Preparation method and application of intercalation-coated composite modified positive electrode material
By introducing metal ions and conductive carbon materials into the V2O5 positive electrode material, the interlayer-covered composite modified structure is formed, which solves the diffusion and stability of layered vanadium-based oxides in zinc-ion batteries, and significantly improves the battery capacity and cycle life.
Patent Information
- Application Number
- CN202310193309.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-23
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2043-02-23
AI Technical Summary
The application of layered vanadium-based oxide positive electrode materials in aqueous zinc ion batteries is limited by slow Zn2+ diffusion and structural instability. Traditional modification methods such as carbon coating and metal ion doping have limited effects, resulting in lower capacity and poor circulation. Stablize.
The preparation method of interlayer-coated composite modified cathode material is adopted. By introducing metal ions into the V2O5 layers and covering conductive carbon materials, the distance between layers is expanded, the electrostatic interaction between zinc ions is reduced, and the conductivity of the material is improved. rate and structural stability.
It effectively improves the capacity and cycle life of the battery. By regulating the amount of metal ion intercalation layer and the amount of conductive carbon material coating, the electrochemical performance of the material is optimized and the service life of the battery is extended.
Smart Images

Figure CN115995543B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of an intercalation-coated composite modified positive electrode material, belonging to the technical field of aqueous zinc ion batteries. Background Art
[0002] In order to alleviate the shortage of fossil energy and the environmental pollution caused by its use, and to improve the utilization efficiency of clean renewable energy, large-scale energy storage technology, especially electrochemical energy storage technology, has developed rapidly in recent years. Aqueous zinc-ion batteries (AZIBs) have great potential for large-scale electrical energy storage applications in the future due to their cost-effectiveness, environmental friendliness, intrinsic safety and highly competitive gravimetric energy density. In view of this, a lot of research work has been carried out on the design and development of high-performance AZIBs. Among them, the development of cathode materials with high voltage, fast kinetics and long cycle stability is a necessary link to improve the competitiveness of AZIBs in the field of energy storage.
[0003] Layered vanadium-based oxides are considered promising cathode materials for aqueous zinc-ion batteries (AZIBs) due to their open-framework crystal structures and high theoretical specific capacities. 2+ Diffusion and poor structural stability limit their widespread application in AZIBs. At present, the modification of V2O5 materials is mainly to carbon-coat them, and most studies use graphene as the coating material. Chinese patent CN109817943A discloses a carbon-coated V2O5 positive electrode material and a preparation method thereof. The method requires a V2O5 positive electrode material with a carbon-coated structure obtained by hydrothermal annealing and secondary high-temperature annealing. The preparation process is complicated, and the cycle stability of the lithium battery assembled therein is better than that of the unmodified V2O5, but its specific capacity is lower. In addition, metal ion doping is another commonly used modification strategy. Chinese patent CN 103268964 A discloses a sodium ion-doped V2O5 prepared by a liquid phase method and a solid phase sintering method for use in aqueous lithium-ion batteries. Unlike traditional lithium-ion batteries, it has a higher discharge capacity under high-rate discharge, but its capacity decays quickly and the cycle is unstable. Summary of the invention
[0004] In view of the shortcomings of the current layered vanadium-based oxide positive electrode materials, the present invention provides a preparation method and application of an intercalation-coated composite modified positive electrode material. By introducing metal ions into the V2O5 interlayer and coating the conductive carbon material, on the one hand, the introduced metal ions can effectively expand the interlayer distance, and the introduced metal ions can play a supporting role in the V2O5 structure interlayer, while maintaining the stability of the V2O5 structure, effectively reducing the electrostatic interaction between the zinc ion embedding / de-embedded and the matrix V2O5 during the charge and discharge process, and is also beneficial to the storage and diffusion of zinc ions. On the other hand, the coated conductive carbon material can not only further increase the conductivity, but also stabilize the material structure. The above-mentioned composite modified positive electrode material is applied to aqueous batteries to effectively improve the battery capacity and cycle life.
[0005] The objectives of the present invention are achieved through the following technical solutions.
[0006] A method for preparing an intercalation-coated composite modified positive electrode material comprises the following steps:
[0007] (1) first dissolving V2O5 powder in water with a purity not less than that of deionized water, then adding a metal ion salt solution and a conductive carbon material, and mixing them evenly to obtain a reaction solution;
[0008] (2) transferring the reaction solution to a reaction kettle, reacting at 140 to 200° C. for 12 to 48 hours, collecting the solid product, washing it, and drying it to obtain an intercalation-coated composite modified positive electrode material;
[0009] The molar ratio of V2O5 to metal ions in the metal ion salt solution is 1:2-15; the mass ratio of V2O5 to the conductive carbon material is 1:1-4.
[0010] Furthermore, V2O5 powder is added to water with a purity not less than that of deionized water, first stirred at a stirring rate of 300-600 r / min for 20-40 min, and then a metal ion salt solution and a conductive carbon material are added, and then stirring is continued for 10-60 min to obtain a reaction solution.
[0011] Furthermore, V2O5 powder is added into water with a purity not less than that of deionized water, and the concentration of V2O5 powder in the water is 0.01-0.2 mol / L; and the concentration of metal ions in the reaction solution is 0.05-0.8 mol / L.
[0012] Furthermore, the metal ion in the metal ion salt solution is Li + 、Na + , K + 、Zn 2+ Mg 2+ , Ca 2+ , Mn 2+or Cs + The anion in the metal ion salt solution is more preferably Cl - 、SO4 2- 、NO3 - 、CO3 2- Or CH3COO-.
[0013] Furthermore, the conductive carbon material is graphene, graphene oxide, nitrogen-doped graphene or carbon nanotubes.
[0014] When the intercalation-coated composite modified positive electrode material prepared by the method of the present invention is used as an active material in a positive electrode in an aqueous zinc ion battery, the electrolyte is a zinc salt electrolyte containing an additive;
[0015] Among them, the additive is a salt solution of metal ions inserted into the active material (i.e., the intercalation-coated composite modified positive electrode material), and the anions in the salt solution are the same as the anions in the zinc salt electrolyte. The zinc salt electrolyte can be the zinc-containing electrolyte commonly used in the field of aqueous zinc ion batteries.
[0016] Furthermore, the concentration of zinc ions in the electrolyte is 1 to 4 mol / L, and the concentration of metal ions is 0.1 to 1 mol / L.
[0017] Furthermore, the anion in the electrolyte is Cl - 、SO4 2- or CF3SO3 2- .
[0018] Furthermore, the loading amount of active material in the positive electrode is 0.5-5 mg / cm 2 .
[0019] Beneficial effects:
[0020] (1) By introducing metal ions into the interlayer of V2O5 and coating the conductive carbon material, on the one hand, the introduced metal ions can effectively expand the interlayer distance, and the introduced metal ions can play a supporting role in the interlayer of the V2O5 structure, while maintaining the stability of the V2O5 structure, effectively reducing the electrostatic interaction between the zinc ion embedding / de-embedding and the matrix V2O5 during the charge and discharge process, and at the same time, it can also change the energy band filling state and Fermi level of the material, showing a reduced band gap, indicating that the conductivity of the material is increased, which is beneficial to the storage and diffusion of zinc ions. On the other hand, the coated conductive carbon material can not only further increase the conductivity, but also play a role in stabilizing the material structure, which is beneficial to maintaining the stability of the V2O5 structure during the ion embedding and de-embedding process, thereby facilitating long-term circulation. Therefore, the above-mentioned composite modified positive electrode material can be applied to aqueous batteries to effectively improve the capacity and cycle life of the battery.
[0021] (2) The selection of intercalation metal ions has a significant impact on its electrochemical zinc storage performance. After the assembled battery shows different capacities and cycle stability, this is because the efficiency of the storage process is not only affected by the interlayer spacing, but also by the interaction between the intercalation metal ions and zinc ions. For example, metal ions with similar ionic radius to zinc ions and small relative molecular mass (such as lithium ions, sodium ions, etc.) produce weak repulsion when interacting with zinc ions, and are ideal intercalation metal ions; other alkaline (earth) metal ions (such as K + ,Mg 2+ etc.) are used for V2O5 interlayer intercalation. Since the electrochemical intercalation process is accompanied by changes in the redox potential, it can change the energy band filling state and the Fermi level, showing a reduced band gap, indicating that the conductivity of the material is increased, which is beneficial to the storage and diffusion of zinc ions.
[0022] (3) The introduction of a small amount of metal ions will lead to incomplete intercalation of the V2O5 interlayer structure, showing that the materials prepared in the same batch are not uniform and the interlayer spacing is different, so the intercalation modification effect cannot be fully exerted; when excessive metal ions are introduced, the V2O5 layered structure will be destroyed and even cause structural collapse. In addition, due to the different degrees of property differences between the intercalated metal ions and zinc ions, excessive embedding will be counterproductive, inhibiting the storage and diffusion of zinc ions and causing capacity reduction. A small amount of conductive carbon material coating will not achieve the best effect of improving conductivity and stabilizing the structure, while an excessive amount of coating will increase the mass of the material, seriously reduce the energy density of the material and reduce the specific capacity of the battery. Therefore, it is necessary to regulate the amount of metal ion intercalation and the amount of conductive carbon material coating to effectively improve the electrochemical properties of the material.
[0023] (4) By adding specific additives to the zinc salt electrolyte, that is, a salt solution of intercalation metal ions with the same anions as the zinc salt, the loss of intercalation metal ions during the cycle can be effectively supplemented, the dissolution of the intercalation material can be inhibited, the stability of the intercalation structure can be maintained, and the Zn dendrite deposition can be alleviated, thereby improving the cycle performance.
[0024] (5) The intercalation-coated composite modified positive electrode material described in the present invention has a large interlayer spacing and good structural stability. It is used as an active material in the positive electrode of an aqueous zinc ion battery, which effectively improves the capacity and cycle life of the battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a transmission electron microscope (TEM) image of the 1# modified positive electrode material prepared in Example 1.
[0026] Figure 2 This is the mapping spectrum of the 1# modified positive electrode material prepared in Example 1.
[0027] Figure 3 This is a cycle performance diagram of a battery assembled using the 1# modified positive electrode material prepared in Example 1 at a current density of 0.1 A / g.
[0028] Figure 4 This is the transmission electron microscope (TEM) image of the 2# modified positive electrode material prepared in Example 2.
[0029] Figure 5 This is the mapping spectrum of the 2# modified positive electrode material prepared in Example 2.
[0030] Figure 6 This is a cycle performance diagram of a battery assembled using the 2# modified positive electrode material prepared in Example 2 at a current density of 0.1 A / g.
[0031] Figure 7 This is a cycle performance diagram of a battery assembled using the 3# modified positive electrode material prepared in Example 3 at a current density of 0.1 A / g.
[0032] Figure 8 This is a cycle performance diagram of a battery assembled using the 4# modified positive electrode material prepared in Example 4 at a current density of 0.1 A / g.
[0033] Fig. 9 This is a scanning electron microscope (SEM) image of the 5# unmodified positive electrode material in Comparative Example 1.
[0034] Fig.10 This is a cycle performance diagram of a battery assembled using 5# unmodified positive electrode material in Comparative Example 1 at a current density of 0.1 A / g.
[0035] Fig.11 This is a cycle performance diagram of the battery assembled using 6# in Comparative Example 2 at a current density of 0.1 A / g.
[0036] Fig.12 This is a cycle performance diagram of a battery assembled using the 7# modified positive electrode material prepared in Comparative Example 3 at a current density of 0.1 A / g.
[0037] Fig.13 This is a cycle performance diagram of a battery assembled with the 8# modified positive electrode material prepared in Comparative Example 4 at a current density of 0.1 A / g.
[0038] Fig.14 This is a cycle performance diagram of a battery assembled with the 9# modified positive electrode material prepared in Comparative Example 5 at a current density of 0.1 A / g.
[0039] Fig.15 This is a cycle performance diagram of a battery assembled with the 1# modified positive electrode material prepared in Example 1 in Comparative Example 6 at a current density of 0.1 A / g. DETAILED DESCRIPTION
[0040] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments, wherein the methods are conventional methods unless otherwise specified, and the raw materials can be obtained from public commercial channels unless otherwise specified.
[0041] In the following embodiments, the assembly steps of the battery are as follows: the positive electrode material prepared in the embodiment or the comparative example is used as the active material, the active material, the conductive agent acetylene black and the binder PVDF (polyvinylidene fluoride) are mixed in a mass ratio of 7:2:1, and NMP (N-methylpyrrolidone) is added dropwise, stirred and mixed into a slurry, and then coated on a titanium foil, and then placed in a vacuum drying oven at 80°C for 12 hours, and finally cut into a circular piece with a diameter of 11 mm as a positive electrode sheet. At this time, the loading amount of the active material on the positive electrode sheet is 0.5-5 mg / cm 2 ; A metal zinc sheet is selected as the negative electrode; the electrolyte is a Zn(CF3SO3)2 electrolyte containing an additive, the concentration of zinc ions in the electrolyte is 1-4 mol / L, the additive is a trifluoromethanesulfonate solution of metal ions inserted into the active material (i.e., the intercalation-coated composite modified positive electrode material), and the concentration of metal ions in the electrolyte is 0.1-2 mol / L; a glass fiber diaphragm (GF / D) is selected as the diaphragm; it is assembled into a 2023 button battery in a glove box, and then the corresponding electrochemical performance tests are carried out.
[0042] Example 1
[0043] (1) First, 0.437 g (2 mmol) of V2O5 powder was added to 50 mL of deionized water, and then stirred at a stirring rate of 400 r / min for 30 min, and then 10 mL of a 1.20 mol / L NaCl solution and 10 mL of a 80 mg / mL nitrogen-doped graphene solution were added, and the mixture was stirred for 60 min to mix well, thereby obtaining a reaction solution;
[0044] (2) The reaction solution was transferred to a reactor, reacted at 180°C for 24 hours, and then cooled to room temperature. The solid product was collected and washed three times with deionized water and ethanol respectively, and finally placed in a constant temperature vacuum oven at 80°C for drying for 12 hours to obtain an intercalation-coated composite modified positive electrode material, which was abbreviated as 1# modified positive electrode material.
[0045] The morphology of the 1# modified cathode material was characterized. Figure 1 In the TEM image, a clear conductive carbon coating layer can be seen, and the layered structure of the material can be observed. At the same time, after the mapping test of the 1# modified positive electrode material, it was shown that the sodium ions were uniformly inserted into the interlayer of the V2O5 structure.
[0046] The 1# modified positive electrode material was used as the active material to assemble a 2023 button cell, where the loading amount of the active material on the positive electrode sheet was 1.6 mg / cm 2 , the concentration of Zn(CF3SO3)2 in the electrolyte is 3 mol / L, and the concentration of NaCF3SO3 in the electrolyte is 1 mol / L. At a current density of 0.1A / g, the initial discharge capacity of the assembled battery is 178mAh / g. There is a certain capacity increase in the first 20 weeks, and then the capacity remains basically unchanged. After 320 cycles, the discharge capacity is about 170mAh / g, and the capacity retention rate is 95.5%. Figure 3 At a high current density of 5A / g, the initial discharge capacity of the assembled battery is 83mAh / g, the coulombic efficiency is about 100%, it can be stably cycled for 1000 cycles, and the discharge specific capacity after 1000 cycles is 66mAh / g.
[0047] Example 2
[0048] (1) First, 0.437 g (2 mmol) of V2O5 powder was added to 50 mL of deionized water, and then stirred at a stirring rate of 400 r / min for 30 min, and then 10 mL of 0.40 mol / L calcium chloride hexahydrate solution and 10 mL of 80 mg / mL nitrogen-doped graphene solution were added, and the mixture was stirred for 60 min to mix well, thereby obtaining a reaction solution;
[0049] (2) The reaction solution was transferred to a reactor, reacted at 180°C for 24 hours, and then cooled to room temperature. The solid product was collected and washed three times with deionized water and ethanol respectively, and finally placed in a constant temperature vacuum oven at 80°C for 12 hours to obtain an intercalation-coated composite modified positive electrode material, which was abbreviated as 2# modified positive electrode material.
[0050] The morphology of the 2# modified cathode material was characterized. Figure 3 In the TEM image, a clear conductive carbon coating layer can be seen, and the layered structure of the material can be observed. At the same time, after the mapping test of the 2# modified positive electrode material, it was shown that calcium ions were uniformly inserted into the interlayer of the V2O5 structure.
[0051] The 2# modified positive electrode material was used as the active material to assemble a 2023 button cell, where the loading amount of the active material on the positive electrode sheet was 1.8 mg / cm 2, the concentration of Zn(CF3SO3)2 in the electrolyte is 3 mol / L, and the concentration of Ca(CF3SO3)2 in the electrolyte is 1 mol / L. At a current density of 0.1A / g, the initial discharge capacity of the assembled battery is 260mAh / g. There is a certain capacity decline trend in the first 5 weeks of the cycle, and then it can be cycled stably for more than 200 cycles, and the discharge capacity after 220 cycles is still about 180mAh / g. Figure 6 At a high current density of 5A / g, the initial discharge capacity of the assembled battery is 57mAh / g, and it can be stably cycled for 1000 cycles. Moreover, the discharge specific capacity after 1000 cycles is 50mAh / g, and the coulombic efficiency during the cycle is about 100%.
[0052] Example 3
[0053] (1) First, 0.437 g (2 mmol) of V2O5 powder was added to 50 mL of deionized water, and then stirred at a stirring rate of 400 r / min for 30 min, and then 10 mL of a 2.40 mol / L NaCl solution and 10 mL of a 80 mg / mL nitrogen-doped graphene solution were added, and the mixture was stirred for 60 min to mix well, thereby obtaining a reaction solution;
[0054] (2) The reaction solution was transferred to a reactor, reacted at 180°C for 24 hours, and then cooled to room temperature. The solid product was collected and washed three times with deionized water and ethanol respectively, and finally placed in a constant temperature vacuum oven at 80°C for drying for 12 hours to obtain an intercalation-coated composite modified positive electrode material, which was abbreviated as 3# modified positive electrode material.
[0055] The 3# modified positive electrode material was used as the active material to assemble into a 2023 button cell, where the loading amount of the active material on the positive electrode sheet was 1.6 mg / cm 2 , the concentration of Zn(CF3SO3)2 in the electrolyte is 3 mol / L, and the concentration of NaCF3SO3 in the electrolyte is 1 mol / L. At a current density of 0.1A / g, the initial discharge capacity of the assembled battery is 257mAh / g. The capacity decreases in the first 70 cycles and then increases. The overall capacity is high. After 280 cycles, the capacity is about 162mAh / g. Figure 7 shown.
[0056] Example 4
[0057] (1) First, 0.437 g (2 mmol) of V2O5 powder was added to 50 mL of deionized water, and then stirred at a stirring rate of 400 r / min for 30 min, and then 10 mL of a 1.20 mol / L NaCl solution and 20 mL of a 80 mg / mL nitrogen-doped graphene solution were added, and the mixture was stirred for 60 min to mix well, thereby obtaining a reaction solution;
[0058] (2) The reaction solution was transferred to a reactor, reacted at 180°C for 24 hours, and then cooled to room temperature. The solid product was collected and washed three times with deionized water and ethanol respectively, and finally placed in a constant temperature vacuum oven at 80°C for 12 hours to obtain an intercalation-coated composite modified positive electrode material, which was abbreviated as 4# modified positive electrode material.
[0059] The 4# modified positive electrode material was used as the active material to assemble a 2023 button cell, where the loading amount of the active material on the positive electrode sheet was 1.6 mg / cm 2 , the concentration of Zn(CF3SO3)2 in the electrolyte is 3 mol / L, and the concentration of NaCF3SO3 in the electrolyte is 1 mol / L. At a current density of 0.1 A / g, the initial discharge capacity of the assembled battery is 125 mAh / g, the capacity increases slightly in the first 6 weeks, and the capacity slowly decreases after 20 cycles, and then stabilizes. After 150 cycles, the capacity is about 116 mAh / g, and the capacity retention rate is 92.8%. Figure 8 shown.
[0060] Comparative Example 1
[0061] The morphology of the unmodified V2O5 powder (abbreviated as 5# unmodified positive electrode material) was characterized. Fig. 9 The SEM image shows that the 5# unmodified positive electrode material is a lamellar structure with a certain thickness.
[0062] The 5# unmodified positive electrode material was used as the active material to assemble a 2023 button cell, where the loading amount of the active material on the positive electrode sheet was 1.6 mg / cm 2 , the concentration of Zn(CF3SO3)2 in the electrolyte is 3 mol / L. At a current density of 0.1A / g, the initial discharge capacity of the assembled battery is less than 50mAh / g, and it is unstable in the first 150 cycles. It first increases significantly and then turns to a significant decrease in capacity. After 150 cycles, the capacity decrease trend becomes gentle, and the discharge capacity at 550 cycles is 75mAh / g. Fig.10 At a high current density of 5A / g, although the initial discharge capacity of the assembled battery is 100mAh / g, the capacity decreases rapidly during the cycle. After 80 cycles, the capacity drops to less than 30mAh / g, and the cycle stability is poor.
[0063] Comparative Example 2
[0064] (1) First, 0.437 g (2 mmol) of V2O5 powder was added to 50 mL of deionized water, and then stirred at a stirring rate of 400 r / min for 30 min, and then 10 mL of 1.20 mol / L NaCl solution was added, and stirring was continued for 60 min to mix well to obtain a reaction solution;
[0065] (2) The reaction solution was transferred to a reactor, reacted at 180°C for 24 hours, and then cooled to room temperature. The solid product was collected and washed three times with deionized water and ethanol respectively, and finally placed in a constant temperature vacuum oven at 80°C for drying for 12 hours to obtain 6# modified positive electrode material.
[0066] The 6# modified positive electrode material was used as the active material to assemble a 2023 button cell, where the loading amount of the active material on the positive electrode sheet was 1.60 mg / cm 2 , the concentration of Zn(CF3SO3)2 in the electrolyte is 3 mol / L, and the concentration of NaCF3SO3 in the electrolyte is 1 mol / L. Fig.11 As shown in the figure, at a current density of 0.1A / g, the initial discharge capacity of the assembled battery is 160mAh / g, and then the capacity continues to decline. After 800 cycles, the discharge capacity is 65mAh / g, the capacity retention rate is 41%, and the coulombic efficiency varies greatly, indicating that the ions cannot be fully embedded / extracted, and the charge and discharge are not complete. At a high current density of 5A / g, the coulombic efficiency of the assembled battery changes greatly during the cycle, indicating that the structure is unstable and the charge and discharge reversibility is poor.
[0067] Comparative Example 3
[0068] (1) First, 0.437 g (2 mmol) of V2O5 powder was added to 50 mL of deionized water, and then stirred at a stirring rate of 400 r / min for 30 min, and then 10 mL of 0.4 mol / L calcium chloride hexahydrate solution was added, and the mixture was stirred for 60 min to be uniformly mixed to obtain a reaction solution;
[0069] (2) The reaction solution was transferred to a reactor, reacted at 180°C for 24 hours, and then cooled to room temperature. The solid product was collected and washed three times with deionized water and ethanol respectively, and finally placed in a constant temperature vacuum oven at 80°C for 12 hours to obtain 7# modified positive electrode material.
[0070] The 7# modified positive electrode material was used as the active material to assemble a 2023 button cell, where the loading amount of the active material on the positive electrode sheet was 1.80 mg / cm 2, the concentration of Zn(CF3SO3)2 in the electrolyte is 3 mol / L, and the concentration of Ca(CF3SO3)2 in the electrolyte is 1 mol / L. Fig.12 As shown in the figure, at a current density of 0.1A / g, the initial discharge capacity of the assembled battery is 285mAh / g, but the capacity decreases rapidly in the early stage of the cycle, and the discharge capacity drops to 40mAh / g after 120 cycles, with a capacity retention rate of 41%, and the coulombic efficiency is unstable at this stage, indicating that the charge and discharge are incomplete. Although it can be cycled for 1000 cycles in the subsequent low-capacity charge and discharge process, the cycle is relatively stable and the capacity is low.
[0071] Comparative Example 4
[0072] (1) First, 0.437 g (2 mmol) of V2O5 powder was added to 50 mL of deionized water, and then stirred at a stirring rate of 400 r / min for 30 min, and then 10 mL of a 6.0 mol / L NaCl solution and 10 mL of a 80 mg / mL nitrogen-doped graphene solution were added, and the mixture was stirred for 60 min to mix well, thereby obtaining a reaction solution;
[0073] (2) The reaction solution was transferred to a reactor, reacted at 180°C for 24 hours, and then cooled to room temperature. The solid product was collected and washed three times with deionized water and ethanol respectively, and finally placed in a constant temperature vacuum oven at 80°C for drying for 12 hours to obtain an intercalation-coated composite modified positive electrode material, which was abbreviated as 8# modified positive electrode material.
[0074] The 8# modified positive electrode material was used as the active material to assemble a 2023 button cell, where the loading amount of the active material on the positive electrode sheet was 1.6 mg / cm 2 , the concentration of Zn(CF3SO3)2 in the electrolyte is 3 mol / L, and the concentration of NaCF3SO3 in the electrolyte is 1 mol / L. Fig.13 As shown, at a current density of 0.1A / g, the assembled battery initially has an ultra-high discharge specific capacity of 400mAh / g, but the capacity drops rapidly to 40mAh / g in the first 30 weeks of cycling, indicating that although excessive sodium ion intercalation will create a larger interlayer spacing and store more capacity in the early stage of the cycle, it cannot maintain the stability of the layered structure, and the structure is easily collapsed as zinc ions are inserted / extracted.
[0075] Comparative Example 5
[0076] (1) First, 0.437 g (2 mmol) of V2O5 powder was added to 50 mL of deionized water, and then stirred at a stirring rate of 400 r / min for 30 min, and then 10 mL of a 1.20 mol / L NaCl solution and 10 mL of a 400 mg / mL nitrogen-doped graphene solution were added, and the mixture was stirred for 60 min to mix well, thereby obtaining a reaction solution;
[0077] (2) The reaction solution was transferred to a reactor, reacted at 180°C for 24 hours, and then cooled to room temperature. The solid product was collected and washed three times with deionized water and ethanol respectively, and finally placed in a constant temperature vacuum oven at 80°C for drying for 12 hours to obtain an intercalation-coated composite modified positive electrode material, which was abbreviated as 9# modified positive electrode material.
[0078] The 9# modified positive electrode material was used as the active material to assemble a 2023 button cell, where the loading amount of the active material on the positive electrode sheet was 1.6 mg / cm 2 , the concentration of Zn(CF3SO3)2 in the electrolyte is 3 mol / L, and the concentration of NaCF3SO3 in the electrolyte is 1 mol / L. Fig.14 As shown, at a current density of 0.1 A / g, the discharge specific capacity of the assembled battery is always low, with an initial discharge specific capacity of about 90 mAh / g. The subsequent capacity decreases slightly but is relatively stable, indicating that excessive conductive carbon coating will reduce the energy density of the material and cause a decrease in the battery specific capacity.
[0079] Comparative Example 6
[0080] Based on Example 1, the 1# modified positive electrode material was used as the active material to assemble a 2023 type button battery, wherein the loading amount of the active material on the positive electrode sheet was 1.6 mg / cm 2 , the concentration of Zn(CF3SO3)2 in the electrolyte is 3 mol / L. Fig.15 As shown, at a current density of 0.1 A / g, the discharge specific capacity of the assembled battery is about 175 mAh / g, and the capacity continues to decrease to 80 mAh / g after 150 cycles. Compared with Example 1, its capacity and stability are poor, indicating that the special electrolyte additive can effectively improve the battery cycle performance. This is because the specific electrolyte additive supplements the loss of intercalated metal ions during the cycle, inhibits the dissolution of intercalated materials, and can alleviate Zn dendrite deposition.
[0081] In summary, the above are only preferred embodiments of the present invention and are not intended to limit the protection scope of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing an intercalation-coated composite modified positive electrode material, characterized in that: The following steps are involved: (1) First, dissolve V2O5 powder in water with a purity not less than that of deionized water, stir at a stirring rate of 300-600 r / min for 20-40 min, then add metal ion salt solution and conductive carbon material, and continue stirring for 10-60 min to mix evenly to obtain a reaction solution; (2) The reaction solution is transferred to a reactor, and after reacting at 140-200 °C for 12-48 h, the solid product is collected and washed and dried to obtain an intercalation-coated composite modified positive electrode material; The molar ratio of V2O5 to metal ions in the metal ion salt solution is 1:2-15; the mass ratio of V2O5 to the conductive carbon material is 1:1-4; The concentration of V2O5 powder in water is 0.01~0.2 mol / L; the concentration of metal ions in the reaction solution is 0.05~0.8 mol / L; The conductive carbon material is graphene, graphene oxide, nitrogen-doped graphene or carbon nanotube; The metal ion in the metal ion salt solution is Li + 、Na + , K + 、Zn 2+ Mg 2+ , Ca 2+ , Mn 2+ or Cs + ; The anion in the metal ion salt solution is Cl - 、SO4 2- 、NO3 - 、CO3 2- or CH3COO - .
2. An application of the intercalation-coated composite modified positive electrode material prepared by the method of claim 1, characterized in that: The intercalation-coated composite modified positive electrode material is used as the active material in the positive electrode in an aqueous zinc ion battery, and the electrolyte is a zinc salt electrolyte containing additives; The additive is a salt solution of metal ions inserted into the active material, and the anions in the salt solution are the same as the anions in the zinc salt electrolyte.
3. The use of an intercalation-coated composite modified positive electrode material according to claim 2, characterized in that: The concentration of zinc ions in the electrolyte is 1~4 mol / L, and the concentration of metal ions is 0.1~1 mol / L.
4. The use of an intercalation-coated composite modified positive electrode material according to claim 2, characterized in that: The anion in the electrolyte is Cl − 、SO4 2− or CF3SO3 2− .
5. The use of an intercalation-coated composite modified positive electrode material according to claim 2, characterized in that: The loading amount of active material in the positive electrode is 0.5~5 mg / cm 2 .