was used as the anode, and 1M KOH was used as the electrolyte to test the electrocatalytic oxygen evolution reaction. 2 At a current density of , the overpotential is 376 mV.

[0091] Comparative Example 2

[0092] 1) Synthesis of ZIF-67: Dissolve 0.249 g (1 mmol) Co(NO3)2·6H2O and 0.328 g (4 mmol) 2-MeIM in 25 mL methanol, stir evenly, then quickly add 2-MeIM solution to Co(NO3)2·6H2O solution, mix evenly to obtain a purple solution; stir at room temperature for 24 h to obtain a purple product, collect the product by centrifugation; dry to obtain ZIF-67;

[0093] 2) Synthesis of Co LDH hollow nanocages: 800 mg Co(NO3)2·6H2O and 320 mg ZIF-67 were dissolved in 200 mL ethanol, homogenized by ultrasound and stirred for 15 min; then refluxed at 90 °C for 3 h in a round-bottom flask with a stirring rate of 900 r; the product was collected by centrifugation and washed three times with ethanol.

[0094] 4) Synthesis of CoSe2 hollow nanocages: Co LDH and selenium powder were placed in the downstream and upstream of a tube furnace, respectively. The temperature was raised to 400°C at 2°C / min under argon protection and kept at this temperature for 2 h. A black product was obtained and collected.

[0095] The catalyst prepared in this comparative example was used as the anode, and 1M KOH was used as the electrolyte to test the electrocatalytic oxygen evolution reaction. 2 At a current density of , the overpotential is 331 mV.

[0096] Comparing Examples 1-7 and Comparative Examples 1-2, the results are as follows:

[0097] Figure 1 The X-ray diffraction spectra of Fe-CoSe2 (Example 2) prepared by the present invention and the comparative example CoSe2 (Comparative Example 2) are shown in Figure 1. It can be seen that the characteristic peaks of CoSe2 in the standard XRD spectrum are consistent, indicating that Fe-CoSe2 has been successfully synthesized, wherein the diffraction peak is the cubic phase of CoSe2.

[0098] Figure 2 is a morphology diagram of the Fe-CoSe2 material prepared by the present invention, Figure 2 a, Figure 2 Figures b and b are scanning electron microscope images and transmission electron microscope images of Fe-CoSe2 nanosheets prepared by the present invention, respectively, which can be clearly seen as hollow nanocages. Figures cf are EDS images of the present invention, which can clearly show that Fe, Co and Se elements are evenly distributed.

[0099] Figure 3 The Fe-Co LDH (Example 1) catalyst prepared by the present invention and the Co LDH (Comparative Example 1) catalyst were subjected to a current density of 10 mA·cm in 1M KOH. -2The overpotentials are 314 mV and 376 mV respectively. The performance of Fe-Co LDH (Example 1) is significantly better than that of other materials.

[0100] Figure 4 The Fe-CoSe2 (Example 2) catalyst prepared by the present invention and the Fe-Co LDH (Example 1) catalyst in 1M KOH have a current density of 10 mA·cm -2 The overpotentials are 302 mV and 314 mV respectively. The performance of Fe-Co LDH (Example 1) is significantly better than that of other materials.

[0101] Figure 5 The Tafel diagram of the Fe-Co LDH (Example 1) catalyst prepared by the present invention is compared with the Co LDH (Comparative Example 1) and Fe-CoSe2 (Example 2) catalysts. The charge transfer rate of the catalyst is obtained through the Tafel diagram. The smaller the tafel slope of the catalyst, the faster the electron transfer rate. It can be seen from the figure that the tafel slopes of Co LDH, Fe-Co LDH (Example 1) and Fe-CoSe2 (Example 2) are 123.84 mV·dec, respectively. -2 、83.45mV·dec -2 and 81.91mV·dec -2 , Fe-CoSe2 (Example 2) obviously has a larger charge transfer rate, which is conducive to the conversion of more reaction intermediates into oxygen on the catalyst surface.

[0102] Figure 6 The LSV diagrams of the Fe-Co LDH materials prepared by the present invention with different Fe addition amounts are shown in Figure 1. The Fe addition amounts are 5% (Example 3), 10% (Example 4), 15% (Example 1), and 30% (Example 5). The LSV diagrams show that the Fe-Co LDH materials with different Fe addition amounts have a current density of 10 mA cm -2 The overpotentials are 326 mV, 336 mV, 314 mV and 313 mV respectively, all of which have very high electrocatalytic activity, among which Example 1 has the highest catalytic activity.

[0103] Figure 7 The CV diagram of the Fe-CoSe2 (Example 2) catalyst prepared by the present invention is shown in Figure 1. The electrochemical active area of ​​the catalyst is obtained through the CV diagram. The larger the active area of ​​the catalyst, the higher the catalytic activity. The Cd1 is obtained by collecting cyclic voltammetry curves at different scan rates and linear fitting. It can be seen from the figure that the Cd1 values ​​of Co LDH, Fe-Co LDH (Example 1) and Fe-CoSe2 (Example 2) are 33.48 mF·cm -2 、71.63mF·cm -2 and 40.31mF·cm-2 , Fe-Co LDH (Example 1) obviously has a larger active area and more active sites, which is conducive to the conversion of more reaction intermediates into oxygen on the catalyst surface.

[0104] Figure 8 The LSV diagrams of different Fe addition amounts in Fe-CoSe2 prepared by the present invention are 5% (Example 6), 10% (Example 7), and 15% (Example 2) of Fe doping. It can be seen from the LSV diagram that at a current density of 10 mA cm -2 The overpotentials are 318 mV, 323 mV, and 302 mV, respectively, all of which have very high electrocatalytic activity, among which Example 1 has the highest catalytic activity.

[0105] The preferred embodiments of the present invention disclosed above are only used to help explain the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to specific implementation methods. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A method for preparing a hollow nanocage electrocatalyst, characterized in that: The hollow nanocage electrocatalyst is composed of two-dimensional nanosheets. The electrocatalyst uses Fe as a transition metal source, and the transition metal source is introduced into the Co LDH hollow nanocage to replace the position of Co, thereby obtaining a Fe-Co LDH hollow nanocage. The preparation method of the hollow nanocage electrocatalyst comprises the following steps: 1) Synthesis of ZIF-67 Dissolve Co(NO3)2·6H2O and 2-MeIM in appropriate amount of methanol respectively, stir evenly, then quickly add 2-MeIM solution into Co(NO3)2·6H2O solution, mix evenly to obtain a purple solution; stir at room temperature for a period of time to obtain a purple product, collect the product by centrifugation; and dry to obtain ZIF-67; 2) Synthesis of Co LDH hollow nanocages Co(NO3)2·6H2O and ZIF-67 were dissolved in ethanol according to the ratio, and then stirred after ultrasonic homogenization; then refluxed at 90°C for a period of time, and the product was collected by centrifugation to obtain Co LDH hollow nanocages; 3) Synthesis of Fe-Co LDH hollow nanocages The Co LDH hollow nanocages and the transition metal source Fe are dissolved in deionized water, and then stirred after ultrasonic homogenization; then the mixture is allowed to stand for a period of time at room temperature, and the product is collected by centrifugation to obtain the Fe-Co LDH hollow nanocages.

2. The preparation method according to claim 1, characterized in that: The electrocatalyst is composed of a combination of two-dimensional nanosheets. The electrocatalyst uses Fe as a transition metal source. The transition metal source is introduced into a Co LDH hollow nanocage to replace the position of Co, thereby obtaining a Fe-Co LDH hollow nanocage. The Fe-Co LDH hollow nanocage is then subjected to high-temperature calcination reaction with selenium powder, and a Fe-CoSe2 hollow nanocage with a hollow porous structure is obtained after selenization.

3. The preparation method according to claim 1 or 2, characterized in that: The content of the transition metal source in the hollow nanocage electrocatalyst is 5-15wt%.

4. The preparation method according to claim 1 or 2, characterized in that: The wall thickness of the hollow nanocage electrocatalyst is 600-800 nm.

5. The preparation method according to claim 2, characterized in that: The steps include: 1) Synthesis of ZIF-67 Dissolve Co(NO3)2·6H2O and 2-MeIM in appropriate amount of methanol respectively, stir evenly, then quickly add 2-MeIM solution into Co(NO3)2·6H2O solution, mix evenly to obtain a purple solution; stir at room temperature for a period of time to obtain a purple product, collect the product by centrifugation; and dry to obtain ZIF-67; 2) Synthesis of Co LDH hollow nanocages Co(NO3)2·6H2O and ZIF-67 were dissolved in ethanol according to the ratio, and then stirred after ultrasonic homogenization; then refluxed at 90°C for a period of time, and the product was collected by centrifugation to obtain Co LDH hollow nanocages; 3) Synthesis of Fe-Co LDH hollow nanocages The Co LDH hollow nanocage and the transition metal source Fe are dissolved in deionized water, and then stirred after ultrasonic homogenization; then the mixture is allowed to stand at room temperature for a period of time, and the product is collected by centrifugation to obtain the Fe-Co LDH hollow nanocage; 4) Synthesis of Fe-CoSe2 hollow nanocages The Fe-Co LDH hollow nanocage and selenium powder were placed in the downstream and upstream of the tube furnace, respectively, and heated to 380-420°C at 1-3°C / min under argon protection, and kept warm for 1-3h; The products were collected to obtain Fe-CoSe2 hollow nanocages.

6. The preparation method according to claim 1 or 5, characterized in that: In step 1), the molar ratio of Co(NO3)2·6H2O and 2-MeIM is 1:4; In step 2), the mass ratio of Co(NO3)2·6H2O and ZIF-67 is 8:2-4; In step 3), the mass ratio of Co LDH hollow nanocages to transition metal source Fe is 20:

3.

7. The preparation method according to claim 5, characterized in that: In step 4), the selenium powder is sufficient.

8. The preparation method according to claim 5, characterized in that: In step 4), the temperature was raised to 400°C at 2°C / min under argon protection and kept at this temperature for 2h.