Adhesive composition, photocurable adhesive layer, and photocurable adhesive sheet
Patent Information
- Application Number
- CN202180053034.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-05-11
- Filing Date
- 2021-08-24
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2041-08-24
AI Technical Summary
[0006]另一方面,显示高流动性的粘合剂虽然高度差吸收性优异,但存在形状稳定性、操作性等加工性降低的问题
[0043] The adhesive composition, photocurable adhesive layer, and photocurable adhesive sheet of the present invention have high light-shielding properties against visible light and excellent height difference absorption properties. Therefore, when used in the production of self-luminous display devices, there is no need to Interstitially fills the height difference between multiple light-emitting elements to prevent reflection from metal wiring, suppress color mixing between multiple light-emitting elements, and improve contrast. In addition, it is cured by irradiation with ultraviolet rays, which improves workability, suppresses the occurrence of glue shortage during cutting, and suppresses the occurrence of overflow and sagging of the adhesive layer from the ends during storage. Therefore, by using the adhesive composition, the photocurable adhesive layer, and the photocurable adhesive sheet of the present invention for the manufacture of a self-luminous display device, it is possible to efficiently manufacture a display device with an improved function of preventing reflection of metal wiring and the like. , a self-luminous display device with improved contrast.
Smart Images

Figure BDA0004096818070000231 
Figure BDA0004096818070000601 
Figure HDA0004096818080000011
Abstract
Description
Technical Field
[0001] The present invention relates to an adhesive composition, a photocurable adhesive layer and a photocurable adhesive sheet, and more particularly to an adhesive composition, a photocurable adhesive layer and a photocurable adhesive sheet suitable for sealing light-emitting elements of self-luminous display devices such as mini / micro LEDs. Background Art
[0002] In recent years, self-luminous display devices represented by mini / micro LED display devices (Mini / Micro Light Emitting Diode Display) have been designed as next-generation display devices. Mini / micro LED display devices, as a basic structure, use a substrate with a large number of tiny LED light-emitting elements (LED chips) arranged at a high density as a display panel, the LED chips are sealed with a sealing material, and a covering member such as a resin film and a glass plate is laminated on the outermost layer.
[0003] Among self-luminous display devices such as mini / micro LED display devices, there are some methods such as white backlight method, white light-emitting color filter method, RGB method, etc. In the white light-emitting color filter method and RGB method, an adhesive colored in black is sometimes used as a sealing material (for example, see patent documents 1 to 3).
[0004] This is because the black adhesive contributes to preventing color mixing and improving contrast by filling the spaces between the RGB LED chips arranged on the substrate of the display panel. In addition, it can prevent reflection of metal wiring, metal oxides such as ITO, etc., which are arranged on the substrate of the display panel.
[0005] In mini / micro LED display devices, LED chips are densely laid on the substrate, and there are a lot of fine height differences between the gaps between the LED chips. The sealing material used in the mini / micro LED display device is required to have the performance of filling these height differences, that is, excellent height difference absorption (also called "height difference tracking"). Therefore, in order to improve the height difference absorption, the above-mentioned black adhesive needs to be designed in a way that shows high fluidity.
[0006] On the other hand, although adhesives showing high fluidity have excellent height difference absorption, they have problems of reduced processability such as shape stability and operability. For example, a laminate having an adhesive layer showing high fluidity is prone to adhesive deficiency during cutting, and the adhesive layer is prone to overflow and droop from the end during storage, and sometimes foreign matter adheres to the overflowed adhesive layer, causing process contamination.
[0007] As an adhesive that takes into account both the above-mentioned height difference absorption and processability, a photocurable adhesive (mixed adhesive) is known (see, for example, Patent Document 4). The mixed adhesive has the following advantages: first, it has high fluidity, is made into a semi-cured state with excellent height difference absorption and fully follows the height difference, and then is irradiated with light to complete the curing, which can improve the processability.
[0008] Prior art literature
[0009] Patent Literature
[0010] Patent Document 1: Japanese Patent Application Publication No. 2019-204905
[0011] Patent Document 2: Japanese Patent Application Publication No. 2017-203810
[0012] Patent Document 3: Japanese Patent Application No. 2018-523854
[0013] Patent Document 4: International Publication No. WO2016 / 170875 Summary of the invention
[0014] Problem that the invention aims to solve
[0015] However, for example, when carbon black or the like is blended into the mixed adhesive to color the mixed adhesive black, light cannot pass through the adhesive, so curing is inhibited, which causes a problem that it is difficult to improve processability.
[0016] The present invention is made based on the above-mentioned situation, and the purpose of the present invention is to provide an adhesive composition, an adhesive layer and an adhesive sheet that are suitable for manufacturing self-luminous display devices such as mini / micro LED display devices with improved functions of preventing reflection of metal wiring, etc. and improved contrast, and have excellent height difference absorption and processability.
[0017] Solutions for solving problems
[0018] The inventors of the present invention have conducted in-depth research to achieve the above-mentioned purpose. As a result, it is found that by making the adhesive composition, the photocurable adhesive layer, and the photocurable adhesive sheet show absorptivity in the visible light region but have high transmittance in the ultraviolet region, they are colored so as to show high light-shielding properties to visible light and can be cured by ultraviolet irradiation. In addition, it is found that as the above-mentioned adhesive composition, by using an adhesive composition containing a polymer having a benzophenone structure in the side chain, a mixture of monomer components constituting the polymer, or a partial polymer of a mixture of monomer components constituting the polymer, it is possible to provide a photocurable adhesive layer and a photocurable adhesive sheet that can take into account excellent height difference absorption before photocuring and excellent processability after photocuring, and the function of preventing reflection of metal wiring, etc. in the self-luminous display device, the contrast is improved, and excellent height difference absorption and processability can be taken into account. The present invention is completed based on these insights.
[0019] A first aspect of the present invention provides an adhesive composition comprising a colorant and a polymer (A) having a benzophenone structure in a side chain, wherein the maximum transmittance of the adhesive composition at a wavelength of 200 to 400 nm is greater than the maximum transmittance at a wavelength of 400 to 700 nm.
[0020] In addition, the second aspect of the present invention provides an adhesive composition, which contains a colorant and a mixture of monomer components constituting a polymer (A) having a benzophenone structure in a side chain or a partial polymer of a mixture of monomer components constituting a polymer (A) having a benzophenone structure in a side chain, wherein the maximum transmittance of the adhesive composition at a wavelength of 200 to 400 nm is greater than the maximum transmittance at a wavelength of 400 to 700 nm. The adhesive composition of the first and second aspects of the present invention may further contain an ethylenically unsaturated compound (B).
[0021] In this specification, the adhesive compositions according to the first and second aspects of the present invention may be collectively referred to as "adhesive composition (A)".
[0022] In addition, in the present specification, when referred to as "polymer (A) having a benzophenone structure in a side chain" or "BP polymer (A)", unless otherwise specified, it includes "polymer (A) having a benzophenone structure in a side chain" and "a mixture of monomer components constituting the polymer (A) having a benzophenone structure in a side chain or a partial polymer of a mixture of monomer components constituting the polymer (A) having a benzophenone structure in a side chain".
[0023] In addition, the third aspect of the present invention provides a photocurable adhesive layer, which is an adhesive layer formed from a cured product of the adhesive composition (A), wherein the cured product is a cured product in which the benzophenone structure remains. In addition, the fourth aspect of the present invention provides a photocurable adhesive sheet having the photocurable adhesive layer of the third aspect of the present invention.
[0024] In this specification, the photocurable adhesive layer on the third side of the present invention may be referred to as "photocurable adhesive layer (A)". In addition, the photocurable adhesive sheet on the fourth side of the present invention may be referred to as "photocurable adhesive sheet (A)".
[0025] The photocurable adhesive layer (A) is formed by the cured product of the adhesive composition (A), and the cured product has a benzophenone structure possessed by the BP polymer (A). The benzophenone structure can be cured by forming a cross-linked structure through ultraviolet irradiation. The photocurable adhesive layer (A) before curing is in a semi-cured state with high fluidity, showing excellent height difference absorption. Therefore, when the photocurable adhesive layer (A) before curing is laminated to a display panel in which light-emitting elements (LED chips) are arranged at a high density, the fine height difference between the light-emitting elements (LED chips) can be fully followed, so that no bubbles remain and there is no gap to fit. On the other hand, the photocurable adhesive layer (A) after curing shows excellent processability. Therefore, when the laminated body including the cured photocurable adhesive layer (A) is cut, the occurrence of glue shortage can be suppressed, and the overflow and sagging of the adhesive layer from the end can be suppressed during storage. In this way, according to the photocurable adhesive layer (A) composed of the above-mentioned cured product of the adhesive composition (A), excellent height difference absorption and processability can be appropriately taken into account.
[0026] The maximum value of the transmittance of the adhesive composition (A) at a wavelength of 200 to 400 nm is greater than the maximum value of the transmittance at a wavelength of 400 to 700 nm. In addition, it is preferred that the maximum value of the transmittance of the photocurable adhesive layer (A) at a wavelength of 200 to 400 nm is greater than the maximum value of the transmittance at a wavelength of 400 to 700 nm. That is, the adhesive composition (A) and the photocurable adhesive layer (A) have high absorptivity to visible light (wavelength 400 to 700 nm) and excellent light shielding properties. The excellent light shielding properties of the adhesive composition (A) and the photocurable adhesive layer (A) to visible light are preferred from the following aspects: the photocurable adhesive layer (A) filled in the fine height difference between the LED chips without gaps will prevent reflection caused by metal wiring on the display panel, etc., prevent the color mixing of the arranged light-emitting elements (LED chips) and improve the contrast. On the other hand, the adhesive composition (A) and the photocurable adhesive layer (A) have high transmittance to ultraviolet rays (wavelength 200 to 400 nm). The adhesive composition (A) and the photocurable adhesive layer (A) have excellent ultraviolet light transmittance, which is preferred from the perspective of improving the processability of the photocurable adhesive layer (A) by causing a curing reaction by irradiating the photocurable adhesive layer (A) with ultraviolet light. That is, the adhesive composition (A) and the photocurable adhesive layer (A) have a maximum transmittance at a wavelength of 200 to 400 nm greater than the maximum transmittance at a wavelength of 400 to 700 nm, which is preferred from the perspective of being able to achieve both excellent light-shielding properties against visible light and a curing reaction based on ultraviolet light irradiation.
[0027] The colorant is preferably a colorant whose maximum transmittance at a wavelength of 200 to 400 nm is greater than the maximum transmittance at a wavelength of 400 to 700 nm. This configuration is preferred from the perspective of achieving a maximum transmittance of the adhesive composition (A) and the photocurable adhesive layer (A) at a wavelength of 200 to 400 nm greater than the maximum transmittance at a wavelength of 400 to 700 nm.
[0028] In this specification, “a colorant having a maximum value of transmittance at a wavelength of 200 to 400 nm greater than a maximum value of transmittance at a wavelength of 400 to 700 nm” may be referred to as “colorant (A)”.
[0029] The adhesive composition (A) preferably further comprises a photopolymerization initiator (C) that absorbs ultraviolet rays with a wavelength of 300 nm to 500 nm to generate free radicals. This configuration is preferred for curing the adhesive composition (A) into a cured product in which the benzophenone structure of the BP polymer (A) remains, thereby obtaining a photocurable adhesive layer (A).
[0030] The storage modulus (G'b85) of the photocurable pressure-sensitive adhesive layer (A) before curing at 85° C. is preferably less than 65 kPa. This configuration is preferred in that the photocurable pressure-sensitive adhesive layer (A) before curing exhibits excellent level difference absorptivity.
[0031] The storage modulus (G'a10) of the photocurable adhesive layer (A) after curing at 10°C and the storage modulus (G'b85) of the photocurable adhesive layer (A) before curing at 85°C preferably satisfy the following relational expression (1).
[0032] 2.8 <G'a10 / G'b85 (1)
[0033] This configuration is preferred because the photocurable pressure-sensitive adhesive layer (A) before curing exhibits excellent level difference absorptivity and the photocurable pressure-sensitive adhesive layer (A) after curing exhibits excellent processability.
[0034] The storage modulus (G'a10) of the photocurable adhesive layer (A) after curing at 10° C. is preferably 90 kPa or more. This configuration is preferred in that the photocurable adhesive layer (A) after curing exhibits excellent processability.
[0035] The curing is preferably based on a wavelength of less than 300 nm and a cumulative light intensity of 3000 mJ / cm 2 This configuration is preferred from the viewpoint that the photocurable adhesive layer (A) forms a crosslinked structure with the benzophenone structure by the ultraviolet irradiation and is cured, thereby exhibiting excellent processability.
[0036] In addition, the fifth aspect of the present invention provides a self-luminous display device, which includes: a display panel in which a plurality of light-emitting elements are arranged on a single surface of a substrate, and the aforementioned photocurable adhesive sheet (A), wherein the light-emitting elements of the aforementioned display panel are sealed by the photocurable adhesive layer (A) of the aforementioned photocurable adhesive sheet (A), and the aforementioned photocurable adhesive layer (A) is cured. In the self-luminous display device of the fifth aspect of the present invention, the aforementioned display panel may be an LED panel in which a plurality of LED chips are arranged on a single surface of a substrate. This configuration is preferred from the following aspects: In the self-luminous display device of the fifth aspect of the present invention, the photocurable adhesive layer (A) that is filled in the minute height difference between the light-emitting elements (LED chips) without gaps can prevent reflection of metal wiring on the substrate, prevent RGB color mixing, and improve contrast.
[0037] The self-luminous display device according to the fifth aspect of the present invention can be manufactured by a method including the following steps.
[0038] A step of laminating a photocurable adhesive layer (A) of a photocurable adhesive sheet (A) on a display panel having a plurality of light-emitting elements arranged on one side of a substrate, and sealing the light-emitting elements with the photocurable adhesive layer (A); and
[0039] A step of curing the photocurable pressure-sensitive adhesive layer (A) by irradiating it with ultraviolet rays.
[0040] Since the photocurable adhesive layer (A) before curing has excellent height difference absorption, it can fully follow the fine height difference between the light-emitting elements, so that there is no residual air bubble and no gap. In addition, the photocurable adhesive layer (A) is cured by irradiating ultraviolet rays, and has excellent processability.
[0041] In the method for manufacturing a self-luminous display device according to the fifth aspect of the present invention, the ultraviolet rays are preferably ultraviolet rays having a wavelength of less than 300 nm. This configuration is preferred because the photocurable adhesive layer (A) forms a crosslinked structure with the benzophenone structure by ultraviolet irradiation and cures, thereby exhibiting excellent processability.
[0042] Effects of the Invention
[0043] The adhesive composition, photocurable adhesive layer, and photocurable adhesive sheet of the present invention have high light-shielding properties for visible light and excellent height difference absorption. Therefore, by being used in the manufacture of a self-luminous display device, they are filled in the height difference between multiple light-emitting elements without gaps, preventing reflection from metal wiring, suppressing color mixing between multiple light-emitting elements, and improving contrast. In addition, by curing by ultraviolet irradiation, the processability is improved, the occurrence of glue shortage can be suppressed during cutting, and the overflow and sagging of the adhesive layer from the end can be suppressed during storage. Therefore, by using the adhesive composition, photocurable adhesive layer, and photocurable adhesive sheet of the present invention for the manufacture of a self-luminous display device, a self-luminous display device with improved function of preventing reflection of metal wiring, etc. and improved contrast can be efficiently manufactured. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 This is a diagram (cross-sectional view) schematically showing one embodiment of the photocurable pressure-sensitive adhesive sheet of the present invention.
[0045] Figure 2 This is a diagram (cross-sectional view) schematically showing one embodiment of the photocurable pressure-sensitive adhesive sheet of the present invention.
[0046] Figure 3 This is a diagram (cross-sectional view) schematically showing one embodiment of the photocurable pressure-sensitive adhesive sheet of the present invention.
[0047] Figure 4Schematic diagram (cross-sectional view) showing one embodiment of a self-luminous display device (mini / micro LED display device) of the present invention.
[0048] Figure 5 Schematic diagram (cross-sectional view) showing the steps of one embodiment of a method for manufacturing a self-luminous display device (mini / micro LED display device) according to the present invention. DETAILED DESCRIPTION
[0049] Although the embodiments of the present invention will be described with reference to the drawings as needed, the present invention is not limited thereto and is merely an example.
[0050] In this specification, "acrylic polymer" refers to a polymer derived from a monomer component containing more than 50% by weight of acrylic monomers (preferably more than 70% by weight, for example more than 90% by weight). The above-mentioned acrylic monomers refer to monomers derived from monomers having at least one (meth)acryloyl group in one molecule. In addition, in this specification, "(meth)acryloyl" is a general term for acryloyl and methacryloyl. Similarly, "(meth)acrylate" is a general term for acrylate and methacrylate, and "(meth)acrylic acid" is a general term for acrylic acid and methacrylic acid.
[0051] In this specification, "ethylenically unsaturated compound" refers to a compound having at least one ethylenically unsaturated group in the molecule. Examples of ethylenically unsaturated groups include (meth)acryloyl, vinyl, allyl, etc. Hereinafter, a compound having one ethylenically unsaturated group is sometimes referred to as a "monofunctional monomer", and a compound having two or more ethylenically unsaturated groups is sometimes referred to as a "multifunctional monomer". In addition, a compound having X ethylenically unsaturated groups in a multifunctional monomer is sometimes referred to as an "X-functional monomer".
[0052] In this specification, the adhesive composition containing an ethylenically unsaturated compound means that the ethylenically unsaturated compound is contained in the form of a partial polymer unless otherwise specified. Such a partial polymer is usually a mixture of the ethylenically unsaturated compound (unreacted monomer) containing an ethylenically unsaturated group and the ethylenically unsaturated compound polymerized with the ethylenically unsaturated group.
[0053] In this specification, the total monomer components constituting the adhesive composition refer to the total amount of the monomer components constituting the polymer contained in the adhesive composition and the monomer components contained in the adhesive composition in the form of unreacted monomers. The composition of the monomer components constituting the adhesive composition is generally substantially consistent with the composition of the monomer components of the adhesive layer formed by the adhesive composition and the composition of the monomer components constituting the photocured product thereof.
[0054] In this specification, the term "active energy ray" is a concept including light such as ultraviolet rays, visible light, infrared rays, α rays, β rays, γ rays, electron rays, neutron rays, radiation such as X rays, and the like.
[0055] [Adhesive composition (A)]
[0056] The adhesive composition of the first aspect of the present invention contains a colorant and a polymer (A) having a benzophenone structure in a side chain, wherein the maximum transmittance of the adhesive composition at a wavelength of 200 to 400 nm is greater than the maximum transmittance at a wavelength of 400 to 700 nm.
[0057] In addition, the adhesive composition of the second aspect of the present invention contains a colorant and a mixture of monomer components constituting a polymer (A) having a benzophenone structure in a side chain or a partial polymer of a mixture of monomer components constituting a polymer (A) having a benzophenone structure in a side chain, and the maximum value of the transmittance of the adhesive composition at a wavelength of 200 to 400 nm is greater than the maximum value of the transmittance at a wavelength of 400 to 700 nm.
[0058] The adhesive composition (adhesive composition (A)) of the first and second aspects of the present invention may further contain an ethylenically unsaturated compound (B).
[0059] The pressure-sensitive adhesive composition (A) may contain, in addition to the above, a photopolymerization initiator (C) which absorbs ultraviolet rays having a wavelength of 300 nm to 500 nm to generate radicals, and other additives, which will be described later.
[0060] It should be noted that, in this specification, the above-mentioned "mixture of monomer components" includes the case where it is composed of a single monomer component and the case where it is composed of two or more monomer components. In addition, the above-mentioned "partially polymerized product of a mixture of monomer components" refers to a composition in which one or more monomer components among the constituent monomer components of the above-mentioned "mixture of monomer components" are partially polymerized.
[0061] The adhesive composition (A) may have any form, for example, a solvent type, an emulsion type, a hot melt type (hot melt type), a solvent-free type (active energy ray curing type, for example, a monomer mixture, or a monomer mixture and a partial polymer thereof, etc.), etc. From the aspect of obtaining an adhesive layer with excellent appearance, the adhesive composition (A) of the present invention is preferably an active energy ray curing type. In this specification, the adhesive composition refers to a composition for forming an adhesive layer, including a composition for forming an adhesive.
[0062] The adhesive composition (A) is not particularly limited, and examples thereof include: a composition containing the BP polymer (A) as an essential component; a composition containing a mixture of monomer components constituting the BP polymer (A) or a partial polymer thereof as an essential component, etc. Although not particularly limited, examples of the former include so-called solvent-based adhesive compositions, water-dispersible adhesive compositions (emulsion-based adhesive compositions), etc., and examples of the latter include so-called active energy ray-curable adhesive compositions, etc.
[0063] As described above, the adhesive composition (A) may be a solvent-based solvent. The above-mentioned solvent is not particularly limited as long as it is an organic compound that can be used as a solvent, and examples thereof include: hydrocarbon solvents such as cyclohexane, hexane, and heptane; aromatic solvents such as toluene and xylene; ester solvents such as ethyl acetate and methyl acetate; ketone solvents such as acetone and methyl ethyl ketone; alcohol solvents such as methanol, ethanol, butanol, and isopropanol, etc. It should be noted that the above-mentioned solvent may be a mixed solvent containing two or more solvents.
[0064] The adhesive composition (A) may be an acrylic adhesive composition in which more than 50% by weight (preferably more than 70% by weight, for example more than 90% by weight) of all monomer components constituting the adhesive composition are acrylic monomers.
[0065] The maximum value of the transmittance of the adhesive composition (A) at a wavelength of 200 to 400 nm (preferably a wavelength of 330 to 400 nm) is larger than the maximum value of the transmittance at a wavelength of 400 to 700 nm.
[0066] The adhesive composition (A) has low transmittance to visible light (wavelength 400 to 700 nm), i.e., high light-shielding property. The photocurable adhesive layer (A) formed by the cured product of the adhesive composition (A) having excellent light-shielding property to visible light seals the fine height difference between the metal wiring layer and the light-emitting element (LED chip) of the self-luminous display device (mini / micro LED display device) without gaps, thereby preventing reflection caused by the metal wiring, etc., preventing color mixing of the light-emitting element (LED chip), and improving the contrast of the image.
[0067] On the other hand, the adhesive composition (A) has a higher transmittance in the ultraviolet region (wavelength 200 to 400 nm, preferably wavelength 330 to 400 nm) than visible light. Therefore, the photocurable adhesive layer (A) formed by the cured product of the adhesive composition (A) can form a cross-linked structure of the benzophenone structure and cure by ultraviolet irradiation. The processability of the photocurable adhesive layer (A) cured by ultraviolet irradiation is improved, and the lack of glue during cutting and the overflow and sagging of the adhesive layer from the end during storage can be suppressed.
[0068] In this specification, "the maximum value of the transmittance at a wavelength of 200 to 400 nm" refers to the highest transmittance in the range of the wavelength region of 200 to 400 nm. For example, when there is a maximum value of the transmittance in the wavelength region of 200 to 400 nm, the maximum value becomes the maximum value of the transmittance. In addition, when there is no maximum value of the transmittance in the wavelength region of 200 to 400 nm, the higher transmittance of the transmittance at a wavelength of 200 nm or 400 nm becomes the maximum value. The same applies to "the maximum value of the transmittance at a wavelength of 330 to 400 nm" and "the maximum value of the transmittance at a wavelength of 400 to 700 nm".
[0069] The maximum value of the transmittance of the adhesive composition (A) at a wavelength of 400 to 700 nm (visible light region) is, for example, 80% or less, or 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less.
[0070] In a preferred embodiment of the present invention, the average transmittance of the adhesive composition (A) at a wavelength of 200 to 400 nm (preferably a wavelength of 330 to 400 nm) is greater than the average transmittance at a wavelength of 400 to 700 nm. The average transmittance of the adhesive composition (A) at a wavelength of 400 to 700 nm (visible light region) is, for example, 80% or less, or 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less.
[0071] [Colorant]
[0072] The adhesive composition (A) contains a colorant. The colorant is not particularly limited, but is preferably a colorant (colorant (A)) whose maximum transmittance at a wavelength of 200 to 400 nm (preferably 330 to 400 nm) is greater than the maximum transmittance at a wavelength of 400 to 700 nm.
[0073] The maximum transmittance of the adhesive composition (A) at a wavelength of 200 to 400 nm (preferably 330 to 400 nm) is greater than the maximum transmittance at a wavelength of 400 to 700 nm, although this configuration is not particularly limited and can be preferably achieved by allowing the adhesive composition (A) to contain a colorant (A).
[0074] When the adhesive composition (A) contains a colorant (A), the transmittance to visible light (wavelength 400 to 700 nm) is reduced, that is, the light shielding property is improved. On the other hand, the transmittance in the ultraviolet region (wavelength 200 to 400 nm, preferably wavelength 330 to 400 nm) becomes higher than that of visible light.
[0075] The maximum transmittance of the colorant (A) at a wavelength of 400 to 700 nm (visible light region) may be, for example, 80% or less, 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less.
[0076] In a preferred embodiment of the present invention, the average transmittance of the colorant (A) at a wavelength of 200 to 400 nm (preferably a wavelength of 330 to 400 nm) is greater than the average transmittance at a wavelength of 400 to 700 nm. The average transmittance of the colorant (A) at a wavelength of 400 to 700 nm (visible light region) is, for example, 80% or less, or 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less.
[0077] The transmittance of the colorant can be measured using a solution or dispersion diluted with an appropriate solvent such as tetrahydrofuran (THF) or a dispersion medium (an organic solvent with low absorption in the wavelength range of 200 to 700 nm) so that the transmittance at a wavelength of 400 nm is about 50 to 60%.
[0078] As long as the colorant can be dissolved or dispersed in the adhesive composition (A), it can be a dye or a pigment. From the perspective of being able to achieve low haze even if added in small amounts, no sedimentation like a pigment, and being easily evenly distributed, a dye is preferred. In addition, from the perspective of being high in color development even if added in small amounts, a pigment is also preferred. When a pigment is used as a colorant, it is preferred that the conductivity is low or there is no conductivity. In addition, when a dye is used, it is preferably used in combination with an antioxidant or the like.
[0079] Examples of ultraviolet-transmitting black pigments include "9050BLACK", "9256BLACK", "9170BLACK", and "UVBK-0001" manufactured by TOKUSHIKI, and "UB-1" manufactured by Mitsubishi Materials Electronic Chemicals Co., Ltd. Examples of ultraviolet-transmitting black dyes include "SOC-L-0123" manufactured by Orient Chemical Industries Co., Ltd.
[0080] The content of the colorant in the adhesive composition (A) is, for example, about 0.01 to 20 parts by weight, preferably 0.1 to 10 parts by weight, relative to 100 parts by weight of the adhesive composition (A), and can be appropriately set according to the type of colorant, the color tone and light transmittance of the photocurable adhesive layer (A), etc. The colorant can also be added in the form of a solution or dispersion formed by dissolving or dispersing in an appropriate solvent.
[0081] [Polymer having a benzophenone structure in a side chain (A)]
[0082] As the base polymer constituting the adhesive composition (A) of the present invention, a polymer (A) having a benzophenone structure in a side chain (BP polymer (A)) is included. That is, the adhesive composition (A) of the present invention is an adhesive composition containing the BP polymer (A) as a base polymer. It should be noted that the BP polymer (A) can be used alone or in combination of two or more.
[0083] The monomer components that can constitute the BP polymer (A) include compounds having an ethylenically unsaturated group and a benzophenone structure in the molecule (hereinafter sometimes referred to as "ethylenically unsaturated BP"), and may further include ethylenically unsaturated compounds that are not ethylenically unsaturated BP (hereinafter sometimes referred to as "other ethylenically unsaturated compounds").
[0084] Preferred examples of the BP polymer (A) include acrylic polymers having a benzophenone structure in a side chain. The BP polymer (A) is preferably a polymer that does not substantially contain an ethylenically unsaturated group.
[0085] In this specification, "benzophenone structure" refers to the general formula: Ar 1 -(C=O)-Ar 2 -, or -Ar 3 -(C=O)-Ar 2 - diaryl ketone structure shown in FIG. Here, Ar in the above general formula 1 is selected from phenyl groups which may have a substituent. 2 ,Ar 3 are each independently selected from a phenylene group which may have a substituent. 2 and Ar 3 The benzophenone structure can be excited by ultraviolet irradiation, and in the excited state, it can extract hydrogen radicals from other molecules or other parts of the molecule.
[0086] The photocurable adhesive layer (A) formed from the cured product of the adhesive composition (A) containing the BP polymer (A) may contain a benzophenone structure. The benzophenone structure is excited by ultraviolet irradiation, thereby forming a crosslinked structure by a hydrogen radical abstraction reaction, thereby enabling the photocurable adhesive layer (A) to be cured.
[0087] As the BP polymer (A), preferably the general formula: Ar 1 -(C=O)-Ar 2 -Ar in 1 is a phenyl group which may have a substituent, and Ar 2It is a polymer having a phenylene group which may have a substituent and has a benzophenone structure in the side chain. 1 and Ar 2 When at least one of the substituents has one or more substituents, the substituents may be independently selected from the group consisting of an alkoxy group (e.g., an alkoxy group having 1 to 3 carbon atoms, preferably a methoxy group), a halogen atom (e.g., F, Cl, Br, etc., preferably Cl or Br), a hydroxyl group, an amino group and a carboxyl group.
[0088] The BP polymer (A) may have a side chain directly bonded to the main chain by a benzophenone structure as described above, or may have a side chain bonded to the main chain by one or more of, for example, an ester bond, an oxyalkylene structure, etc. As a suitable example of the BP polymer (A), a polymer comprising a repeating unit derived from an ethylenically unsaturated BP may be listed. The repeating unit may be a polymer residue obtained by reacting an ethylenically unsaturated group of a corresponding ethylenically unsaturated BP.
[0089] Examples of the ethylenically unsaturated BP include 4-acryloxybenzophenone, 4-acryloxy-4'-methoxybenzophenone, 4-acryloxyethoxy-4'-methoxybenzophenone, 4-acryloxy-4'-bromobenzophenone, and 2-hydroxy-4-acryloxybenzophenone; 4-[(2-acryloxy)ethoxy]benzophenone, 4-[(2-acryloxy)ethoxy]-4'-bromobenzophenone; 4-methacryloxybenzophenone, 4-methacryloxy-4'-methoxybenzophenone, 4-acryloxy-4'-bromobenzophenone, and 2-hydroxy-4-acryloxybenzophenone; 4-[(2-acryloxy)ethoxy]benzophenone, 4-[(2-acryloxy)ethoxy]-4'-bromobenzophenone, and 4-methacryloxybenzophenone; 4-methacryloyloxy-4'-bromobenzophenone, 4-methacryloyloxyethoxy-4'-bromobenzophenone, 2-hydroxy-4-methacryloyloxybenzophenone, etc., optionally substituted methacryloxybenzophenone; 4-[(2-methacryloyloxy)ethoxy]benzophenone, 4-[(2-methacryloyloxy)ethoxy]-4'-methoxybenzophenone, etc., optionally substituted methacryloxyalkoxybenzophenone; 4-vinylbenzophenone, 4'-bromo-3-vinylbenzophenone, 2-hydroxy-4-methoxy-4'-vinylbenzophenone, etc., optionally substituted vinylbenzophenone, etc., but not limited to these. Olefinically unsaturated BP can be used alone or in combination of two or more for the preparation of BP polymer (A). Olefinically unsaturated BP can use commercially available substances, and can also be synthesized by a known method. From the viewpoint of reactivity and the like, an ethylenically unsaturated BP having a (meth)acryloyl group, that is, an ethylenically unsaturated BP belonging to an acrylic monomer can be preferably used.
[0090] The BP polymer (A) may be a copolymer having repeating units derived from ethylenically unsaturated BP and repeating units derived from ethylenically unsaturated compounds (other ethylenically unsaturated compounds) that are not ethylenically unsaturated BP. Such a BP polymer (A) may be a copolymer comprising monomer components of the above-mentioned ethylenically unsaturated BP and the above-mentioned other ethylenically unsaturated compounds. In addition, the BP polymer may also be a copolymer obtained by copolymerizing a partial polymer (prepolymer) of a monomer mixture consisting only of the above-mentioned other ethylenically unsaturated compounds with the above-mentioned ethylenically unsaturated BP. As the above-mentioned other ethylenically unsaturated compounds, one or more acrylic monomers may be preferably used. As a suitable example of the BP polymer (A), an acrylic BP polymer in which more than 50% by weight (preferably more than 70% by weight, for example more than 90% by weight) of the monomer components constituting the BP polymer (A) are acrylic monomers can be cited.
[0091] The monomer components constituting the BP polymer (A) may contain one or more selected from (meth)acrylic acid alkyl esters having an alkyl group at the ester terminal as the above-mentioned other ethylenically unsaturated compound. Hereinafter, (meth)acrylic acid alkyl esters having a linear or branched alkyl group with a carbon number of not less than X and not more than Y at the ester terminal are sometimes referred to as “(meth)acrylic acid C X-Y The monomer components constituting the BP polymer (A) preferably contain at least (meth)acrylic acid C 1-20 As the other monomer, alkyl esters more preferably include (meth) acrylic acid C 4-20 Alkyl esters, preferably (meth)acrylic acid C 4-18 Alkyl esters (such as acrylic acid C 4-9 alkyl esters).
[0092] As (meth)acrylic acid C 1-20Specific non-limiting examples of the alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, sec-butyl (meth)acrylate, tert-butyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, dodecyl (meth)acrylate, tridecyl (meth)acrylate, tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, hexadecyl (meth)acrylate, heptadecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, and the like. As particularly preferred (meth)acrylic acid alkyl esters, n-butyl acrylate (BA), 2-ethylhexyl acrylate (2EHA), isononyl acrylate, etc. can be cited. As other specific examples of (meth)acrylic acid alkyl esters that can be preferably used, n-butyl methacrylate (BMA), 2-ethylhexyl methacrylate (2EHMA), isostearyl acrylate (iSTA), etc. can be cited. (Meth)acrylic acid alkyl esters can be used alone or in combination of two or more. The monomer components constituting the BP polymer (A) can contain one or more selected from the copolymerizable monomers described later as the above-mentioned other ethylenically unsaturated compounds.
[0093] The adhesive composition (A) may be a photocurable acrylic adhesive composition in which more than 50 wt % (preferably more than 70 wt %, for example more than 90 wt %) of all monomer components are acrylic monomers. The photocurable acrylic adhesive composition forms an acrylic photocured product by photocuring.
[0094] The weight average molecular weight (Mw) of the BP polymer (A) is not particularly limited, and may be, for example, 0.5×10 4 ~500×10 4 From the viewpoint of the cohesiveness of the photocurable adhesive layer (A) and the handling properties of the photocurable adhesive sheet (A), the Mw of the BP polymer (A) is usually 1×10 4 The above is appropriate, preferably 5×10 4 Above, can be 10×10 4 Above, can be 15×10 4 Above, it can also be 20×10 4From the viewpoint of the height difference absorption of the photocurable adhesive layer (A), the Mw of the BP polymer (A) is usually 200×10 4 The following are suitable, preferably 150×10 4 Below, can be 100×10 4 Below, can be 70×10 4 Below, 50×10 4 the following.
[0095] The weight average molecular weight (Mw) of the polymer refers to a value converted to standard polystyrene obtained by gel permeation chromatography (GPC). As a GPC apparatus, for example, a model "HLC-8320GPC" (column: TSKgelGMH-H(S), manufactured by Tosoh Corporation) can be used.
[0096] The glass transition temperature (Tg) of the BP polymer (A) is not particularly limited. The Tg of the BP polymer (A) may be, for example, -80°C or higher and 150°C or lower, -80°C or higher and 50°C or lower, or -80°C or higher and 10°C or lower. From the viewpoint of the height difference absorption of the photocurable adhesive layer (A), it is appropriate that the Tg of the BP polymer (A) is lower than 0°C, preferably -10°C or lower, -20°C or lower, -30°C or lower, -40°C or lower, or -50°C or lower. In addition, from the viewpoint of improving the cohesiveness of the photocurable adhesive layer (A) and the processability after photocuring, it is generally advantageous for the Tg of the BP polymer (A) to be -75°C or higher, or -70°C or higher. In some embodiments, the Tg of the BP polymer (A) may be -55°C or higher, or -45°C or higher. The Tg of the BP polymer (A) may be adjusted by the type and amount of the monomer components constituting the BP polymer.
[0097] Here, the glass transition temperature (Tg) of a polymer refers to the glass transition temperature obtained by the Fox equation based on the composition of the monomer components constituting the polymer. The above-mentioned Fox equation is shown below and is a relationship between the Tg of a copolymer and the glass transition temperature Tgi of a homopolymer formed by homopolymerizing each of the monomers constituting the copolymer.
[0098] 1 / Tg=Σ(Wi / Tgi)
[0099] In the above Fox formula, Tg represents the glass transition temperature of the copolymer (unit: K), Wi represents the weight fraction of monomer i in the copolymer (copolymerization ratio based on weight), and Tgi represents the glass transition temperature of the homopolymer of monomer i (unit: K).
[0100] As the glass transition temperature of the homopolymer used in the calculation of Tg, the value described in the known document is used. For example, for the monomers listed below, the following values are used as the glass transition temperature of the homopolymer of the monomer.
[0101] 2-Ethylhexyl acrylate: -70℃
[0102] n-Butyl acrylate: -55℃
[0103] Isostearyl acrylate: -18℃
[0104] Methyl methacrylate: 105°C
[0105] Methyl acrylate: 8℃
[0106] Cyclohexyl acrylate: 15℃
[0107] N-vinyl-2-pyrrolidone: 54°C
[0108] 2-Hydroxyethyl acrylate: -15℃
[0109] 4-Hydroxybutyl acrylate: -40℃
[0110] Isobornyl acrylate: 94°C
[0111] Acrylic acid: 106°C
[0112] Methacrylic acid: 228°C
[0113] For the glass transition temperature of the homopolymer of the monomer other than the above-mentioned examples, the numerical value recorded in "Polymer Handbook" (3rd edition, John Wiley & Sons, Inc., 1989) is used. In the case where multiple values are recorded in the document, the highest value is adopted. For the monomer whose glass transition temperature of the homopolymer is not recorded in the above-mentioned Polymer Handbook, the value obtained by the determination method recorded in Japanese Patent Publication No. 2007-51271 is used. It should be noted that for the polymer with the nominal value of the glass transition temperature provided by the manufacturer, the nominal value can also be adopted.
[0114] The BP polymer (A) preferably contains, for example, about 0.5 mg or more of benzophenone structures calculated as 4-benzoylphenyl acrylate per 1 g of the polymer. Hereinafter, the value obtained by converting the number of benzophenone structures contained in 1 g of the BP polymer into the amount calculated as 4-benzoylphenyl acrylate is sometimes referred to as the BP equivalent of the BP polymer (unit: mg / g). For example, when 40 μmol of benzophenone structures are contained in 1 g, the BP equivalent of the polymer is calculated to be 10 mg / g.
[0115] From the viewpoint of obtaining a higher photocuring effect (for example, the effect of improving processability by photocuring), in some embodiments, the BP equivalent of the BP polymer (A) is generally appropriate to be 0.1 mg / g or more, and may be 0.5 mg / g or more, 1 mg / g or more, 5 mg / g or more, 8 mg / g or more, 10 mg / g or more, 15 mg / g or more, or 20 mg / g or more. In addition, in some embodiments, from the viewpoint of improving the impact resistance and peel strength of the joint based on the photocured material, the BP equivalent of the BP polymer (A) is generally appropriate to be 100 mg / g or less, and may be 80 mg / g or less, 60 mg / g or less, 40 mg / g or less, 25 mg / g or less, or 15 mg / g or less. The BP equivalent of the BP polymer (A) can be adjusted by the composition of the monomer components constituting the BP polymer (A).
[0116] On top of this, from the viewpoint of reducing the peeling force by photocuring and performing reprocessing and repair, the BP equivalent is preferably 50 mg / g or more, and may be 100 mg / g or more.
[0117] The weight ratio of the BP polymer (A) in the whole adhesive composition (A), that is, the weight fraction of the BP polymer in the adhesive composition (A) is not particularly limited, and can be set in a manner that appropriately balances the height difference absorption of the photocurable adhesive layer (A) and the processability of its photocured product. In some embodiments, the weight fraction of the above-mentioned BP polymer (A) can be, for example, 1% by weight or more, and 5% by weight or more is usually appropriate, and can be 10% by weight or more, 15% by weight or more, 25% by weight or more, 35% by weight or more, 45% by weight or more, or 55% by weight or more. When the weight fraction of the BP polymer (A) increases, there is a tendency for G'a10 / G'b85 described later to increase.
[0118] The method may be implemented in such a way that the weight fraction of the BP polymer (A) in the adhesive composition (A) is substantially 100 wt% (e.g., 99.5 wt% or more). In addition, from the viewpoint of the ease of adhesive performance, in some embodiments, the weight fraction of the BP polymer (A) in the adhesive composition (A) may be, for example, less than 99 wt%, less than 95 wt%, less than 85 wt%, less than 70 wt%, less than 50 wt%, or less than 40 wt%.
[0119] In terms of 4-benzoylphenyl acrylate conversion, it is preferred that, for example, about 0.1 mg or more of benzophenone structure is contained in each 1 g of the adhesive composition (A). Hereinafter, the weight of 4-benzoylphenyl acrylate converted to benzophenone structure contained in each 1 g of the adhesive composition (A) is sometimes referred to as the BP equivalent of the adhesive composition (unit: mg / g). From the viewpoint of obtaining a higher photocuring effect (for example, the effect of improving processability by photocuring), in some embodiments, the BP equivalent of the adhesive composition is generally appropriate to be 0.3 mg / g or more, and may be 0.5 mg / g or more, 1 mg / g or more, 5 mg / g or more, 10 mg / g or more, or 20 mg / g or more. In addition, in some embodiments, from the perspective of impact resistance of the joints based on the photocured material and suppression of strain within the photocured material, the BP equivalent of the adhesive composition is generally appropriate to be 100 mg / g or less, and can be 80 mg / g or less, 60 mg / g or less, 40 mg / g or less, 25 mg / g or less, or 15 mg / g or less.
[0120] [Ethylenically unsaturated compound (B)]
[0121] The adhesive composition (A) may further contain an ethylenically unsaturated compound (B) on the basis of the BP polymer (A). When the adhesive composition (A) is a solvent-free type (active energy ray curable) adhesive composition, the adhesive composition (A) preferably contains an ethylenically unsaturated compound (B). On the other hand, when the adhesive composition (A) is a solvent-type or emulsion-type adhesive composition, it may not contain an ethylenically unsaturated compound (B).
[0122] In addition, when the adhesive composition (A) contains a mixture of monomer components constituting the BP polymer (A) or a partial polymer of a mixture of monomer components constituting the BP polymer (A), the above-mentioned other ethylenically unsaturated compound may be contained as the monomer component, and therefore, the ethylenically unsaturated compound (B) may not necessarily be contained. When the adhesive composition (A) containing the mixture of the monomer components or a partial polymer thereof contains the ethylenically unsaturated compound (B), the ethylenically unsaturated compound (B) may be the same as or different from the above-mentioned other ethylenically unsaturated compound.
[0123] Examples of compounds that can be used as the ethylenically unsaturated compound (B) include the above-mentioned (meth)acrylic acid alkyl esters and the above-mentioned ethylenically unsaturated BPs. Among these, it is preferred to use at least (meth)acrylic acid alkyl esters (e.g., (meth)acrylic acid C 1-20 Alkyl esters, more preferably (meth) acrylic acid C 4-18 Alkyl ester, more preferably acrylic acid C 4-9As particularly preferred (meth)acrylic acid alkyl esters, n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA) can be listed. As other specific examples of (meth)acrylic acid alkyl esters that can be preferably used, isononyl acrylate, n-butyl methacrylate (BMA), 2-ethylhexyl methacrylate (2EHMA), isostearyl acrylate (iSTA) and the like can be listed. (Meth)acrylic acid alkyl esters can be used alone or in combination of two or more. In some embodiments, the ethylenically unsaturated compound (B) preferably includes any one or both of n-butyl acrylate (BA) and 2-ethylhexyl acrylate (2EHA), and more preferably includes at least BA.
[0124] The ethylenically unsaturated compound (B) may contain acrylic acid C in a ratio of 40% by weight or more. 4-9 Alkyl esters. Acrylic acid C 4-9 The proportion of the alkyl ester in the monomer component may be, for example, 50% by weight or more, 60% by weight or more, or 65% by weight or more. In addition, from the viewpoint of improving the cohesiveness of the photocurable adhesive layer (A), the acrylic acid C 4-9 The proportion of the alkyl ester in the ethylenically unsaturated compound (B) is usually appropriately 99.5% by weight or less, and may be 95% by weight or less, 85% by weight or less, 70% by weight or less, or 60% by weight or less.
[0125] As other examples of compounds that can be used as ethylenically unsaturated compounds (B), ethylenically unsaturated compounds (copolymerizable monomers) that can copolymerize with (meth) alkyl acrylates can be listed. As copolymerizable monomers, monomers having polar groups (e.g., carboxyl groups, hydroxyl groups, rings containing nitrogen atoms, etc.) can be suitably used. Monomers having polar groups can, for example, contribute to the introduction of crosslinking points into a polymer containing repeating units derived from the monomer, or to the improvement of the cohesive force of the photocurable adhesive layer (A). Copolymerizable monomers can be used alone or in combination of two or more.
[0126] Specific non-limiting examples of the copolymerizable monomer include the following.
[0127] Carboxyl group-containing monomers: for example, acrylic acid, methacrylic acid, carboxyethyl acrylate, carboxypentyl acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, isocrotonic acid, etc.
[0128] Monomers containing anhydride groups: for example, maleic anhydride and itaconic anhydride.
[0129] Hydroxyl-containing monomers: for example, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, 12-hydroxylauryl (meth)acrylate, hydroxyalkyl (meth)acrylates such as (4-hydroxymethylcyclohexyl)methyl (meth)acrylate, and the like.
[0130] Monomers containing sulfonic acid groups or phosphoric acid groups: for example, styrene sulfonic acid, allyl sulfonic acid, sodium vinyl sulfonate, 2-(meth)acrylamide-2-methylpropanesulfonic acid, (meth)acrylamidepropanesulfonic acid, sulfopropyl (meth)acrylate, (meth)acryloyloxynaphthalenesulfonic acid, 2-hydroxyethylacryloyl phosphate, etc.
[0131] Epoxy group-containing monomers: for example, epoxy group-containing acrylates such as glycidyl (meth)acrylate and 2-ethyl glycidyl (meth)acrylate, allyl glycidyl ether, and glycidyl (meth)acrylate.
[0132] Cyano-containing monomers: such as acrylonitrile, methacrylonitrile, etc.
[0133] Isocyanate group-containing monomers: for example, 2-(meth)acryloyloxyethyl isocyanate, (meth)acryloyl isocyanate, m-isopropenyl-α,α-dimethylbenzyl isocyanate, and the like.
[0134] Amide group-containing monomers: for example (meth)acrylamide; N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dipropyl (meth)acrylamide, N,N-diisopropyl (meth)acrylamide, N,N-di(n-butyl) (meth)acrylamide, N,N-di(tert-butyl) (meth)acrylamide and other N,N-dialkyl (meth)acrylamide; N-ethyl (meth)acrylamide, N-isopropyl (meth)acrylamide, N-butyl (meth)acrylamide, N-n-butyl (meth)acrylamide and other N-alkyl (meth)acrylamide; N-vinyl carboxylic acid amides such as N-vinyl acetamide; monomers having hydroxyl and amide groups, such as N-(2-hydroxyethyl) (methyl)acrylamide; N-hydroxyalkyl(meth)acrylamide, such as N-(2-hydroxypropyl)(meth)acrylamide, N-(1-hydroxypropyl)(meth)acrylamide, N-(3-hydroxypropyl)(meth)acrylamide, N-(2-hydroxybutyl)(meth)acrylamide, N-(3-hydroxybutyl)(meth)acrylamide, and N-(4-hydroxybutyl)(meth)acrylamide; monomers having an alkoxy group and an amide group, such as N-methoxymethyl(meth)acrylamide, N-methoxyethyl(meth)acrylamide, and N-butoxymethyl(meth)acrylamide; and N,N-dimethylaminopropyl(meth)acrylamide, N-(meth)acrylmorpholine, and the like.
[0135] Amino group-containing monomers: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, tert-butylaminoethyl (meth)acrylate. Monomers having epoxy groups: for example, glycidyl (meth)acrylate, methylglycidyl (meth)acrylate, allyl glycidyl ether.
[0136] Monomers having a ring containing a nitrogen atom: for example, N-vinyl-2-pyrrolidone, N-methylvinylpyrrolidone, N-vinylpyridine, N-vinylpiperidone, N-vinylpyrimidine, N-vinylpiperazine, N-vinylpyrazine, N-vinylpyrrole, N-vinylimidazole, N-vinyloxazole, N-(meth)acryloyl-2-pyrrolidone, N-(meth)acryloylpiperidine, N-(meth)acryloylpyrrolidine, N-vinylmorpholine, N-vinyl-3-morpholinone, N-vinyl-2-caprolactam, N-vinyl-1,3-oxazin-2-one, N-vinyl-3,5-morpholinedione, N-vinylpyrazole, N-vinylisoxazole, N-vinylthiazole, N-vinylisothiazole, N-vinylpyridazine, etc. (for example, lactams such as N-vinyl-2-caprolactam).
[0137] Monomers having a succinimide skeleton include, for example, N-(meth)acryloyloxymethylenesuccinimide, N-(meth)acryloyl-6-oxyhexamethylenesuccinimide, and N-(meth)acryloyl-8-oxyhexamethylenesuccinimide.
[0138] Maleimides: for example, N-cyclohexylmaleimide, N-isopropylmaleimide, N-laurylmaleimide, N-phenylmaleimide, etc.
[0139] Itaconimides: for example, N-methyl itaconimide, N-ethyl itaconimide, N-butyl itaconimide, N-octyl itaconimide, N-2-ethylhexyl itaconimide, N-cyclohexyl itaconimide, N-lauryl itaconimide, etc.
[0140] Aminoalkyl (meth)acrylates: for example, aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, N,N-diethylaminoethyl (meth)acrylate, tert-butylaminoethyl (meth)acrylate.
[0141] Alkoxy-containing monomers: for example, alkoxyalkyl (meth)acrylates (alkoxyalkyl (meth)acrylates) such as 2-methoxyethyl (meth)acrylate, 3-methoxypropyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, propoxyethyl (meth)acrylate, butoxyethyl (meth)acrylate, and ethoxypropyl (meth)acrylate; and alkoxyalkyl (meth)acrylates (for example, alkoxypolyalkylene glycol (meth)acrylate) such as methoxyethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, and methoxypolypropylene glycol (meth)acrylate.
[0142] Alkoxysilyl-containing monomers: for example, alkoxysilyl-containing (meth)acrylates such as 3-(meth)acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-(meth)acryloxypropylmethyldimethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane, and alkoxysilyl-containing vinyl compounds such as vinyltrimethoxysilane and vinyltriethoxysilane.
[0143] Vinyl esters: such as vinyl acetate, vinyl propionate, etc.
[0144] Vinyl ethers: vinyl alkyl ethers such as methyl vinyl ether and ethyl vinyl ether.
[0145] Aromatic vinyl compounds: for example, styrene, α-methylstyrene, vinyltoluene, etc.
[0146] Olefins: such as ethylene, butadiene, isoprene, isobutylene, etc.
[0147] (Meth)acrylates having an alicyclic hydrocarbon group: (meth)acrylates having an alicyclic hydrocarbon group such as cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentyl (meth)acrylate, and adamantyl (meth)acrylate.
[0148] (Meth)acrylates having an aromatic hydrocarbon group: for example, (meth)acrylates having an aromatic hydrocarbon group, such as phenyl (meth)acrylate, phenoxyethyl (meth)acrylate, and benzyl (meth)acrylate.
[0149] In addition, (meth)acrylates containing heterocycles such as tetrahydrofurfuryl (meth)acrylate, (meth)acrylates containing halogen atoms such as (meth)acrylates containing vinyl chloride groups and fluorine atoms, (meth)acrylates containing silicon atoms such as silicone (meth)acrylates, and (meth)acrylates obtained from terpene compound derivative alcohols, etc.
[0150] When using such a copolymerizable monomer, its usage is not particularly limited, and it is usually appropriate to set it to 0.01% by weight or more of the total monomer components constituting the adhesive composition (A). From the viewpoint of better exerting the use effect of the copolymerizable monomer, the usage of the copolymerizable monomer (that is, the weight fraction of the copolymerizable monomer in the above-mentioned total monomer components) can be set to 0.1% by weight or more of the total monomer components, or it can be set to 0.5% by weight or more. In addition, from the viewpoint of easily obtaining a balance of adhesive properties, it is usually appropriate to set the usage of the copolymerizable monomer to 50% by weight or less of the total monomer components, preferably to 40% by weight or less.
[0151] The copolymerizable monomer may include a monomer having a nitrogen atom. By using a monomer having a nitrogen atom, the cohesive force of the photocurable adhesive layer (A) can be increased, and the peel strength after photocuring can be preferably increased. As a suitable example of a monomer having a nitrogen atom, a monomer having a ring containing a nitrogen atom can be listed. As a monomer having a ring containing a nitrogen atom, the substances exemplified above can be used, for example, N-vinyl cyclic amides shown in general formula (1) can be used.
[0152]
[0153] Here, in the general formula (1), R 1 is a divalent organic group, specifically -(CH2) n -. n is an integer of 2 to 7 (preferably 2, 3 or 4). Among them, N-vinyl-2-pyrrolidone can be preferably used. Other suitable examples of the monomer having a nitrogen atom include (meth)acrylamide.
[0154] The amount used when using a monomer having a nitrogen atom (preferably a monomer having a ring containing a nitrogen atom such as N-vinyl cyclic amide) is not particularly limited, for example, it can be more than 1% by weight of the total monomer components, it can be more than 2% by weight, it can be more than 3% by weight, and further can be more than 5% by weight or more than 7% by weight. In one embodiment, the amount of the monomer containing a nitrogen atom can be more than 10% by weight of the total monomer components, it can be more than 15% by weight, or it can be more than 20% by weight. In addition, it is appropriate to set the amount of the monomer containing a nitrogen atom to less than 40% by weight of the total monomer components, it can be less than 35% by weight, it can be less than 30% by weight, or it can be less than 25% by weight. In another embodiment, the amount of the monomer containing a nitrogen atom can be less than 20% by weight of the total monomer components, or it can be less than 15% by weight. Alternatively, it is also possible not to use a monomer containing a nitrogen atom as the above-mentioned copolymerizable monomer.
[0155] The copolymerizable monomers may contain hydroxyl-containing monomers. By using hydroxyl-containing monomers, the cohesion of the photocurable adhesive layer (A) and the degree of crosslinking (e.g., crosslinking based on isocyanate crosslinking agent) can be appropriately adjusted. The amount used when using hydroxyl-containing monomers is not particularly limited, for example, it can be more than 0.01% by weight of all monomer components, can be more than 0.1% by weight, can be more than 0.5% by weight, can be more than 1% by weight, can also be more than 5% by weight or more than 10% by weight. In addition, from the viewpoint of suppressing the water absorption of the photocurable adhesive layer (A) or its photocured product, in some embodiments, it is appropriate to set the amount of hydroxyl-containing monomers to be less than 40% by weight of all monomer components, can be less than 30% by weight, can be less than 25% by weight, can be less than 20% by weight. In another embodiment, the amount of hydroxyl-containing monomers can be less than 15% by weight of all monomer components, can be less than 10% by weight, can be less than 5% by weight. Alternatively, hydroxyl-containing monomers may not be used as the copolymerizable monomers.
[0156] The ratio of carboxyl group-containing monomer in all monomer components can be, for example, less than 2 wt %, less than 1 wt %, or less than 0.5 wt % (for example, less than 0.1 wt %). The adhesive composition (A) can also be substantially free of carboxyl group-containing monomer as its constituent monomer component. Here, substantially free of carboxyl group-containing monomer means that carboxyl group-containing monomer is at least intentionally not used. This can be advantageous from the viewpoints of the metal corrosion prevention of the photocurable adhesive layer (A) formed by the adhesive composition (A) and its photocured product.
[0157] The copolymerizable monomer may contain a (meth)acrylate containing an alicyclic hydrocarbon group. Thus, the cohesive force of the photocurable adhesive layer (A) can be increased, and the peel strength after photocuring can be increased. As the (meth)acrylate containing an alicyclic hydrocarbon group, the substances exemplified above can be used, for example, cyclohexyl acrylate and isobornyl acrylate can be preferably used. The amount used when using the (meth)acrylate containing an alicyclic hydrocarbon group is not particularly limited, for example, it can be set to more than 1% by weight, more than 3% by weight, or more than 5% by weight of the total monomer components. In one embodiment, the amount of the (meth)acrylate containing an alicyclic hydrocarbon group can be more than 10% by weight of the total monomer components, or more than 15% by weight. It is appropriate to set the upper limit of the amount of the (meth)acrylate containing an alicyclic hydrocarbon group to about 40% by weight or less, for example, it can be less than 30% by weight, or less than 25% by weight (for example, less than 15% by weight, and further less than 10% by weight). Alternatively, the (meth)acrylate containing an alicyclic hydrocarbon group may not be used as the copolymerizable monomer.
[0158] The above-mentioned copolymerizable monomer may contain an alkoxysilyl-containing monomer. The alkoxysilyl-containing monomer is typically an ethylenically unsaturated compound having at least one (preferably two or more, for example, two or three) alkoxysilyl group in one molecule, and its specific example is as described above. The above-mentioned alkoxysilyl-containing monomer may be used alone or in combination of two or more. By using an alkoxysilyl-containing monomer, a cross-linked structure based on a condensation reaction of a silanol group (silanol condensation) can be introduced into the photocurable adhesive layer (A).
[0159] The amount used when using an alkoxysilyl-containing monomer is not particularly limited. In some embodiments, the amount of the alkoxysilyl-containing monomer can be set to, for example, 0.005% by weight or more of the total monomer components constituting the adhesive composition (A), and it is usually appropriate to set it to 0.01% by weight or more, and it can be set to 0.03% by weight or more, or it can be set to 0.05% by weight or more. In addition, from the perspective of the height difference absorption of the adhesive composition (A), it is usually appropriate to set the amount of the alkoxysilyl-containing monomer to be less than 1.0% by weight of the total monomer components, and it can be less than 0.5% by weight or less, or it can be less than 0.1% by weight.
[0160] As further other examples of compounds that can be used as the ethylenically unsaturated compound (B), polyfunctional monomers can be cited. When a binder composition (A) comprising a polyfunctional monomer is cured to produce a curable binder layer (A), the polyfunctional monomer can be reacted to obtain a curable binder layer (A) cross-linked with the polyfunctional monomer. Examples of the polyfunctional monomer include bifunctional monomers such as 1,6-hexanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, allyl (meth)acrylate, vinyl (meth)acrylate, and divinylbenzene; trifunctional or higher polyfunctional monomers such as trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tetramethylolmethane tri(meth)acrylate, and dipentaerythritol hexa(meth)acrylate; and epoxy acrylates, polyester acrylates, and urethane acrylates. Preferred examples thereof include 1,6-hexanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and dipentaerythritol hexa(meth)acrylate. The polyfunctional monomer may be used alone or in combination of two or more.
[0161] The amount used when using a multifunctional monomer is not particularly limited, and can be set to be less than 5.0% by weight of all monomer components constituting the adhesive composition (A). Thus, it is possible to avoid forming an excessive cross-linked structure when the photocurable adhesive layer (A) is formed (i.e., the stage before photocuring), thereby improving the height difference absorptivity of the photocurable adhesive layer (A). The amount of the multifunctional monomer used, for example, can be less than 4.0% by weight of all monomer components, can be less than 3.0% by weight, can be less than 2.0% by weight, can be less than 1.0% by weight, can be less than 0.5% by weight, or can be less than 0.3% by weight. It is also possible not to use a multifunctional monomer. In addition, in some embodiments, from the viewpoint of imparting appropriate cohesiveness to the photocurable adhesive layer (A), the amount of the multifunctional monomer used relative to all monomer components can be, for example, more than 0.001% by weight, can be more than 0.005% by weight, can be more than 0.01% by weight, or can be more than 0.03% by weight.
[0162] The weight ratio of the BP polymer (A) in the total amount of the BP polymer (A) and the ethylenically unsaturated compound (B) contained in the adhesive composition (A) is not particularly limited, and can be set in a manner that appropriately balances the height difference absorption of the photocurable adhesive layer (A) formed by the adhesive composition (A) and the processability of its photocured product. In some embodiments, the weight fraction of the above-mentioned BP polymer (A) can be, for example, 0.5% by weight or more, usually 1% by weight or more, preferably 1.5% by weight or more, and more preferably 5% by weight or more. From the viewpoint of improving the effect of photocuring, it can be 10% by weight or more, 15% by weight or more, 25% by weight or more, 35% by weight or more, 45% by weight or more, or 55% by weight or more. In addition, from the viewpoint of the ease of preparation and coating properties of the adhesive composition (A), in some embodiments, the weight ratio of the BP polymer (A) in the above-mentioned total amount can be, for example, less than 99 weight %, less than 95 weight %, less than 85 weight %, less than 70 weight %, less than 50 weight %, or less than 40 weight %.
[0163] The weight ratio of the organic solvent to the total weight of the adhesive composition (A) may be, for example, 30% by weight or less, 20% by weight or less is advantageous, preferably 10% by weight or less, and more preferably 5% by weight or less. In some embodiments, the weight ratio of the organic solvent may be 3% by weight or less, 1% by weight or less, 0.5% by weight or less, 0.1% by weight or less, 0.05% by weight or less, or substantially no organic solvent may be contained.
[0164] From the viewpoint of coating properties in the above-mentioned normal temperature range, the viscosity of the above-mentioned adhesive composition (A) (measured by BH-type viscometer, No. 5 rotor, at 10 rpm, and measuring temperature of 30°C. The same applies below.) is appropriately 1000 Pa·s or less, preferably 100 Pa·s or less, and more preferably 50 Pa·s or less. The viscosity of the above-mentioned adhesive composition (A) can be, for example, 30 Pa·s or less, 20 Pa·s or less, 10 Pa·s or less, or 5 Pa·s or less. The lower limit of the viscosity of the adhesive composition (A) is not particularly limited. From the viewpoint of suppressing shrinkage cavities of the adhesive composition within the coating range and overflow of the adhesive composition at the outer edge of the coating range, it is usually appropriate to be 0.1 Pa·s or more, and can be 0.5 Pa·s or more, or 1 Pa·s or more.
[0165] The adhesive composition (A) contains at least a compound having one ethylenically unsaturated group (i.e., a monofunctional monomer) (B1) as the ethylenically unsaturated compound (B). The monofunctional monomer (B1) can be selected from the examples of the ethylenically unsaturated compound (B) to be used. The monofunctional monomer can be used alone or in combination of two or more.
[0166] The weight ratio of the monofunctional monomer (B1) in the total amount of the BP polymer (A) and the ethylenically unsaturated compound (B) may be, for example, 1% by weight or more, 5% by weight or more, or 15% by weight or more. In some embodiments, from the viewpoints of the ease of preparation and coating of the adhesive composition (A), the weight ratio of the monofunctional monomer (B1) may be 25% by weight or more, 35% by weight or more, or 45% by weight or more. In addition, in the total amount, the weight ratio of the monofunctional monomer (B1) may be, for example, 99% by weight or less, and generally 95% by weight or less is appropriate, and may be 85% by weight or less, 75% by weight or less, 65% by weight or less, 55% by weight or less, or 45% by weight or less.
[0167] In the embodiment in which the adhesive composition (A) includes a monofunctional monomer (B1), the glass transition temperature (Tg) obtained by the Fox equation based on the composition of the monofunctional monomer (B1) is not particularly limited, and may be, for example, -80°C or higher and 250°C or lower. From the viewpoint of compatibility of the polymer derived from the monofunctional monomer (B1) with other components, the Tg based on the composition of the monofunctional monomer (B1) is generally preferably 150°C or lower, 100°C or lower, 70°C or lower, 50°C or lower, or 30°C or lower. In some embodiments, from the viewpoint of the height difference absorption of the photocurable adhesive layer (A), the Tg based on the composition of the monofunctional monomer (B1) is preferably lower than 0°C, more preferably -10°C or lower, -20°C or lower, -30°C or lower, or -40°C or lower. In addition, from the viewpoint of the cohesiveness of the photocurable adhesive layer (A) and the processability after photocuring, the Tg based on the composition of the monofunctional monomer (B1) is generally advantageously -60°C or higher, and may be -54°C or higher, -50°C or higher, -45°C or higher, -35°C or higher, or -25°C or higher. The above Tg can be adjusted by the compounds used as the monofunctional monomers and their usage ratios.
[0168] In the adhesive composition (A) comprising the BP polymer (A) and the monofunctional monomer (B1), the photocurable adhesive layer (A) formed from the adhesive composition, and the photocured product thereof, the Tg (hereinafter referred to as "TgA ”) and the Tg (hereinafter referred to as “Tg B1 ".) can be obtained through Tg B1 [℃]-Tg A [°C] The calculated Tg difference [°C] (hereinafter also referred to as ΔTg) is set in a range of, for example, above -50°C and below 70°C. From the viewpoint of compatibility between the photocurable adhesive layer (A) and its photocured product, it is advantageous that the absolute value of the Tg difference is not too large. In some embodiments, ΔTg may be, for example, above -10°C, preferably above 0°C, above 7°C, above 10°C, above 20°C, or above 30°C.
[0169] The adhesive composition (A) may contain at least a compound having two or more ethylenically unsaturated groups (i.e., a multifunctional monomer) (B2) as the above-mentioned ethylenically unsaturated compound (B). The multifunctional monomer (B2) may be used alone or in combination of two or more from the examples of the above-mentioned multifunctional monomers. The amount of the multifunctional monomer (B2) used may be set in the same manner as the ratio of the multifunctional monomer to the total monomer components constituting the adhesive composition (A).
[0170] In the method of using a monofunctional monomer (B1) and a polyfunctional monomer (B2) in combination as the ethylenically unsaturated compound (B), the weight ratio of the monofunctional monomer (B1) in the ethylenically unsaturated compound (B) may be, for example, 1% by weight or more, and generally 25% by weight or more is appropriate, and may be 50% by weight or more, 75% by weight or more, 95% by weight or more, or 99% by weight or more. In addition, the weight ratio of the monofunctional monomer (B1) in the ethylenically unsaturated compound (B) may be, for example, 99.9% by weight or less, or 99.8% by weight or less.
[0171] In the adhesive composition (A), the ethylenically unsaturated compound (B) may be contained in the form of a partial polymer or in the form of an unreacted monomer in its entirety. A preferred embodiment of the adhesive composition (A) contains the ethylenically unsaturated compound (B) in the form of a partial polymer. There is no particular limitation on the polymerization method for partially polymerizing the ethylenically unsaturated compound (B), and for example, various polymerization methods known in the art may be appropriately selected and used: photopolymerization by irradiation with light such as ultraviolet rays; radiation polymerization by irradiation with radiation such as β rays and γ rays; thermal polymerization such as solution polymerization, emulsion polymerization, and bulk polymerization; and the like. From the viewpoint of efficiency and simplicity, photopolymerization may be preferably used. Photopolymerization makes it possible to easily control the polymerization conversion rate (monomer conversion rate) by polymerization conditions such as the amount of light irradiation (amount of light).
[0172] The polymerization conversion rate of the ethylenically unsaturated compound (B) in the above-mentioned partial polymer is not particularly limited. From the viewpoints of the ease of preparation and coating of the adhesive composition (A), it is appropriate that the above-mentioned polymerization conversion rate is usually about 50% by weight or less, preferably about 40% by weight or less (e.g., about 35% by weight or less). The lower limit of the polymerization conversion rate is not particularly limited, and is typically about 1% by weight or more, and it is usually appropriate to set it to about 5% by weight or more.
[0173] The adhesive composition (A) containing a partial polymer of an ethylenically unsaturated compound (B) can be obtained, for example, by partially polymerizing a monomer mixture containing the entire amount of the ethylenically unsaturated compound (B) used to prepare the adhesive composition by an appropriate polymerization method (e.g., photopolymerization). In addition, the adhesive composition (A) containing a partial polymer of an ethylenically unsaturated compound (B) can also be a mixture of a partial polymer of a monomer mixture containing a portion of the ethylenically unsaturated compound (B) used to prepare the adhesive composition and the remaining ethylenically unsaturated compound (B) or its partial polymer. It should be noted that in this specification, "complete polymer" refers to a polymerization conversion rate higher than 95% by weight.
[0174] The above-mentioned partial polymer can be prepared, for example, by irradiating the ethylenically unsaturated compound (B) with ultraviolet rays. When the above-mentioned partial polymer is prepared in the presence of the BP polymer (A), the ultraviolet irradiation conditions are set in such a way that the ethylenically unsaturated groups react and the benzophenone structure is not excited by light, thereby obtaining an adhesive composition (A) containing the partial polymer of the ethylenically unsaturated compound (B) and the BP polymer (A). As the light source, it is preferred to use a light source such as the above-mentioned black light lamp, UV-LED lamp, etc. that can irradiate ultraviolet rays that do not contain components with a wavelength lower than 300nm or have a small amount of such components.
[0175] Alternatively, the adhesive composition (A) may be prepared by preparing a partial polymer of the ethylenically unsaturated compound (B) in advance and then mixing the partial polymer with the BP polymer (A). When the partial polymer is prepared by irradiating the ethylenically unsaturated compound (B) with ultraviolet light in the absence of a component containing a benzophenone structure, as the ultraviolet light source, both a light source that does not excite the benzophenone structure and a light source that excites the benzophenone structure may be used.
[0176] When preparing the partial polymer of the ethylenically unsaturated compound (B), the reaction of the ethylenically unsaturated group can be promoted by using a photopolymerization initiator. As a photopolymerization initiator, a ketal photopolymerization initiator, an acetophenone photopolymerization initiator, a benzoin ether photopolymerization initiator, an acylphosphine oxide photopolymerization initiator, an α-ketol photopolymerization initiator, an aromatic sulfonyl chloride photopolymerization initiator, a photoactive oxime photopolymerization initiator, a benzoin photopolymerization initiator, a benzyl photopolymerization initiator, a benzophenone photopolymerization initiator, an alkylphenone photopolymerization initiator, a thioxanthone photopolymerization initiator, etc. can be used. It is preferred to use a photopolymerization initiator that absorbs light with a wavelength of more than 300nm (for example, light with a wavelength of more than 300nm and less than 500nm) to generate free radicals. The photopolymerization initiator can be used alone or in combination of two or more.
[0177] [Photopolymerization initiator]
[0178] The adhesive composition (A) may contain a photopolymerization initiator as required for the purpose of improving or imparting photocurability. When the adhesive composition (A) is a solvent-free (active energy ray-curable) adhesive composition, the adhesive composition (A) preferably contains a photopolymerization initiator. On the other hand, when the adhesive composition (A) is a solvent-based or emulsion-based adhesive composition, it may not contain a photopolymerization initiator.
[0179] As the photopolymerization initiator, ketal photopolymerization initiator, acetophenone photopolymerization initiator, benzoin ether photopolymerization initiator, acylphosphine oxide photopolymerization initiator, α-ketol photopolymerization initiator, aromatic sulfonyl chloride photopolymerization initiator, photoactive oxime photopolymerization initiator, benzoin photopolymerization initiator, benzyl photopolymerization initiator, benzophenone photopolymerization initiator, alkylphenone photopolymerization initiator, thioxanthone photopolymerization initiator, etc. can be used. One type of the photopolymerization initiator can be used alone or two or more types can be used in appropriate combination.
[0180] Specific examples of the ketal-based photopolymerization initiator include 2,2-dimethoxy-1,2-diphenylethane-1-one and the like.
[0181] Specific examples of acetophenone-based photopolymerization initiators include: 1-hydroxycyclohexyl-phenyl-ketone, 4-phenoxydichloroacetophenone, 4-tert-butyl-dichloroacetophenone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propane-1-one, 2-hydroxy-2-methyl-1-phenyl-propane-1-one, methoxyacetophenone, etc.
[0182] Specific examples of the benzoin ether-based photopolymerization initiator include benzoin ethers such as benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, and benzoin isobutyl ether, and substituted benzoin ethers such as anisoin methyl ether.
[0183] Specific examples of the acylphosphine oxide-based photopolymerization initiator include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, bis(2,4,6-trimethylbenzoyl)-2,4-di-n-butoxyphenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and bis(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide.
[0184] Specific examples of the α-ketol-based photopolymerization initiator include 2-methyl-2-hydroxypropiophenone, 1-[4-(2-hydroxyethyl)phenyl]-2-methylpropane-1-one, and the like.
[0185] Specific examples of the aromatic sulfonyl chloride-based photopolymerization initiator include 2-naphthalenesulfonyl chloride and the like.
[0186] Specific examples of the photoactive oxime-based photopolymerization initiator include 1-phenyl-1,1-propanedione-2-(O-ethoxycarbonyl)-oxime and the like.
[0187] Specific examples of the benzoin-based photopolymerization initiator include benzoin and the like.
[0188] Specific examples of the benzil-based photopolymerization initiator include benzil and the like.
[0189] Specific examples of the benzophenone-based photopolymerization initiator include benzoylbenzoic acid, 3,3′-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, and α-hydroxycyclohexylphenylketone.
[0190] Specific examples of the thioxanthone-based photopolymerization initiator include thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, isopropylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone.
[0191] As the photopolymerization initiator contained in the adhesive composition (A), a photopolymerization initiator (sometimes referred to as "photopolymerization initiator (C)") that generates free radicals by absorbing light having a wavelength of 300 nm or more (e.g., light having a wavelength of 300 nm or more and 500 nm or less) can be preferably used. When the adhesive composition (A) contains the photopolymerization initiator (C), it is preferred from the perspective of curing the adhesive composition (A) into a cured product in which the benzophenone structure of the BP polymer (A) remains.
[0192] The photopolymerization initiator may be used alone or in combination of two or more. In some embodiments, a photopolymerization initiator containing no phosphorus element in the molecule may be preferably used. The adhesive composition (A) may be substantially free of a photopolymerization initiator containing phosphorus element in the molecule.
[0193] The content of the photopolymerization initiator in the adhesive composition (A) is not particularly limited and can be set in a manner that appropriately exerts the desired effect. In some embodiments, relative to 100 parts by weight of the monomer component constituting the adhesive composition (A), the content of the photopolymerization initiator can be set to, for example, about 0.005 parts by weight or more, usually 0.01 parts by weight or more is appropriate, preferably 0.05 parts by weight or more, can be set to 0.10 parts by weight or more, can be set to 0.15 parts by weight or more, and can also be set to 0.20 parts by weight or more. By increasing the content of the photopolymerization initiator, the photocurability of the adhesive composition (A) is improved. In addition, relative to 100 parts by weight of the monomer component constituting the adhesive composition (A), the content of the photopolymerization initiator is usually set to 5 parts by weight or less, preferably 2 parts by weight or less, can be set to 1 part by weight or less, can be set to 0.7 parts by weight or less, and can also be set to 0.5 parts by weight or less. From the viewpoint of suppressing the gelation of the adhesive composition (A), it can be advantageous that the content of the photopolymerization initiator is not too much.
[0194] [Crosslinking agent]
[0195] In the adhesive composition (A), for example, known crosslinking agents such as isocyanate crosslinking agents, epoxy crosslinking agents, oxazoline crosslinking agents, aziridine crosslinking agents, carbodiimide crosslinking agents, melamine crosslinking agents, urea crosslinking agents, metal alkoxide crosslinking agents, metal chelate crosslinking agents, metal salt crosslinking agents, hydrazine crosslinking agents, and amine crosslinking agents can be mixed as needed. As a crosslinking agent, peroxide can also be used. When the adhesive composition (A) is a solvent-type or emulsion-type adhesive composition, it is preferably mixed with a crosslinking agent.
[0196] The above-mentioned crosslinking agent can be used alone or in combination of two or more. The photocurable adhesive layer (A) formed by the adhesive composition (A) containing the crosslinking agent preferably mainly contains the crosslinking agent in the form after the crosslinking reaction. By using a crosslinking agent, the cohesive force of the photocurable adhesive layer (A) can be appropriately adjusted.
[0197] The amount used when using a crosslinking agent (the total amount thereof when using two or more crosslinking agents) is not particularly limited. From the perspective of realizing an adhesive that exerts adhesive properties such as bonding force and cohesion in a well-balanced manner, it is appropriate that the amount of the crosslinking agent used is generally about 5 parts by weight or less relative to 100 parts by weight of the monomer component constituting the adhesive composition (A), which can be 3 parts by weight or less, 1 part by weight or less, 0.50 parts by weight or less, 0.30 parts by weight or less, or 0.20 parts by weight or less. The lower limit of the amount of the crosslinking agent used is not particularly limited, and it can be an amount of more than 0 parts by weight relative to 100 parts by weight of the monomer component constituting the adhesive composition (A). In some embodiments, the amount of the crosslinking agent used can be, for example, 0.001 parts by weight or more, 0.01 parts by weight or more, 0.05 parts by weight or more, or 0.10 parts by weight or more relative to 100 parts by weight of the monomer component constituting the adhesive composition (A).
[0198] [Chain transfer agent]
[0199] The adhesive composition (A) may contain various chain transfer agents known in the past. As the chain transfer agent, thiols such as n-dodecyl mercaptan, tert-dodecyl mercaptan, thioglycolic acid, and α-thioglycerol may be used. Alternatively, a chain transfer agent that does not contain a sulfur atom (non-sulfur chain transfer agent) may also be used. Specific examples of non-sulfur chain transfer agents include: anilines such as N,N-dimethylaniline and N,N-diethylaniline; terpenes such as α-pinene and terpinolene; styrenes such as α-methylstyrene and α-methylstyrene dimer; compounds having a benzylidene group such as dibenzylideneacetone, cinnamyl alcohol, and cinnamaldehyde; hydroquinones such as hydroquinone and 1,4-dihydroxynaphthalene; quinones such as benzoquinone and naphthoquinone; olefins such as 2,3-dimethyl-2-butene and 1,5-cyclooctadiene; alcohols such as phenol, benzyl alcohol, and allyl alcohol; benzyl hydrogens such as diphenylbenzene and triphenylbenzene; etc. The chain transfer agent may be used alone or in combination of two or more. When a chain transfer agent is used, its amount may be, for example, about 0.01 to 1 part by weight relative to 100 parts by weight of the monomer component. It is also preferable to implement the reaction without using a chain transfer agent.
[0200] As other components that can be included in the adhesive composition (A), silane coupling agents can be listed. By using a silane coupling agent, the peel strength to an adherend (such as a glass plate) can be improved. In addition, a silane coupling agent can be contained in the photocurable adhesive layer (A). The photocurable adhesive layer (A) containing a silane coupling agent can be suitably formed using an adhesive composition (A) containing a silane coupling agent. The silane coupling agent can be used alone or in combination of two or more.
[0201] The adhesive composition (A) may contain various conventional additives in the adhesive field such as tackifier resins (e.g., rosin-based, petroleum-based, terpene-based, phenol-based, ketone-based tackifier resins), viscosity modifiers (e.g., tackifiers), leveling agents, antioxidants, plasticizers, fillers, stabilizers, preservatives, anti-aging agents, etc. as other optional components as necessary. Such various additives can be used by conventional methods. Conventionally known substances are not particularly characteristic of the present invention, so detailed description is omitted.
[0202] It should be noted that the adhesive composition (A) can exert good adhesive force without using the above-mentioned tackifying resin. Therefore, in some embodiments, the content of the above-mentioned tackifying resin in the above-mentioned photocurable adhesive layer (A) or the adhesive composition (A) can be set to, for example, less than 10 parts by weight, and then less than 5 parts by weight relative to 100 parts by weight of the monomer component. The content of the above-mentioned tackifying resin can be less than 1 part by weight (for example, less than 0.5 parts by weight), or less than 0.1 parts by weight (0 parts by weight or more and less than 0.1 parts by weight). The photocurable adhesive layer (A) or the adhesive composition (A) may not contain a tackifying resin.
[0203] [Photocurable Adhesive Layer (A)]
[0204] The photocurable adhesive layer (A) is formed by a cured product as an adhesive composition (A) and a cured product with a benzophenone structure remaining. The benzophenone structure forms a cross-linked structure by ultraviolet irradiation, which can cure the photocurable adhesive layer (A). The photocurable adhesive layer (A) before curing is in a semi-cured state with high fluidity, showing excellent height difference absorption. Therefore, when the photocurable adhesive layer (A) of the aforementioned photocurable adhesive sheet (A) is laminated to a display panel in which light-emitting elements (LED chips) are arranged at a high density, it will fully follow the fine height difference between the light-emitting elements (LED chips), so that there are no bubbles and no gaps. On the other hand, the cured photocurable adhesive layer (A) shows excellent processability. Therefore, when the laminated body including the cured photocurable adhesive layer (A) is cut, the occurrence of glue deficiency can be suppressed, and the overflow and sagging of the adhesive layer from the end can be suppressed during storage. As described above, according to the photocurable adhesive layer (A) composed of the cured product of the adhesive composition (A), both excellent level difference absorption property and processability can be suitably achieved.
[0205] The method for preparing the photocurable adhesive layer (A) is not particularly limited, and the adhesive composition (A) can be prepared, for example, by irradiating the adhesive composition (A) with active energy rays, heating and drying, etc. Specifically, the adhesive composition (A) can be applied (coated) on a substrate or a release liner, and dried, cured, or dried and cured as required.
[0206] It should be noted that the adhesive composition (A) can be applied (coated) using a known coating method, for example, a coating machine such as a gravure roll coater, a reverse roll coater, a lick roll coater, a dip roll coater, a rod coater, a knife coater, a spray coater, a comma coater, or a direct coater can be used.
[0207] When the adhesive composition (A) is cured by irradiation with active energy rays, it is preferably performed in a manner that the ethylenically unsaturated groups contained in the adhesive composition (A) react and the benzophenone structure contained in the photocurable adhesive layer (A) remains. As the active energy rays used to form the photocurable adhesive layer (A), ultraviolet rays are preferably not containing components with a wavelength of less than 300 nm or having a small amount of such components.
[0208] When the adhesive composition (A) contains a BP polymer (A) and an ethylenically unsaturated compound (B), the photocurable adhesive layer (A) may contain a BP polymer (A) and a polymer (E) derived from the ethylenically unsaturated compound (B). In this embodiment, the adhesive composition (A) may be a composition in which the ethylenically unsaturated compound (B) does not contain ethylenically unsaturated BP. According to the adhesive composition (A) of such a composition, a photocurable adhesive layer (A) comprising a BP polymer (A) and a polymer (E) derived from an ethylenically unsaturated compound (B), wherein the polymer (E) is a polymer without a benzophenone structure (sometimes referred to as a "non-BP polymer"), may be manufactured.
[0209] On the other hand, when the adhesive composition (A) contains a mixture of monomer components constituting the BP polymer (A) or a partial polymer of the mixture of the monomer components, the photocurable adhesive layer (A) may be a photocurable adhesive layer containing two or more polymers having different monomer compositions, and at least one of the above two or more polymers is a polymer having a benzophenone structure in the side chain (sometimes referred to as "BP polymer (A')"). The above-mentioned photocurable adhesive layer may contain only two or more BP polymers (A') as the above-mentioned two or more polymers, or may contain a non-BP polymer and a BP polymer (A') in combination. The non-BP polymer can be formed by using an adhesive composition containing an ethylenically unsaturated compound that does not have a benzophenone structure and polymerizing the ethylenically unsaturated compound. The BP polymer (A') may be, for example, the BP polymer (A) contained in the above-mentioned adhesive composition (A), or it may be a modified product thereof, or it may be a substance formed by copolymerizing the ethylenically unsaturated BP contained in the above-mentioned adhesive composition (A) with other ethylenically unsaturated compounds.
[0210] The two or more polymers may or may not be chemically bonded. In some embodiments, the photocurable pressure-sensitive adhesive layer (A) may contain at least one BP polymer in a form that is not chemically bonded to a polymer other than the BP polymer.
[0211] The irradiation of active energy rays for curing the adhesive composition (A) is preferably carried out in a manner that the ethylenically unsaturated groups react and the benzophenone structure remains. As the above-mentioned adhesive composition (A), an adhesive composition comprising a BP polymer (A) and an ethylenically unsaturated compound (B) can be preferably used. As a light source for curing the adhesive composition (A) to form a photo-crosslinkable adhesive, a light source such as the above-mentioned black light lamp, UV-LED lamp, etc. that can irradiate ultraviolet rays that do not contain components with a wavelength lower than 300nm or have a small amount of such components can be preferably used.
[0212] In a preferred embodiment of the present invention, the maximum transmittance of the photocurable adhesive layer (A) at a wavelength of 200 to 400 nm (preferably a wavelength of 330 to 400 nm) is greater than the maximum transmittance at a wavelength of 400 to 700 nm. The photocurable adhesive layer (A) having excellent light-shielding properties for visible light seals the fine height difference between the metal wiring layer and the light-emitting element (LED chip) of the self-luminous display device (mini / micro LED display device) without a gap, thereby preventing reflection caused by metal wiring, etc., preventing color mixing of the light-emitting element (LED chip), and improving the contrast of the image. On the other hand, the photocurable adhesive layer (A) having a high transmittance in the ultraviolet region (wavelength of 200 to 400 nm, preferably a wavelength of 330 to 400 nm) forms a cross-linked structure of the benzophenone structure and cures by irradiating ultraviolet rays, thereby improving processability, and can suppress glue shortage during cutting, and overflow and sagging of the adhesive layer from the end during storage.
[0213] In addition, in a preferred embodiment of the present invention, the maximum value of the transmittance of the photocurable adhesive layer (A) at a wavelength of 400 to 700 nm (visible light region) is, for example, less than 80%, or less than 70%, less than 60%, less than 50%, less than 40%, less than 30%, less than 20%, less than 10% or less than 5%.
[0214] In a preferred embodiment of the present invention, the average transmittance of the photocurable adhesive layer (A) at a wavelength of 200 to 400 nm (preferably a wavelength of 330 to 400 nm) is greater than the average transmittance at a wavelength of 400 to 700 nm. The average transmittance of the photocurable adhesive layer (A) at a wavelength of 400 to 700 nm (visible light region) is, for example, 80% or less, or 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less.
[0215] The photocurable adhesive layer (A) preferably contains, for example, about 0.1 mg or more of a benzophenone structure per 1 g of the adhesive layer, calculated on the basis of 4-benzoylphenyl acrylate. Hereinafter, the weight calculated on the basis of 4-benzoylphenyl acrylate of the benzophenone structure contained in each 1 g of the photocurable adhesive layer (A) is sometimes referred to as the BP equivalent of the adhesive layer (unit: mg / g). From the viewpoint of obtaining a higher photocuring effect (for example, the effect of improving processability by photocuring), it is appropriate that the BP equivalent of the adhesive layer is usually 0.3 mg / g or more, and may be 0.5 mg / g or more, 1 mg / g or more, 5 mg / g or more, 10 mg / g or more, or 20 mg / g or more. In addition, from the perspective of impact resistance of the joints of the photocured material and suppression of strain within the photocured material, the BP equivalent of the adhesive layer is generally appropriate to be 100 mg / g or less, and can be 80 mg / g or less, 60 mg / g or less, 40 mg / g or less, 25 mg / g or less, or 15 mg / g or less.
[0216] (Storage modulus)
[0217] The storage modulus (G'b85) of the photocurable adhesive layer (A) before curing at 85°C is not particularly limited, and is, for example, preferably less than 65 kPa, more preferably less than 60 kPa, further preferably less than 55 kPa, particularly preferably less than 50 kPa, and further preferably less than 45 kPa. Such a configuration is preferred for achieving excellent height difference absorption of the photocurable adhesive layer (A) before curing. In addition, G'b85 is not particularly limited, and from the viewpoint of handling and operability, it is, for example, preferably greater than 5 kPa, more preferably greater than 10 kPa, and further preferably greater than 15 kPa. The storage modulus (G'b85) of the photocurable adhesive layer (A) before curing at 85°C can be adjusted by the composition of the adhesive composition (A) (e.g., Mw and Tg of the BP polymer (A); weight fraction of the BP polymer (A); composition of the monomer components constituting the BP polymer (A) and the ethylenically unsaturated compound (B), type and amount of functional groups; type and amount of crosslinking agent), etc.
[0218] The storage modulus (G'a10) of the photocurable adhesive layer (A) after curing at 10°C is not particularly limited, and is, for example, preferably 90 kPa or more, more preferably 100 kPa or more, more preferably 110 kPa or more, more preferably 120 kPa or more, more preferably 130 kPa or more, more preferably greater than 146 kPa, more preferably 180 kPa or more, further preferably 200 kPa or more, particularly preferably 250 kPa or more, and further may be 300 kPa or more, or 350 kPa or more. Such a configuration is preferred for achieving excellent processability of the photocurable adhesive layer (A) after curing. In addition, G'a10 is not particularly limited, and from the viewpoint of bonding reliability, is, for example, 5000 kPa or less, preferably 2500 kPa or less, and more preferably 1000 kPa or less. The storage modulus (G'a10) of the cured photocurable adhesive layer (A) at 10°C can be adjusted by the composition of the adhesive composition (A) (for example, Mw, Tg, BP equivalent of the BP polymer (A); weight fraction of the BP polymer (A); composition of the monomer components constituting the BP polymer (A) and the ethylenically unsaturated compound (B), type and amount of functional groups; type and amount of the crosslinking agent), etc.
[0219] The ratio (G'a10 / G'b85) of the storage modulus (G'a10) of the photocurable adhesive layer (A) at 10°C after curing to the storage modulus (G'b85) of the photocurable adhesive layer (A) before curing at 85°C is not particularly limited, and is preferably greater than 2.8, more preferably greater than 2.9, further preferably greater than 3, particularly preferably greater than 3.1, and further may be greater than 3.2, greater than 3.3, greater than 3.3, greater than 3.4, greater than 3.5, greater than 3.6, greater than 3.7, greater than 3.8, greater than 3.9, greater than 4, greater than 5, greater than 6, greater than 7, greater than 8, greater than 9, greater than 10, or greater than 11. Such a configuration is preferred from the viewpoint of being able to achieve both excellent height difference absorption of the photocurable adhesive layer (A) before curing and excellent processability of the photocurable adhesive layer (A) after curing. In addition, G'a10 / G'b85 is not particularly limited, and is preferably 100 or less, more preferably 50 or less, and further preferably 30 or less, from the viewpoint of handling property, operability, and bonding reliability. The ratio (G'a10 / G'b85) of the storage modulus (G'a10) of the photocurable adhesive layer (A) after curing at 10°C to the storage modulus (G'b85) of the photocurable adhesive layer (A) before curing at 85°C can be adjusted by the composition of the adhesive composition (A) (e.g., Tg, Mw, BP equivalent of the BP polymer (A); weight fraction of the BP polymer (A); composition of the monomer components constituting the BP polymer (A) and the ethylenically unsaturated compound (B), the type and amount of the functional groups; the type and amount of the crosslinking agent), etc.
[0220] The storage modulus (G'b10) of the photocurable adhesive layer (A) before curing at 10°C is not particularly limited. From the viewpoint of handling and operability, it is, for example, preferably 10 kPa or more, more preferably 50 kPa or more, further preferably 70 kPa or more, or may be 90 kPa or more, or 100 kPa or more. In addition, G'b10 is not particularly limited. From the viewpoint of bonding reliability, it is, for example, 5000 kPa or less, preferably 2500 kPa or less, and more preferably 1000 kPa or less. The storage modulus (G'b10) of the photocurable adhesive layer (A) before curing at 10°C can be adjusted by the composition of the adhesive composition (A) (for example, Mw and Tg of the BP polymer (A); weight fraction of the BP polymer (A); composition of the monomer components constituting the BP polymer (A) and the ethylenically unsaturated compound (B), type and amount of functional groups; type and amount of the crosslinking agent), etc.
[0221] The storage modulus (G'a85) of the photocurable adhesive layer (A) after curing at 85°C is not particularly limited. From the viewpoint of handling and operability, it is, for example, preferably 10 kPa or more, preferably 20 kPa or more, and more preferably 30 kPa or more. In addition, G'a85 is not particularly limited. From the viewpoint of bonding reliability, it is, for example, 1000 kPa or less, preferably 500 kPa or less, and more preferably 200 kPa or less. The storage modulus (G'a85) of the photocurable adhesive layer (A) after curing at 85°C can be adjusted by the composition of the adhesive composition (A) (for example, Mw, Tg, BP equivalent of the BP polymer (A); weight fraction of the BP polymer (A); composition of the monomer components constituting the BP polymer (A) and the ethylenically unsaturated compound (B), type and amount of functional groups; type and amount of cross-linking agent), etc.
[0222] The storage modulus (G'a25) of the photocurable adhesive layer (A) after curing at 25°C is not particularly limited, and is, for example, preferably 70 kPa or more, more preferably greater than 100 kPa, more preferably 150 kPa or more, and further preferably 170 kPa or more. Such a configuration is preferred for achieving excellent processability of the photocurable adhesive layer (A) after curing. In addition, G'a25 is not particularly limited, and from the perspective of bonding reliability, is, for example, 5000 kPa or less, preferably 2500 kPa or less, and more preferably 1000 kPa or less. The storage modulus (G'a25) of the photocurable adhesive layer (A) after curing at 25°C can be adjusted by the composition of the adhesive composition (A) (for example, Mw, Tg, BP equivalent of the BP polymer (A); weight fraction of the BP polymer (A); composition of the monomer components constituting the BP polymer (A) and the ethylenically unsaturated compound (B), type and amount of functional groups; type and amount of crosslinking agent), etc.
[0223] The storage modulus (G'b25) of the photocurable adhesive layer (A) before curing at 25°C is not particularly limited, and is, for example, 300 kPa or less, preferably 250 kPa or less, and more preferably 200 kPa or less. Such a configuration is preferred for achieving excellent height difference absorption of the photocurable adhesive layer (A) before curing. In addition, G'b25 is not particularly limited, and from the viewpoint of bonding reliability, for example, it is preferably 10 kPa or more, more preferably 30 kPa or more, and further preferably 50 kPa or more. The storage modulus (G'b25) of the photocurable adhesive layer (A) before curing at 25°C can be adjusted by the composition of the adhesive composition (A) (for example, Mw and Tg of the BP polymer (A); the weight fraction of the BP polymer (A); the composition of the monomer components constituting the BP polymer (A) and the ethylenically unsaturated compound (B), the type and amount of the functional groups; the type and amount of the crosslinking agent), etc.
[0224] The ratio (G'a25 / G'b85) of the storage modulus (G'a25) of the adhesive layer A at 25°C after curing to the storage modulus (G'b85) of the photocurable adhesive layer (A) before curing at 85°C is not particularly limited, and is, for example, preferably 0.3 or more, more preferably 0.5 or more, more preferably 1 or more, more preferably greater than 3, preferably 3.5 or more, and more preferably 4 or more. Such a configuration is preferred from the perspective of being able to take into account both the excellent height difference absorption of the adhesive layer A before curing and the excellent processability of the adhesive layer A after curing. In addition, G'a25 / G'b85 is not particularly limited, and is, for example, 100 or less, preferably 50 or less, and more preferably 30 or less from the perspective of handling, operability, and bonding reliability. The ratio (G'a25 / G'b85) of the storage modulus (G'a25) of the cured adhesive layer A at 25°C to the storage modulus (G'b85) of the photocurable adhesive layer (A) before curing at 85°C can be adjusted by the composition of the adhesive composition (A) (for example, the Mw, Tg, and BP equivalent of the BP polymer (A); the weight fraction of the BP polymer (A); the composition of the monomer components constituting the BP polymer (A) and the ethylenically unsaturated compound (B), the type and amount of the functional groups; the type and amount of the cross-linking agent), etc.
[0225] The curing conditions in the above-mentioned "cured photocurable adhesive layer (A)" are not particularly limited, and preferably ultraviolet rays that allow the adhesive layer (A) to show transmittance. More preferably, ultraviolet rays have a wavelength of 200 to 400 nm, and even more preferably have a wavelength of less than 300 nm. As a light source for ultraviolet irradiation, for example, a high-pressure mercury lamp, a low-pressure mercury lamp, a microwave excitation lamp, a metal halide lamp, a chemical lamp, a black light lamp, or an LED can be used. In addition, the irradiation energy, irradiation time, and irradiation method of the radiation used for curing can be appropriately set as long as the photocurable adhesive layer (A) can be cured and will not cause adverse effects on the adherend. For example, when ultraviolet rays are used as the radiation used for curing, the irradiation amount (cumulative light amount) is preferably 1000 mJ / cm 2 ~10000mJ / cm 2 , more preferably 2000mJ / cm 2 ~4000mJ / cm 2 , more preferably 3000mJ / cm 2 .
[0226] In addition, the above-mentioned storage modulus is a value measured by dynamic viscoelasticity measurement.
[0227] [VOC emission]
[0228] The VOC (volatile organic compound) emission of the photocurable adhesive layer (A) is not particularly limited. The above-mentioned VOC emission can be, for example, less than 5000 μg / g, less than 3000 μg / g, or less than 1000 μg / g. In some embodiments, the VOC emission of the photocurable adhesive layer (A) is preferably less than 500 μg / g, more preferably less than 300 μg / g, and further preferably less than 100 μg / g. A photocurable adhesive layer (A) with a small VOC emission is low in odor and is preferred from the perspective of environmental hygiene. A small VOC emission of the photocurable adhesive layer (A) is also preferred from the perspective of suppressing foaming caused by volatile organic compounds (VOCs) in the photocurable adhesive layer (A) and low pollution. Regarding the VOC emission of the photocurable adhesive layer (A), an appropriate amount of the photocurable adhesive layer (A) (for example, about 1 mg to 2 mg) is used as a measurement sample and measured by the following method. It should be noted that the thickness of the measurement sample is preferably 1 mm or less.
[0229] [VOC measurement test]
[0230] Place the measurement sample in a 20 mL vial and cap it tightly. Next, heat the vial at 80°C for 30 minutes, and use a headspace autosampler (HSS) to inject 1.0 mL of the heated gas (sample gas) into a gas chromatography (GC) measuring device. Based on the obtained gas chromatogram, the amount of gas generated from the measurement sample is calculated in the form of n-decane conversion. Based on the obtained value, the VOC emission (μg / g) per 1 g of the measurement sample is calculated. It should be noted that the n-decane conversion regards the detection intensity of the generated gas obtained by GCMass as the detection intensity of n-decane, and is calculated by applying a pre-made standard curve for n-decane. The settings of HSS and GC are shown below.
[0231] HSS: Agilent Technologies, Model "7694"
[0232] Heating time: 30 minutes
[0233] Pressurization time: 0.12 minutes
[0234] Ring filling time: 0.12 minutes
[0235] Ring equilibration time: 0.05 minutes
[0236] Injection time: 3 minutes
[0237] Sample ring temperature: 160°C
[0238] Conveyor line temperature: 200°C
[0239] GC device: Agilent Technologies, model "6890"
[0240] Column: J&W capillary column manufactured by GL Science, trade name "DB-WAP" (inner diameter 0.533 mm × length 30 m, membrane thickness 1.0 μm)
[0241] Column temperature: 250°C (increase temperature from 40°C to 90°C at 10°C / min, then increase temperature to 250°C at 20°C / min, and hold for 5 minutes)
[0242] Column pressure: 24.3 kPa (constant flow mode)
[0243] Carrier gas: Helium (5.0mL / min)
[0244] Inlet: split (split ratio 12:1)
[0245] Inlet temperature: 250℃
[0246] Detector: FID
[0247] Detector temperature: 250°C
[0248] In general, volatile organic compounds that may be a factor in increasing the VOC emission of an adhesive include organic solvents (e.g., residues of organic solvents contained in the adhesive composition (A)), unreacted products of ethylenically unsaturated compounds contained in the adhesive composition (e.g., unpolymerized acrylic monomers, hereinafter referred to as "residual monomers"), etc. The photocurable adhesive layer (A) can suppress the content of such organic solvents and residual monomers to a level that satisfies any of the above-mentioned VOC emissions. The photocurable adhesive layer (A) has a structure that limits the amount of residual monomers, and can utilize the benzophenone structure of the BP polymer (A) to form new crosslinks in the system, thereby forming a photocured material with improved processability.
[0249] It should be noted that the VOC emission of the photocurable adhesive layer (A) disclosed herein is preferably as low as possible in principle, but from the practical viewpoints of productivity and cost, in some embodiments, the VOC emission may be, for example, 10 μg / g or more, 30 μg / g or more, 80 μg / g or more, 150 μg / g or more, or 200 μg / g or more.
[0250] The VOC emission of the photocurable adhesive layer (A) can be adjusted by the composition of the adhesive composition (A) (for example, the composition of the monomer components constituting the BP polymer (A) and the ethylenically unsaturated compound (B), the amount of the organic solvent), the curing conditions of the adhesive composition (A) (heating conditions, ultraviolet irradiation conditions), etc.
[0251] (Gel rate)
[0252] The gel fraction of the photocurable adhesive layer (A) is not particularly limited. From the viewpoint of the cohesiveness of the photocurable adhesive layer (A), the handleability of the adhesive sheet having the photocurable adhesive layer (A), etc., it is usually appropriate to be 5% or more, preferably 15% or more, 25% or more, or 35% or more. The gel fraction of the photocurable adhesive layer (A) is in principle 100% or less. In addition, from the viewpoint of the height difference absorption of the surface shape of the adherend, the gel fraction of the photocurable adhesive layer (A) is preferably less than 85%, less than 70%, less than 55%, or less than 40%.
[0253] The gel fraction was measured by the following method. That is, about 0.5 g of the sample was accurately weighed, and its weight was set as W1. The sample was wrapped in a porous PTFE (polytetrafluoroethylene) sheet, immersed in ethyl acetate at room temperature for 1 week and then dried, and the weight W2 of the component insoluble in ethyl acetate was measured, and W1 and W2 were substituted into the following formula to calculate the gel fraction.
[0254] Gel fraction (%) = W2 / W1×100;
[0255] As the porous PTFE sheet, a product of Nitto Denko Corporation, trade name "NITOFLON NTF1122" or an equivalent product thereof can be used.
[0256] In some embodiments of the photocurable adhesive layer (A), the photocurable adhesive layer (A) is irradiated with a high pressure mercury lamp at an illumination of 300 mW / cm 2 、Accumulated light intensity 10000mJ / cm 2 The gel fraction of the photocured material obtained by irradiating the photocured material with ultraviolet rays under the conditions of can be, for example, 70% or more, preferably 90% or more, 95% or more, or 98% or more. The gel fraction of the photocured material is in principle 100% or less. The gel fraction is measured according to the above method.
[0257] The gel fraction of the photocurable adhesive layer (A) can be adjusted by the composition of the adhesive composition (A) (for example, Mw, Tg, BP equivalent of the BP polymer (A); weight fraction of the BP polymer (A); composition of the monomer components constituting the BP polymer (A) and the ethylenically unsaturated compound (B), type and amount of functional groups; type and amount of the cross-linking agent), the adhesive composition (A), curing conditions of the photocurable adhesive layer (A) (heating conditions, ultraviolet irradiation conditions), etc.
[0258] The glass transition temperature (Tg) of the photocurable adhesive layer (A) is not particularly limited, but is preferably -60 to 20° C., more preferably -40 to 10° C., and further preferably -30 to 0° C. When the Tg is higher than 20° C., adhesive strength cannot be developed at room temperature.
[0259] The Tg is not particularly limited, and can be measured, for example, by using the adhesive layer as a sample for measurement by differential scanning calorimetry (DSC) in accordance with JIS K 7121. Specifically, for example, the measurement can be performed using a measuring apparatus "Q-2000" manufactured by TA Instruments under the conditions of -80°C to 80°C and a heating rate of 10°C / min.
[0260] The thickness of the photocurable adhesive layer (A) is not particularly limited and can be appropriately set in a manner that can fully seal the light-emitting elements arranged on the display panel described later. For example, the thickness of the photocurable adhesive layer (A) is adjusted in a manner that is 1.0 to 4.0 times, preferably 1.1 to 3.0 times, more preferably 1.2 to 2.5 times, and further preferably 1.3 to 2.0 times the height of the light-emitting element. By setting the above-mentioned thickness to more than 1.0 times, the photocurable adhesive layer (A) is easy to follow the height difference, and the height difference absorption is improved. In addition, by setting the above-mentioned thickness to less than 4.0, it is not easy to cause deformation of the photocurable adhesive layer (A), and the processability is improved.
[0261] The thickness of the photocurable adhesive layer (A) is, for example, about 10 to 500 μm, or may be more than 20 μm, more than 30 μm, more than 40 μm, or more than 50 μm. The thickness of the photocurable adhesive layer (A) may also be less than 400 μm, less than 300 μm, less than 250 μm, or less than 200 μm. By making the above-mentioned thickness more than 10 μm, the photocurable adhesive layer (A) easily follows the height difference portion, and the height difference absorption is improved. In addition, by making the above-mentioned thickness less than 500 μm, it is not easy to cause deformation of the photocurable adhesive layer (A), and the processability is improved.
[0262] The photocurable adhesive layer (A) exhibits excellent light-shielding properties against visible light, and thus can prevent reflection and gloss on the metal surface even when a metal adherend is laminated on the photocurable adhesive layer (A). The reflectivity in the visible light region of 5° regular reflection when a metal adherend is laminated on the photocurable adhesive layer (A) is preferably 50% or less, more preferably 30% or less, further preferably 15% or less, and particularly preferably 10% or less. The glossiness (based on JIS Z 8741-1997) when a metal adherend is laminated on the photocurable adhesive layer (A) is preferably 100% or less, more preferably 80% or less, further preferably 60% or less, and particularly preferably 50% or less.
[0263] In addition, copper, aluminum, stainless steel, etc. can be used as the above-mentioned metal adherend.
[0264] [Formation of Photocured Material]
[0265] The photocurable adhesive layer (A) can be photocrosslinked by irradiating ultraviolet rays containing wavelength components that can excite the benzophenone structure. It is preferred to use a light source that can irradiate ultraviolet rays containing components with a wavelength lower than 300nm. Examples of the light source include high-pressure mercury lamps, low-pressure mercury lamps, metal halide lamps, super UV lamps, etc., but are not limited to these. The light irradiated by the above light source may also contain components with a wavelength of more than 300nm.
[0266] It should be noted that as a light source capable of irradiating ultraviolet rays that do not contain a wavelength component (e.g., a component with a wavelength lower than 300 nm) that can excite a benzophenone structure or a small amount of such wavelength component, black light lamps, UV-LED lamps, etc. can be cited. These light sources can be preferably used as a light source for promoting the reaction (polymerization reaction or curing reaction) of an ethylenically unsaturated group by light irradiation performed in the presence of a benzophenone structure. In the ultraviolet irradiation for reacting an ethylenically unsaturated group, the above-mentioned photopolymerization initiator (C) can be used to promote the reaction.
[0267] The photocurable adhesive layer (A) may be a composition that is substantially free of a photopolymerization initiator that generates free radicals by absorbing light with a wavelength of more than 300 nm, for example, it may be a composition that is substantially free of a photopolymerization initiator that generates free radicals by absorbing visible light of more than 380 nm (especially more than 400 nm). This may be advantageous from the perspective of the optical properties of the photocurable adhesive layer (A). It should be noted that the photopolymerization initiator that does not generate free radicals by absorbing light with a wavelength of more than 300 nm refers to the photopolymerization initiator that does not contain a form that can generate the above-mentioned free radicals (a form having a part that is cleaved by the above-mentioned light), and the cleavage residue of the above-mentioned photopolymerization initiator may be allowed. A preferred embodiment of the photocurable adhesive layer (A) is substantially free of a photopolymerization initiator that contains a phosphorus element in the molecule. The photocurable adhesive layer (A) disclosed herein may be substantially free of any one of a photopolymerization initiator that contains a phosphorus element in the molecule and a cleavage residue of the photopolymerization initiator.
[0268] [Photocurable adhesive sheet (A)]
[0269] The photocurable pressure-sensitive adhesive sheet (A) has a photocurable pressure-sensitive adhesive layer (A).
[0270] As long as the photocurable adhesive sheet (A) has an adhesive surface formed by the surface of the photocurable adhesive layer (A), its form is not particularly limited. The photocurable adhesive sheet (A) can be a single-sided adhesive sheet with only one side as an adhesive surface, or a double-sided adhesive sheet with two sides as adhesive surfaces. In the case where the photocurable adhesive sheet A is a double-sided adhesive sheet, the photocurable adhesive sheet (A) can have a form in which two adhesive surfaces are provided by the photocurable adhesive layer (A), or a form in which one adhesive surface is provided by the photocurable adhesive layer (A) and another adhesive surface is provided by an adhesive layer (other adhesive layer) other than the photocurable adhesive layer (A). From the viewpoint of bonding adherends to each other, it is preferably a double-sided adhesive sheet, and more preferably a double-sided adhesive sheet in which both sides of the sheet are surfaces of the photocurable adhesive layer (A).
[0271] The photocurable adhesive sheet (A) may be an adhesive sheet without a substrate (substrate layer), i.e., a so-called "substrate-free type" adhesive sheet (sometimes referred to as a "substrate-free adhesive sheet"), or an adhesive sheet with a substrate (sometimes referred to as an "adhesive sheet with a substrate"). As the substrate-free adhesive sheet in the present invention, for example, there can be listed: a double-sided adhesive sheet consisting only of a photocurable adhesive layer (A), and a double-sided adhesive sheet formed of a photocurable adhesive layer (A) and other adhesive layers (adhesive layers other than the photocurable adhesive layer (A)). As the adhesive sheet with a substrate in the present invention, for example, there can be listed: a single-sided adhesive sheet having a photocurable adhesive layer (A) on one side of a substrate, a double-sided adhesive sheet having a photocurable adhesive layer (A) on both sides of a substrate, and a double-sided adhesive sheet having a photocurable adhesive layer (A) on one side of a substrate and other adhesive layers on the other side.
[0272] Among the above, from the viewpoint of improving optical properties such as transparency, a substrate-free adhesive sheet is preferred, and a double-sided adhesive sheet consisting of only a photocurable adhesive layer (A) and having no substrate (substrate-free double-sided adhesive sheet) is more preferred. In addition, when the photocurable adhesive sheet (A) is an adhesive sheet having a substrate, although there is no particular limitation, from the viewpoint of processability, a double-sided adhesive sheet having a photocurable adhesive layer (A) on both sides of the substrate (double-sided adhesive sheet with a substrate) is preferred.
[0273] It should be noted that the above-mentioned "substrate (substrate layer)" refers to the portion that is adhered to the adherend together with the adhesive layer when the photocurable adhesive layer (A) is used for (adhered to) the adherend (optical component, etc.), and does not include a release film (release film) that is peeled off when the adhesive sheet is used (adhered).
[0274] Photocurable adhesive sheet A is as described above, and can be an adhesive sheet with a substrate. As such substrate, various optical films such as plastic film, anti-reflection (AR) film, polarizing plate, phase difference plate, etc. can be listed. As the raw materials of the above-mentioned plastic film, for example, polyester resins such as polyethylene terephthalate (PET), acrylic resins such as polymethyl methacrylate (PMMA), polycarbonate, triacetyl cellulose (TAC), polysulfone, polyarylate, polyimide, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, ethylene-propylene copolymer, trade name "Arton" (cyclic olefin polymer, JSR Co., Ltd.), trade name "ZEONOR" (cyclic olefin polymer, Japan Zeon Co., Ltd.) and other cyclic olefin polymers and other plastic materials can be listed. It should be noted that these plastic materials can be used alone or in combination with more than 2 kinds.
[0275] The substrate is preferably transparent. The total light transmittance of the substrate in the visible light wavelength region (according to JIS K7361-1) is not particularly limited, but is preferably 85% or more, more preferably 88% or more. In addition, the haze of the substrate (according to JIS K7136) is not particularly limited, but is preferably 1.5% or less, more preferably 1.0% or less. Examples of such transparent substrates include PET films, non-oriented films such as "Arton" and "ZEONOR".
[0276] The thickness of the substrate is not particularly limited, and is preferably 12 to 75 μm. It should be noted that the substrate may have any form of a single layer or a multilayer. In addition, the surface of the substrate may be appropriately subjected to known and commonly used surface treatments such as anti-reflection treatment (AR treatment), anti-glare treatment and other anti-reflection treatments, corona discharge treatment, plasma treatment and other physical treatments, primer treatment and other chemical treatments.
[0277] As described above, the photocurable adhesive sheet (A) may have other adhesive layers (adhesive layers other than the adhesive layer A). The other adhesive layers are not particularly limited, and examples thereof include adhesive layers formed by known and commonly used adhesives such as urethane adhesives, acrylic adhesives, rubber adhesives, silicone adhesives, polyester adhesives, polyamide adhesives, epoxy adhesives, vinyl alkyl ether adhesives, and fluorine adhesives. It should be noted that the above adhesives may be used alone or in combination of two or more.
[0278] The photocurable pressure-sensitive adhesive sheet (A) may have other layers (eg, an intermediate layer, a primer layer, etc.) in addition to the photocurable pressure-sensitive adhesive layer (A), the substrate, and other pressure-sensitive adhesive layers, as long as the effects of the present invention are not impaired.
[0279] The photocurable adhesive sheet (A) may be provided with a release film (release film) on the adhesive surface until use. The form in which the adhesive surface of the photocurable adhesive sheet (A) is protected by the release film is not particularly limited, and may be a form in which two release films are used to protect each adhesive surface, or may be a form in which each adhesive surface is protected by a release film with both sides being release surfaces by being wound into a roll. The release film is used as a protective material for the adhesive layer and is peeled off when it is attached to the adherend. It should be noted that in the photocurable adhesive sheet (A), the release film also serves as a support for the adhesive layer. It should be noted that the release film may not necessarily be provided.
[0280] The thickness (total thickness) of the photocurable adhesive sheet (A) is not particularly limited, and is preferably 10 μm to 1 mm, more preferably 100 to 500 μm, and further preferably 150 to 350 μm. By making the thickness above 10 μm or more, the photocurable adhesive layer (A) can easily follow the height difference portion, and the height difference absorption can be improved. It should be noted that the thickness of the photocurable adhesive sheet (A) does not include the thickness of the release film.
[0281] The photocurable adhesive sheet (A) includes the photocurable adhesive layer (A) and thus has light absorptivity to visible light. The total light transmittance of the photocurable adhesive sheet (A) is, for example, 80% or less, or 70% or less, 60% or less, 50% or less, 40% or less, 30% or less, 20% or less, 10% or less, or 5% or less.
[0282] Since the photocurable adhesive sheet (A) has a photocurable adhesive layer (A), it has excellent height difference absorption before curing. For example, on the basis of a height difference of 5 to 10 μm, the height difference absorption is also excellent for a higher height difference of more than 40 μm. Furthermore, the height difference absorption is also excellent for a high height difference of more than 80 μm.
[0283] Furthermore, since the photocurable adhesive sheet (A) has the photocurable adhesive layer (A), it has excellent processability after curing, and can suppress adhesive deficiency during cutting and adhesive layer overflow and sagging from the edge during storage.
[0284] Furthermore, since the photocurable pressure-sensitive adhesive sheet (A) has the photocurable pressure-sensitive adhesive layer (A), it is also excellent in adhesion reliability.
[0285] Figures 1 to 3 This is a diagram (cross-sectional view) schematically showing one embodiment of the photocurable pressure-sensitive adhesive sheet (A) of the present invention.
[0286] One embodiment of the photocurable adhesive sheet (A) is shown in Figure 1. The photocurable adhesive sheet 1A is constituted in the form of a single-sided adhesive photocurable adhesive sheet, and the single-sided adhesive photocurable adhesive sheet includes: a photocurable adhesive layer 10 having one surface 10A serving as an adhesive surface (adhesive surface) to an adherend, and a substrate S1 laminated on the other surface 10B of the photocurable adhesive layer 10. The photocurable adhesive layer 10 is bonded to one surface S1A of the substrate S1. As the substrate S1, for example, a plastic film such as a polyester film can be used. The substrate S1 can be, for example, an optical film such as a polarizing plate or a covering member. In Figure 1 In the embodiment shown, the photocurable adhesive layer 10 has a single-layer structure. The adhesive sheet 1A before use (before being attached to an adherend) is, for example, Figure 1 As shown, the adhesive surface 10A may be protected by a release film S2 whose at least the adhesive layer side serves as a release surface (release surface), and the adhesive sheet 50 with a release film may be in the form. Alternatively, the second surface S1B (the surface on the opposite side to the first surface S1A, also referred to as the back surface) of the substrate S1 may serve as a release surface, and the adhesive surface 10A may be protected by being wound or laminated in a manner such that the adhesive surface 10A abuts against the second surface S1B of the substrate S1.
[0287] The release film is not particularly limited, and for example, a release film obtained by subjecting the surface of a film substrate such as a resin film or paper to a release treatment, a release film formed of a low-adhesive material such as a fluorine-based polymer (polytetrafluoroethylene, etc.) or a polyolefin-based resin (polyethylene, polypropylene, etc.), etc. can be used. For example, a release treatment agent such as an organosilicon-based or long-chain alkyl-based release treatment agent can be used in the above-mentioned release treatment. In some embodiments, a resin film subjected to a release treatment can be preferably used as the release film.
[0288] The photocurable adhesive sheet (A) may be a double-sided adhesive sheet without a substrate composed of the photocurable adhesive layer (A). Figure 2 As shown, the substrate-free double-sided adhesive sheet 1B can be in a form in which each surface 10A, 10B of the adhesive layer 10 is protected by a release film S3, S4 whose at least the adhesive layer side becomes a release surface (release surface) before use. Alternatively, the back side of the release film S4 (the surface on the opposite side to the adhesive side) becomes the release surface, and the adhesive surface 10A, 10B is protected by winding or stacking in a manner that the adhesive surface 10B abuts against the back side of the release film S4. Such a substrate-free double-sided adhesive sheet can be used, for example, by bonding a substrate to any surface of the adhesive layer.
[0289] The photocurable adhesive sheet (A) may be a constituent element of an optical member with an adhesive sheet in which an optical member is bonded to one surface of an adhesive layer. Figure 1 The photocurable adhesive sheet 1A shown may be Figure 3As shown, the optical member S5 is bonded to one surface 10A of the adhesive layer 10, which is a component of the optical member 100 with an adhesive sheet. The optical member may be, for example, a glass plate, a resin film, a metal plate, or an LED panel described later.
[0290] The photocurable adhesive layer (A) constituting the photocurable adhesive sheet (A) may be a cured layer of the corresponding adhesive composition (A). For example, the photocurable adhesive layer (A) may be formed by curing the adhesive composition (A) after imparting (e.g., applying) the adhesive composition (A) to an appropriate surface. The curing of the adhesive composition (A) may preferably be carried out by irradiation with active energy rays. As the active energy ray for forming the photocurable adhesive layer (A), it is preferably ultraviolet rays, more preferably ultraviolet rays that do not contain components with a wavelength of less than 300nm or components of the wavelength.
[0291] The adhesive composition (A) can be applied by using a conventional coating machine such as a gravure roll coater, a reverse roll coater, a lick roll coater, a dip roll coater, a rod coater, a knife coater, or a spray coater. In the photocurable adhesive sheet (A) having a substrate, as a method for providing the photocurable adhesive layer (A) on the substrate, a direct method of directly applying the adhesive composition (A) to the substrate to form the photocurable adhesive layer (A) can be used, or a transfer method of transferring the photocurable adhesive layer (A) formed on the release surface to the substrate can be used.
[0292] <Self-luminous display device>
[0293] The self-luminous display device of the fifth side of the present invention is a display device as follows: a large number of tiny light-emitting elements are arranged on a wiring substrate, and each light-emitting element selectively emits light through a light-emitting control means connected thereto, thereby directly displaying visual information such as text / images / videos on a display screen through the flashing of each light-emitting element. As self-luminous display devices, mini / micro LED display devices and organic EL (electroluminescent) display devices can be cited. The photocurable adhesive sheet A of the first side of the present invention is particularly suitable for the manufacture of mini / micro LED display devices.
[0294] Figure 4 It is a schematic diagram (cross-sectional view) showing an embodiment of a self-luminous display device (mini / micro LED display device) according to the fifth aspect of the present invention.
[0295] Figure 4In the embodiment, the mini / micro LED display device 200A is composed of the following components: a display panel on which a plurality of LED chips 23 are arranged on a single surface of a substrate 21 via a metal wiring layer 22, an adhesive layer 20 laminated on the display panel and sealing the metal wiring layer 22 and the plurality of LED chips 23, and a covering member 24 laminated on the upper part (image display side) of the adhesive layer 20. The covering member 24 is not particularly limited and can be composed of the same material as the above-mentioned "base material".
[0296] In the mini / micro LED display device 200A of this embodiment, a metal wiring layer 22 for transmitting a light emission control signal to each LED chip 23 is stacked on the substrate 21 of the display panel. The LED chips 23 emitting red (R), green (G), and blue (B) light are alternately arranged on the substrate 21 of the display panel with the metal wiring layer 22 interposed therebetween. The metal wiring layer 22 is formed of a metal such as copper, and reflects the light emitted by each LED chip 23, thereby reducing the image recognition. In addition, the light emitted by each LED chip 23 of each color of RGB is mixed, and the contrast is reduced.
[0297] In the mini / micro LED display device 200A of this embodiment, each LED chip 23 arranged on the display panel is sealed by an adhesive layer 20. The adhesive layer 20 is composed of a cured product of the photocurable adhesive layer (A) of the present invention. The adhesive layer 20 fully follows the minute height differences between the plurality of LED chips 23 and seals without gaps.
[0298] The adhesive layer 20 has sufficient light-shielding properties in the visible light region. The fine height differences between the LED chips 23 are sealed without gaps by the adhesive layer 20 with high light-shielding properties, thereby preventing reflection caused by the metal wiring layer 22, preventing color mixing between the LED chips 23, and improving contrast.
[0299] In addition, the adhesive layer 20 is a cured product of the photocurable adhesive layer (A), and thus has excellent processability, so that the adhesive layer 20 can be prevented from being insufficient during the cutting process of the mini / micro LED display device 200A of this embodiment, and from overflowing and sagging from the end during storage.
[0300] The self-luminous display device (mini / micro LED display device) of this embodiment may also have optical components other than the display panel, adhesive layer, and covering member. As the above-mentioned optical components, there is no particular limitation, and examples include polarizing plates, phase difference plates, anti-reflection films, viewing angle adjustment films, optical compensation films, etc. It should be noted that the optical components also include components (appearance films, decorative films, surface protection plates, etc.) that maintain the recognizability of display devices and input devices and perform decoration and protection functions.
[0301] The self-luminous display device (mini / micro LED display device) of the present embodiment is not particularly limited, but can be preferably manufactured by a method including the following steps.
[0302] (1) A step of laminating a photocurable adhesive layer (A) of a photocurable adhesive sheet (A) on a display panel having a plurality of light emitting elements arranged on one surface of a substrate, and sealing the light emitting elements with the photocurable adhesive layer (A).
[0303] (2) A step of curing the photocurable adhesive layer (A) by irradiating it with ultraviolet rays.
[0304] Figure 5 FIG. 1 is a diagram schematically showing the steps of one embodiment of a method for manufacturing a self-luminous display device (mini / micro LED display device) according to the fifth aspect of the present invention. Figure 5 As shown in (a), a display panel using the photocurable adhesive sheet 1C of the fourth aspect of the present invention and a plurality of light emitting elements (LED chips) 23 arranged on one surface of a substrate 21 via a metal wiring layer 22 is provided.
[0305] In this embodiment, the photocurable adhesive sheet 1C is composed of a photocurable adhesive layer 10 and a cover member 24. In this embodiment, the photocurable adhesive sheet 1C has a cover member 24, but it is also possible not to have a cover member 24. The cover member 24 is not particularly limited and can be composed of the same material as the above-mentioned "base material" or a release film (release film).
[0306] Then, if Figure 5 As shown in (b), the main surface 10A of the non-laminated covering member 24 in the photocurable adhesive layer 10 of the photocurable adhesive sheet 1C is laminated on the surface of the display panel where a plurality of LED chips are arranged, and the LED chip 23 and the metal wiring layer 22 are sealed by the photocurable adhesive layer 10. The lamination can be performed by a known method, for example, under heating and pressurizing conditions using an autoclave. The photocurable adhesive layer 10 of the photocurable adhesive sheet 1C has high fluidity and shows excellent height difference absorption. Therefore, the photocurable adhesive layer 10 is sealed in a manner that fills the height difference between the metal wiring layer 22 and the plurality of LED chips 23 without a gap.
[0307] Then, if Figure 5As shown in (c), the photocurable adhesive layer 10 is irradiated with ultraviolet rays to be cured. By irradiation with ultraviolet rays, the benzophenone structure contained in the photocurable adhesive layer 10 is excited, thereby forming a cross-linked structure by utilizing the abstraction reaction of hydrogen radicals, and starting the curing reaction. As ultraviolet rays, there is no particular limitation as long as the benzophenone structure is excited to cure the photocurable adhesive layer 10, and ultraviolet rays that are transparent to the photocurable adhesive layer 10 are preferably used. That is, the photocurable adhesive layer 10 has a high light-shielding property to visible light and a high transmittance to ultraviolet rays, so the photocurable adhesive layer 10 can be cured by ultraviolet rays. Figure 5 (c) is an embodiment in which the photocurable adhesive layer 10 is irradiated with ultraviolet rays U to be cured.
[0308] As the ultraviolet rays, ultraviolet rays having a wavelength of 200 to 400 nm are preferred, and ultraviolet rays having a wavelength of less than 300 nm are more preferred.
[0309] As a light source for ultraviolet irradiation, for example, a high-pressure mercury lamp, a low-pressure mercury lamp, a microwave excitation lamp, a metal halide lamp, a chemical lamp, a black light lamp, or an LED can be used. In addition, the ultraviolet irradiation time and irradiation method can be appropriately set as long as the photocurable adhesive layer 10 can be cured without causing adverse effects on the display panel, and the photocurable adhesive layer 10 is cured and shows sufficient processability. For example, the ultraviolet irradiation amount (cumulative light amount) is preferably 1000mJ / cm 2 ~10000mJ / cm 2 , more preferably 2000mJ / cm 2 ~4000mJ / cm 2 , more preferably 3000mJ / cm 2 .
[0310] By curing the photocurable adhesive layer 10, as Figure 5 As shown in (d), a self-luminous display device (mini / micro LED display device) 200B can be obtained. Figure 5 In (d), the adhesive layer 20 is an adhesive layer formed by curing the photocurable adhesive layer 10. The self-luminous display device (mini / micro LED display device) 200B is an embodiment of an example of a self-luminous display device (mini / micro LED display device) of the fifth side of the present invention.
[0311] The processability of the adhesive layer 20 is improved, and the adhesive shortage during cutting and the overflow and sagging of the adhesive layer from the end during storage can be suppressed. In addition, the adhesive layer 20 can suppress the generation of gases such as carbon dioxide caused by heating of the display panel, prevent the generation of bubbles, and improve the bonding reliability.
[0312] Example
[0313] The present invention will be described in more detail below based on examples, but the present invention is not limited to these examples.
[0314] [Example 1]
[0315] (Preparation of Adhesive Composition)
[0316] In a separable flask equipped with a thermometer, a stirrer, a reflux condenser, and a nitrogen inlet tube, an acrylic copolymer having a benzophenone structure in the side chain (manufactured by BASF, trade name "acResin A260UV", Tg: -39°C, Mw: 19×10 4 Adhesive composition A was prepared by mixing 50 parts by weight of butyl acrylate (BA), 26 parts by weight of N-vinyl-2-pyrrolidone (NVP), 16 parts by weight of isobornyl acrylate (IBXA) and 0.2 parts by weight of a photopolymerization initiator having an absorption peak in the wavelength range of 300 nm to 500 nm (manufactured by IGM Regins, trade name "Omnirad 184").
[0317] (Preparation of black adhesive composition)
[0318] 0.5 parts by weight of a 20% dispersion of a black pigment ("9256BLACK" manufactured by TOKUSHIKI) was added to 100 parts by weight of the above-mentioned adhesive composition A to prepare a black adhesive composition B1.
[0319] (Production of Photocurable Adhesive Sheet)
[0320] The black adhesive composition B1 prepared above was applied to the release surface of a release film R1 (MRF#38, manufactured by Mitsubishi Resins Co., Ltd.) with a thickness of 38 μm, which was used as the release surface on one side of the polyester film, and the release film R2 (MRE#38, manufactured by Mitsubishi Resins Co., Ltd.) which was used as the release surface on one side of the polyester film was covered to block the air. A black light lamp (manufactured by Toshiba Corporation, trade name FL15BL) was used from one side of the laminate to illuminate the laminate at an illumination of 5 mW / cm 2 、Accumulated light quantity 1300mJ / cm 2 Thus, a photocurable adhesive sheet D1 having a thickness of about 100 μm and a photocurable adhesive layer C1 of the black adhesive composition B1 and sandwiched between the release films R1 and R2 was obtained as a substrate-free double-sided adhesive sheet.
[0321] The illuminance value of the black light lamp is a value measured by an industrial UV inspection device (manufactured by TOPCON, trade name: UVR-T1, light receiving unit model UD-T36) having a peak sensitivity wavelength of about 350 nm.
[0322] [Example 2]
[0323] A black adhesive composition B2 is prepared by adding 1 part by weight of a 20% dispersion of a black pigment ("9256BLACK" manufactured by TOKUSHIKI) to 100 parts by weight of the adhesive composition A. In addition, a photocurable adhesive sheet D2 having a thickness of about 100 μm and sandwiched between the above-mentioned release films R1 and R2 is obtained in the form of a substrate-free double-sided adhesive sheet by the same method as in Example 1. The photocurable adhesive layer C2, which is a cured product of the above-mentioned black adhesive composition B2, is sandwiched by the above-mentioned release films R1 and R2.
[0324] [Example 3]
[0325] A black adhesive composition B3 is prepared by adding 2 parts by weight of a 20% dispersion of a black pigment ("9256BLACK" manufactured by TOKUSHIKI) to 100 parts by weight of the adhesive composition A. In addition, a photocurable adhesive sheet D3 having a thickness of about 100 μm and sandwiched between the above-mentioned release films R1 and R2 is obtained in the form of a substrate-free double-sided adhesive sheet by the same method as in Example 1. The photocurable adhesive layer C3 having a thickness of about 100 μm and being a cured product of the above-mentioned black adhesive composition B3 is obtained.
[0326] [Example 4]
[0327] A black adhesive composition B4 is prepared by adding 4 parts by weight of a 20% dispersion of a black pigment ("9256BLACK" manufactured by TOKUSHIKI) to 100 parts by weight of the adhesive composition A. In addition, a photocurable adhesive sheet D4 having a thickness of about 100 μm and sandwiched by the above-mentioned release films R1 and R2 is obtained in the form of a substrate-free double-sided adhesive sheet by the same method as in Example 1.
[0328] [Comparative Example 1]
[0329] No black pigment is added to 100 parts by weight of the adhesive composition A. In addition, a photocurable adhesive sheet D5 having a thickness of about 100 μm and sandwiched between the above-mentioned peeling films R1 and R2 is obtained in the form of a substrate-free double-sided adhesive sheet by the same method as in Example 1.
[0330] [Comparative Example 2]
[0331] (Preparation of prepolymer)
[0332] In a separable flask equipped with a thermometer, a stirrer, a reflux condenser, and a nitrogen inlet tube, 67 parts by weight of butyl acrylate (BA), 14 parts by weight of cyclohexyl acrylate (CHA), 19 parts by weight of 4-hydroxybutyl acrylate (4-HBA), 0.09 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name "Irgacure 184"), and 0.09 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name "Irgacure 651") were added as monomer components, and nitrogen was passed through the flask, and nitrogen substitution was performed for about 1 hour while stirring. Then, the flask was heated at 5 mW / cm 2 The polymerization was carried out by irradiating UVA, and the reaction rate was adjusted to 5 to 15% to obtain an acrylic prepolymer solution.
[0333] (Preparation of Adhesive Composition)
[0334] To the acrylic prepolymer solution A obtained above (the total amount of the prepolymer was 100 parts by weight), 9 parts by weight of 2-hydroxyethyl acrylate (HEA), 8 parts by weight of 4-hydroxybutyl acrylate (4-HBA), 0.02 parts by weight of dipentaerythritol hexaacrylate (manufactured by Shin-Nakamura Industrial Chemical, trade name "KAYARAD DPHA") as a multifunctional monomer, 0.35 parts by weight of 3-glycidoxypropyltrimethoxysilane as a silane coupling agent, and 0.45 parts by weight of a polymerization initiator ("Irgacure 651" manufactured by BASF) were added to obtain an adhesive composition.
[0335] (Preparation of black adhesive composition)
[0336] To 100 parts by weight of the above-mentioned adhesive composition, 5.8 parts by weight of a 20% dispersion of a black pigment ("9256BLACK" manufactured by TOKUSHIKI) and 0.2 parts by weight of an additional photopolymerization initiator ("Irgacure 651" manufactured by BASF) were added to obtain a black adhesive composition.
[0337] (Manufacturing of adhesive sheet)
[0338] The black adhesive composition prepared above was applied to the release surface of a release film R1 (MRF#38, manufactured by Mitsubishi Resins Co., Ltd.) with a thickness of 38 μm, which was used as the release surface on one side of the polyester film, and the release film R2 (MRE#38, manufactured by Mitsubishi Resins Co., Ltd.) which was used as the release surface on one side of the polyester film was covered to block the air. A black light lamp (manufactured by Toshiba Corporation, trade name FL15BL) was used from one side of the laminate to illuminate the laminate at an illumination of 5 mW / cm 2 、Accumulated light quantity 1300mJ / cm 2Thus, a double-sided adhesive sheet without substrate was obtained in which an adhesive layer having a thickness of about 50 μm, which was a cured product of the black adhesive composition, was sandwiched between the release films R1 and R2.
[0339] [Example 5]
[0340] (Preparation of black adhesive composition)
[0341] To 100 parts by weight of the adhesive composition prepared in Comparative Example 2, 4 parts by weight of a 20% dispersion of a black pigment ("9256BLACK" manufactured by TOKUSHIKI), 0.2 parts by weight of an additional photopolymerization initiator ("Irgacure 651" manufactured by BASF), and 1 part of 4-acryloxybenzophenone manufactured by Ark Pharm were added to obtain a black adhesive composition.
[0342] (Production of Photocurable Adhesive Sheet)
[0343] The black adhesive composition prepared above was applied to the release surface of a release film R1 (MRF#38, manufactured by Mitsubishi Resins Co., Ltd.) with a thickness of 38 μm, which was used as the release surface on one side of the polyester film, and the release film R2 (MRE#38, manufactured by Mitsubishi Resins Co., Ltd.) which was used as the release surface on one side of the polyester film was covered to block the air. A black light lamp (manufactured by Toshiba Corporation, trade name FL15BL) was used from one side of the laminate to illuminate the laminate at an illumination of 5 mW / cm 2 、Accumulated light quantity 1300mJ / cm 2 Thus, a double-sided adhesive sheet without substrate was obtained, in which an adhesive layer having a thickness of about 100 μm, which was a cured product of the black adhesive composition, was sandwiched between the release films R1 and R2.
[0344] The illuminance value of the black light lamp is a value measured by an industrial UV inspection device (manufactured by TOPCON, trade name: UVR-T1, light receiving unit model UD-T36) having a peak sensitivity wavelength of about 350 nm.
[0345] [Example 6]
[0346] A photocurable adhesive sheet was prepared in the same manner as in Example 5 except that 4-acryloxybenzophenone was changed to 2 parts.
[0347] (evaluate)
[0348] The following evaluations were performed using the PSA sheets obtained in the above Examples and Comparative Examples. The evaluation methods are shown below. The results are shown in Table 1.
[0349] [Evaluation of transmittance]
[0350] The release film on one side of the adhesive sheet was peeled off, and the alkali-free glass was bonded to the exposed side. Then, the release film on the other side of the adhesive sheet was peeled off to obtain a sample in which the adhesive sheet was bonded to the alkali-free glass plate.
[0351] The total light transmittance was measured using a haze meter (manufactured by Murakami Color Science Laboratory Co., Ltd., trade name “HN-150”) according to the method specified in JIS K7361.
[0352] [Evaluation of storage modulus]
[0353] The evaluation was performed using ARES GII manufactured by TA Instruments.
[0354] The adhesive sheet stacked to a thickness of about 1 mm was clamped between 8 mm parallel plates, and the storage modulus G' at 10°C, 25°C and 85°C was read when the measurement was performed from -50°C to 100°C with an initial strain of 1%, a frequency of 1 Hz, and a heating rate of 5°C / min. This was taken as the storage modulus G' before curing (G'b10, G'b25, G'b85).
[0355] Regarding the storage modulus G' after curing, the cumulative light intensity is 3000mJ / cm 2 The PSA sheets sandwiched between release films were irradiated with a high pressure mercury lamp to obtain a sheet having a thickness of about 1 mm and evaluated in the same manner as above as the storage modulus G' (G'a10, G'a25, G'a85) after curing.
[0356] This integrated light quantity is a value measured by an industrial UV inspection device (manufactured by TOPCON, trade name: UVR-T1, light receiving unit model UD-T36) having a peak sensitivity wavelength of about 350 nm.
[0357] In addition, since the pressure-sensitive adhesive sheet of Comparative Example 2 did not show photocurability, the storage modulus G′ after curing was not evaluated.
[0358] [Evaluation of height difference followability]
[0359] (Production of uneven adherends)
[0360] After bonding the laminate of TAC film (thickness 60μm) and adhesive (thickness 20μm) to a 45mm×50mm glass plate, a CO2 laser (wavelength 10.6μm / laser diameter 0μm) was used to perform linear etching processing on the central 10mm×10mm range at a vertical spacing of 150μm / lateral spacing of 225μm, thereby obtaining an adherend A in which the TAC film and adhesive layer were processed into a grid-like concave-convex shape.
[0361] The adherend A simulates an LED panel in which a plurality of LED films are arranged on a substrate.
[0362] (Manufacturing of adhesive sheet)
[0363] Two adhesive sheets prepared in Examples 1 to 4 and Comparative Example 1 were stacked to a thickness of about 200 μm. Five adhesive sheets prepared in Comparative Example 2 were stacked to a thickness of about 250 μm. The release film on one side of the stacked adhesive sheets was peeled off, and a 75 μm thick PET film was bonded to the exposed side.
[0364] (Vacuum bonding)
[0365] Using a vacuum laminating device (SE340aaH manufactured by CRIMB Products), the adhesive surface exposed by peeling off the release film on the other side of the laminated adhesive sheet obtained above was laminated to the processed surface of the adherend A with a precision within the processing range that the adhesive sheet can completely cover the adherend A, and evaluation samples consisting of PET film / laminated adhesive sheet / adherend A were obtained. Furthermore, an autoclave treatment (under conditions of 50°C / 0.5MPa for 60 minutes) was performed to make them adhere closely.
[0366] (Evaluation of height difference followability)
[0367] In the evaluation samples, the area of the white portion was calculated by taking pictures with a fixed-point camera to evaluate the step followability, utilizing the property that when the pressure-sensitive adhesive sheet can follow the uneven pattern, the processed portion of the adherend A is recognized as transparent, and the portion that cannot follow is recognized as white.
[0368] Height difference tracking property (%) = 100 - {[Area of white part during evaluation] / [Area of white part before lamination = 1 cm 2 ]×100}
[0369] [Evaluation of processability]
[0370] (Preparation of Laminated Product for Processability Evaluation)
[0371] The release film of the laminated adhesive sheet produced in the evaluation of the height difference followability was peeled off and attached to the fr-4 substrate (thickness 1.2 mm) manufactured by MISUMI Corporation. After autoclaving (15 minutes at 50°C / 0.5 MPa), Examples 1 to 4 and Comparative Example 1 showing photocurability were irradiated with ultraviolet light. The ultraviolet light irradiation conditions were set to a high-pressure mercury lamp and a cumulative light intensity of 3000 mJ / cm 2 The accumulated light amount is a value measured by an industrial UV inspection device (manufactured by TOPCON, trade name: UVR-T1, light receiving unit model: UD-T36) having a peak sensitivity wavelength of about 350 nm.
[0372] (Processing)
[0373] The obtained laminate for processability evaluation was cut using DTF6450 manufactured by Disco Co. The cutting conditions were blade type P1A861 (abrasive grain #400), spindle 30 krpm, speed 30 mm / s, and cooling water 1 L / min.
[0374] (Evaluation of processability)
[0375] The cut edge was observed from the laminated pressure-sensitive adhesive sheet side using a stereo microscope, and the processability was evaluated based on the amount of adhesive overflow from the cut edge. The evaluation criteria were as follows.
[0376] ○: 0~150μm
[0377] △: 150~200μm
[0378] ×: 200 μm or more
[0379] [Evaluation of reflectivity]
[0380] A plate is prepared by laminating a black acrylic plate with aluminum foil. The release film on one side of the adhesive sheets prepared in Examples 1 to 4 and Comparative Examples 1 and 2 is peeled off, and a PET film with a thickness of 75 μm is adhered to the exposed side. The release film on the other side is peeled off, and the exposed adhesive surface is laminated on the aluminum foil side of the above-mentioned plate as a sample. For the obtained sample, the PET film is set to the light source side in a spectrophotometer U4100 (manufactured by Hitachi High-Technologies Corporation), and the reflectivity (%) in the visible light region of 5° regular reflection is measured.
[0381] [Table 1]
[0382]
[0383] Examples 1 to 6, which are photocurable adhesive sheets, show excellent height difference tracking (height difference absorption) and processability, and the transmittance and reflectivity are also suppressed. When used as sealing materials for LED panels, excellent anti-reflection effects and improved contrast can be expected. On the other hand, although Comparative Example 1, which is a photocurable adhesive sheet but does not contain a colorant, shows excellent height difference tracking (height difference absorption) and processability, the transmittance and reflectivity are high. When used as a sealing material for LED panels, anti-reflection effects and improved contrast cannot be expected. Comparative Example 2, which is an adhesive sheet containing a colorant but not showing photocurability, shows excellent height difference tracking (height difference absorption), but has poor processability.
[0384] The following are additional notes on variations of the present invention.
[0385] [Supplementary Note 1] An adhesive composition comprising a colorant and a polymer (A) having a benzophenone structure in a side chain,
[0386] The maximum value of the transmittance of the adhesive composition at a wavelength of 200 to 400 nm is greater than the maximum value of the transmittance at a wavelength of 400 to 700 nm.
[0387] [Supplementary Note 2] An adhesive composition comprising a colorant and a mixture of monomer components constituting a polymer (A) having a benzophenone structure in a side chain or a partial polymer of a mixture of monomer components constituting a polymer (A) having a benzophenone structure in a side chain,
[0388] The maximum value of the transmittance of the adhesive composition at a wavelength of 200 to 400 nm is greater than the maximum value of the transmittance at a wavelength of 400 to 700 nm.
[0389] [Supplementary Note 3] The adhesive composition according to Supplementary Note 1 or 2, wherein the colorant has a maximum value of transmittance at a wavelength of 200 to 400 nm that is greater than a maximum value of transmittance at a wavelength of 400 to 700 nm.
[0390] [Appendix 4] The adhesive composition according to any one of Appendices 1 to 3, further comprising an ethylenically unsaturated compound (B).
[0391] [Appendix 5] The adhesive composition according to any one of Appendices 1 to 4, further comprising a photopolymerization initiator (C) that absorbs ultraviolet rays having a wavelength of 300 nm to 500 nm to generate radicals.
[0392] [Appendix 6] A photocurable adhesive layer, which is an adhesive layer formed from a cured product of the adhesive composition described in any one of Appendices 1 to 5,
[0393] The cured product is a cured product in which the benzophenone structure of the polymer (A) having a benzophenone structure in a side chain remains.
[0394] [Supplementary Note 7] The photocurable adhesive layer according to Supplementary Note 6, wherein the maximum value of the transmittance at a wavelength of 200 to 400 nm is larger than the maximum value of the transmittance at a wavelength of 400 to 700 nm.
[0395] [Supplementary Note 8] The photocurable adhesive layer according to Supplementary Note 6 or 7, wherein the storage modulus (G'b85) of the photocurable adhesive layer at 85° C. before curing is less than 65 kPa.
[0396] [Note 9] A photocurable adhesive layer according to any one of Notes 6 to 8, wherein the storage modulus (G'a10) of the photocurable adhesive layer at 10°C after curing and the storage modulus (G'b85) of the photocurable adhesive layer at 85°C before curing satisfy the following relationship (1).
[0397] 2.8 <G'a10 / G'b85 (1)
[0398] [Appendix 10] The photocurable adhesive layer according to any one of Appendices 6 to 9, wherein the storage modulus (G'a10) of the photocurable adhesive layer at 10° C. after curing is 90 kPa or more.
[0399] [Supplement 11] The photocurable adhesive layer according to any one of Supplements 6 to 10, wherein the curing is based on a wavelength of less than 300 nm and a cumulative light amount of 3000 mJ / cm 2 Curing by ultraviolet radiation.
[0400] [Appendix 12] A photocurable adhesive sheet comprising the photocurable adhesive layer according to any one of Appendices 6 to 11.
[0401] [Supplementary Note 13] A self-luminous display device comprising:
[0402] A display panel having a plurality of light emitting elements arranged on one surface of a substrate, and
[0403] The photocurable adhesive sheet according to Supplementary Note 12,
[0404] The light emitting element of the display panel is sealed by the photocurable adhesive layer of the photocurable adhesive sheet.
[0405] The aforementioned photocurable adhesive layer is cured.
[0406] [Supplement 14] The self-luminous display device according to Supplement 13, wherein the display panel is an LED panel in which a plurality of LED chips are arranged on a single surface of a substrate.
[0407] [Supplement 15] A method for manufacturing a self-luminous display device according to Supplement 13 or 14, comprising the following steps:
[0408] A step of laminating the photocurable adhesive layer of the photocurable adhesive sheet described in Supplementary Note 12 on a display panel having a plurality of light emitting elements arranged on one side of a substrate, and sealing the light emitting elements with the photocurable adhesive layer; and
[0409] A step of curing the photocurable adhesive layer by irradiating it with ultraviolet rays.
[0410] [Supplementary Note 16] The manufacturing method according to Supplementary Note 15, wherein the ultraviolet rays have a wavelength of less than 300 nm.
[0411] Industrial Applicability
[0412] The photocurable adhesive sheet of the present invention is suitable for sealing light-emitting elements of self-luminous display devices such as mini / micro LEDs.
[0413] Description of Reference Numerals
[0414] 1A~1C Light-curing adhesive sheet
[0415] 10 Photocurable adhesive layer
[0416] 10A One surface (bonding surface)
[0417] 10B Another Surface
[0418] S1 Substrate
[0419] S1A Side 1
[0420] S1B Second side (back side)
[0421] S2~S4 peeling film
[0422] S5 Optics
[0423] 50 Adhesive sheet with release film
[0424] 100 Components with adhesive sheets
[0425] 200A, 200B Self-luminous display device (mini / micro LED display device)
[0426] 20 Adhesive layer (after curing)
[0427] 21 substrate
[0428] 22 Metal wiring layer
[0429] 23. Light-emitting element (LED chip)
[0430] 24 Covering components
Claims
1. An adhesive composition comprising a colorant, a polymer (A) having a benzophenone structure in a side chain, and an ethylenically unsaturated compound (B), The maximum transmittance of the adhesive composition at a wavelength of 200 to 400 nm is greater than the maximum transmittance at a wavelength of 400 to 700 nm. The ethylenically unsaturated compound (B) includes an alkyl (meth)acrylate having an alkyl group at the ester terminal.
2. An adhesive composition comprising a colorant, a mixture of monomer components constituting a polymer (A) having a benzophenone structure in a side chain or a partially polymerized product of a mixture of monomer components constituting a polymer (A) having a benzophenone structure in a side chain, and an ethylenically unsaturated compound (B), The maximum transmittance of the adhesive composition at a wavelength of 200 to 400 nm is greater than the maximum transmittance at a wavelength of 400 to 700 nm. The ethylenically unsaturated compound (B) includes an alkyl (meth)acrylate having an alkyl group at the ester terminal.
3. The adhesive composition according to claim 1 or 2, in, The colorant is a colorant whose maximum value of transmittance at a wavelength of 200 to 400 nm is greater than the maximum value of transmittance at a wavelength of 400 to 700 nm. 4 . The adhesive composition according to claim 1 , further comprising a photopolymerization initiator (C) that absorbs ultraviolet rays having a wavelength of 300 nm to 500 nm to generate radicals.
5. A photocurable adhesive layer, which is an adhesive layer formed from a cured product of the adhesive composition according to any one of claims 1 to 4, The cured product is a cured product in which the benzophenone structure of the polymer (A) having a benzophenone structure in a side chain remains. 6 . The photocurable adhesive layer according to claim 5 , wherein the maximum value of the transmittance at a wavelength of 200 to 400 nm is greater than the maximum value of the transmittance at a wavelength of 400 to 700 nm.
7. The photocurable adhesive layer according to claim 5 or 6, in, The storage modulus (G'b85) of the photocurable adhesive layer at 85° C. before curing is less than 65 kPa.
8. The photocurable adhesive layer according to claim 5 or 6, in, The storage modulus (G'a10) of the photocurable adhesive layer at 10°C after curing and the storage modulus (G'b85) of the photocurable adhesive layer at 85°C before curing satisfy the following relationship (1): 2.8 <G'a10 / G'b85 (1)。 9. The photocurable adhesive layer according to claim 5 or 6, in, The storage modulus (G'a10) of the photocurable adhesive layer after curing at 10° C. is 90 kPa or more.
10. The photocurable adhesive layer according to claim 5 or 6, in, The curing is based on a wavelength below 300nm and a cumulative light amount of 3000mJ / cm 2 Curing by ultraviolet radiation. 11 . A photocurable adhesive sheet comprising the photocurable adhesive layer according to claim 5 .
12. A self-luminous display device, comprising: A display panel having a plurality of light emitting elements arranged on one surface of a substrate, and The photocurable adhesive sheet according to claim 11, The light-emitting element of the display panel is sealed by the photo-curable adhesive layer of the photo-curable adhesive sheet. The photocurable adhesive layer is cured.
13. The self-luminous display device according to claim 12, in, The display panel is an LED panel in which a plurality of LED chips are arranged on a single surface of a substrate.
14. A method for manufacturing a self-luminous display device according to claim 12 or 13, comprising the following steps: A step of laminating the photocurable adhesive layer of the photocurable adhesive sheet according to claim 11 on a display panel having a plurality of light emitting elements arranged on one surface of a substrate, and sealing the light emitting elements with the photocurable adhesive layer; and A step of curing the photocurable adhesive layer by irradiating it with ultraviolet rays.
15. The manufacturing method according to claim 14, in, The ultraviolet rays are ultraviolet rays with a wavelength below 300 nm.