A kind of impermeable concrete and preparation method thereof

By using a combination of slow-release expansion agent and composite fiber in concrete, the problem of insufficient impermeability and durability of existing concrete is solved, high compressive strength and impermeability are improved, and excessive addition of expansion agent is avoided. The negative impact on compressive strength ensures the stable performance of concrete in long-term use.

CN116003048BInactive Publication Date: 2024-10-11CHINA RAILWAY FIRST GROUP CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211542636.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-02
Publication Date
2024-10-11
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing concrete has deficiencies in impermeability and durability. Especially in high-pressure and high-temperature environments, it is prone to reduced waterproofing and crack resistance. Excessive addition of expansion agents can lead to a decrease in compressive strength.

Method used

An impermeable concrete formula is used, including cement, coarse aggregate, fly ash, slow-release expansion agent and composite fiber. The slow-release expansion agent consists of a core layer and a coating layer. The core layer is expansion agent, melamine/ Graphene oxide/sepiolite composite, the coating layer is guar gum and boric acid, the composite fiber is composed of lignin fiber, basalt fiber and epoxy-modified polypropylene fiber. Through specific proportions and preparation methods, the compressive strength and Impermeability.

Benefits of technology

Significantly improves the compressive strength and impermeability of concrete, delays the release of expansion agent, avoids the negative impact of excessive addition of expansion agent on compressive strength, enhances the durability and compactness of concrete, and ensures efficient waterproofing performance .

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention provides a kind of impermeable concrete, it includes the following raw materials in parts by weight: 280-300 parts of cement, 1000-1050 parts of coarse aggregate, 40-50 parts of fly ash, 30-38 parts of expansion agent, 5.6-7.5 parts of water reducer, 20-26 parts of composite fiber and 160-180 parts of water; the composite fiber includes lignin fiber, basalt fiber, epoxy modified polypropylene fiber; the expansion agent is a slow-release expansion agent; the slow-release expansion agent is composed of a core layer and a coating layer, the core layer is composed of expansion agent, melamine / graphene oxide / sepiolite composite, and the coating layer is composed of guar gum and boric acid. The concrete of the present invention has good use performance, durability, and impermeability, can meet the needs of different application scenarios, and solves the problem of poor durability and impermeability of current concrete.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to an anti-seepage concrete and a preparation method thereof. Background Art

[0002] As one of the most important civil engineering materials, concrete is in great demand due to its abundant raw materials, low price and simple production process. Its application fields are becoming more and more extensive, and there are more and more types of concrete. In order to meet the application of concrete in different application fields, the development of concrete with different functions has attracted wide attention. For example, if ordinary concrete materials are used in the water-rich pressure sand layer of the subway, it will have problems with insufficient waterproof and anti-seepage performance.

[0003] On the one hand, the existing ordinary concrete materials have poor impermeability due to their own capillary pores and small cracks, which make them insufficiently airtight. On the other hand, their impermeability is reduced due to their low tensile strength and easy cracking. At present, most of the methods of improving the impermeability of concrete are adopted by adding additives such as expansion agents to concrete materials. However, adding too many expansion agents and other ingredients will cause the compressive strength and other properties of concrete to decrease. Therefore, research and development of concrete with both good strength and crack resistance and impermeability to meet the needs of different application scenarios has become an urgent problem to be solved. Summary of the invention

[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide an impermeable concrete with good performance, durability, high compressive strength and good impermeability, which solves the current problems of poor durability and impermeability of concrete.

[0005] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0006] A kind of impermeable concrete, comprising the following raw materials in parts by weight: 280-300 parts of cement, 1000-1050 parts of coarse aggregate, 40-50 parts of fly ash, 30-38 parts of expansion agent, 5.6-7.5 parts of water reducer, 20-26 parts of composite fiber and 160-180 parts of water; the composite fiber comprises lignin fiber, basalt fiber and epoxy modified polypropylene fiber; the expansion agent is a slow-release expansion agent; the slow-release expansion agent is composed of a core layer and a coating layer, the core layer is composed of the expansion agent and melamine / graphene oxide / sepiolite composite, and the coating layer is composed of guar gum and boric acid;

[0007] Preferably, the weight ratio of the lignin fiber, basalt fiber, and epoxy-modified polypropylene fiber is 1:1:5-7;

[0008] Furthermore, the preparation method of the epoxy-modified polypropylene fiber is as follows: heating the polypropylene fiber resin to a molten state, adding an epoxy silane coupling agent thereto, stirring and degassing, and then spinning to obtain the epoxy-modified polypropylene fiber;

[0009] Preferably, the weight ratio of the expander to the melamine / graphene oxide / sepiolite composite is 1:5;

[0010] Preferably, the preparation method of the melamine / graphene oxide / sepiolite composite is: dispersing melamine and graphene oxide in ethanol, adding sepiolite thereto under stirring conditions for adsorption and assembly, and then taking out and drying to obtain the melamine / graphene oxide / sepiolite composite;

[0011] Preferably, the mass ratio of melamine, graphene oxide and sepiolite is 1:1:10;

[0012] Preferably, the preparation method of the sustained-release swelling agent is as follows: the swelling agent and the melamine / graphene oxide / sepiolite composite are uniformly mixed and placed in a granulator as a core layer, and the guar gum solution and the boric acid solution are sprayed into the core layer at the same time; granulation is performed to obtain the sustained-release swelling agent;

[0013] Preferably, the coarse aggregate is crushed stone and fine sand; the particle size of the crushed stone is 6-8 mm; the fineness modulus of the fine sand is 2.2-1.6;

[0014] Preferably, the cement is P042.5;

[0015] Preferably, the water reducer is a polycarboxylate water reducer;

[0016] Furthermore, the method for preparing the impermeable concrete specifically comprises the following steps:

[0017] (1) Material preparation: weigh the materials in the above-mentioned weight proportions; and uniformly mix the water reducer with water to obtain a water reducer solution;

[0018] (1) placing cement and fly ash in a mixer and stirring them uniformly, and then adding a water reducing agent solution thereto under stirring conditions to obtain cement slurry;

[0019] After the coarse aggregate, expansion agent and composite fiber are mixed evenly, they are added into cement slurry under stirring conditions, and after stirring evenly, impermeable concrete can be obtained.

[0020] Beneficial Effects

[0021] The anti-seepage concrete of the present invention has reasonable proportions of various raw material components, and the raw materials cooperate with each other to prepare an anti-seepage concrete with good compressive strength, strong anti-seepage ability and good durability.

[0022] The slow-release expansion agent and the composite fiber in the impermeable concrete of the present invention cooperate with each other to effectively block the capillary channels in the concrete, thereby preventing water from penetrating into the concrete, significantly improving the compactness of the concrete and further improving the impermeability of the concrete.

[0023] In the present invention, composite fibers are composed of basalt fibers, lignin fibers, and epoxy-modified polypropylene fibers in specific proportions. The interaction between the three fibers improves the interfacial force in the concrete material, inhibits the development of cracks, and improves the anti-seepage and anti-cracking properties and compressive strength of the concrete. The addition of the composite fibers effectively reduces the amount of expansion agent added, avoiding excessive addition of the expansion agent. At the same time, in the present application, the expansion agent is a slow-release expansion agent, which realizes the slow release of the expansion agent, effectively alleviating the problem of reduced compressive strength of the concrete caused by excessive addition of the expansion agent, and the slow-release property of the expansion agent also improves the durability of the concrete, thereby having high anti-seepage performance while ensuring the compressive strength of the concrete material for a long time.

[0024] The core layer of the slow-release expansion agent of the present invention is an expansion agent and a melamine / graphene oxide / sepiolite composite; the expansion agent in the slow-release expansion agent plays a role first, followed by the melamine / graphene oxide / sepiolite composite; the two cooperate with each other to ensure that the anti-permeability of the concrete is continuously enhanced under the condition of reducing the amount of expansion agent added; the adsorption and assembly of melamine and graphene oxide in the melamine / graphene oxide / sepiolite composite delays the expansion speed of the sepiolite, makes it expand slowly, inhibits the development of cracks, and improves the durability of the concrete material; and the addition of melamine and graphene oxide also improves the bonding force between concrete materials, thereby improving the compactness of the concrete material and improving the compressive strength of the concrete. DETAILED DESCRIPTION

[0025] The technical solution of the present invention is described in detail below in conjunction with specific embodiments. It should be noted that the protection scope of the present invention is not limited to the technical solution disclosed in the specific embodiments; the raw materials used in the present invention can be obtained from the market unless otherwise specified, and the methods described are conventional methods unless otherwise specified.

[0026] Preparation of composite fibers:

[0027] Preparation of epoxy-modified polypropylene fiber: heat the polypropylene fiber resin to a molten state, add an epoxy silane coupling agent (the amount added is 10% of the mass of the polypropylene fiber) thereto, stir evenly, let it stand for degassing, and then spin to obtain epoxy-modified polypropylene fiber; wherein the epoxy silane coupling agent is preferably γ-glycidyloxypropyltrimethoxysilane;

[0028] Preparation of composite fiber: lignin fiber, basalt fiber and epoxy-modified polypropylene fiber were mixed uniformly at a weight ratio of 1:1:5 to obtain composite fiber No. 1;

[0029] The lignin fiber, basalt fiber and epoxy-modified polypropylene fiber are uniformly mixed in a weight ratio of 1:1:6 to obtain mixed fiber No. 2;

[0030] The lignin fiber, basalt fiber and epoxy-modified polypropylene fiber were mixed uniformly at a weight ratio of 1:1:7 to obtain composite fiber No. 3;

[0031] Preparation of sustained-release bulking agent:

[0032] (1) Preparation of melamine / graphene oxide-coated sepiolite composite: melamine and graphene oxide are dispersed in 2 times the mass of industrial ethanol, sepiolite is added thereto under stirring conditions for adsorption assembly, and then taken out and dried to obtain a melamine / graphene oxide / sepiolite composite; wherein the mass ratio of melamine, graphene oxide, and sepiolite is 1:1:10;

[0033] (2) The expander and melamine / graphene oxide / sepiolite composite are uniformly mixed and placed in a granulator as a core layer, and the guar gum solution and the boric acid solution are sprayed into the core layer at the same time; granulation is performed to obtain a sustained-release expander; wherein the weight ratio of the expander to the melamine / graphene oxide / sepiolite composite is 1:5; the expander is a UEA expander; the mass concentration of the guar gum solution is 2wt%; and the mass concentration of the boric acid solution is 1wt%.

[0034] Examples 1-5

[0035] A kind of impermeable concrete comprises the following raw materials in parts by weight: 280-300 parts of cement, 1000-1050 parts of coarse aggregate, 40-50 parts of fly ash, 30-38 parts of expansion agent, 5.6-7.5 parts of water reducer, 20-26 parts of composite fiber and 160-180 parts of water; the composite fiber comprises lignin fiber, basalt fiber and epoxy modified polypropylene fiber; the expansion agent is a slow-release expansion agent; the slow-release expansion agent consists of a core layer and a coating layer, the core layer consists of the expansion agent and a melamine / graphene oxide / sepiolite composite, and the coating layer consists of guar gum and boric acid.

[0036] In Examples 1-5, the addition amount (parts by weight) of each raw material in the impermeable concrete is shown in Table 1.

[0037] Table 1 Ingredients of Example 1-5 Anti-seepage Concrete

[0038] Example 1 Example 2 Example 3 Example 4 Example 5 cement 280 285 290 295 300 coarse aggregate 1000 1015 1025 1030 1050 Fly ash 40 42 45 48 50 Bulking Agent 30 32 34 36 38 Water reducing agent 5.6 6.1 6.6 7.0 7.5 Composite Fiber 20 22 23 24 26 water 160 165 170 175 180

[0039] In Examples 1-5, the coarse aggregate is crushed stone and fine sand; the particle size of the crushed stone is 6-8 mm; the fineness modulus of the fine sand is 2.2-1.6; the cement is P042.5; the water reducer is polycarboxylate water reducer; the composite fiber is composite fiber No. 2;

[0040] Example 6

[0041] The raw material composition and proportion of concrete in Example 6 are substantially the same as those in Example 3, except that the composite fiber used therein is composite fiber No. 1;

[0042] Example 7

[0043] The raw material composition and proportion of concrete in Example 6 are substantially the same as those in Example 3, except that the composite fiber used therein is composite fiber No. 3;

[0044] The method for preparing the impermeable concrete in Examples 1-7 specifically comprises the following steps:

[0045] (1) Material preparation: weigh the materials in the above-mentioned weight proportions; and uniformly mix the water reducer with water to obtain a water reducer solution;

[0046] (2) placing cement and fly ash in a mixer and stirring them uniformly, and then adding a water reducing agent solution thereto under stirring conditions to obtain cement slurry;

[0047] (3) After the coarse aggregate, expansion agent and composite fiber are mixed evenly, they are added to the cement slurry under stirring conditions, and after stirring evenly, impermeable concrete can be obtained.

[0048] The concrete is molded and cured according to the test standards of corresponding performance, and concrete samples can be obtained for testing.

[0049] Comparative Example 1

[0050] The raw material composition and proportion of the impermeable concrete of Comparative Example 1 and Example 3 are basically the same, except that the epoxy-modified polypropylene fiber in the composite fiber is replaced by an equal amount of polypropylene fiber. The concrete preparation method is the same as that of Example 3.

[0051] Comparative Example 2

[0052] The raw material composition and proportion of the impermeable concrete of Comparative Example 2 are substantially the same as those of Example 3, except that an equal amount of sepiolite is used to replace the melamine / graphene oxide / sepiolite composite in the preparation of the slow-release expansion agent.

[0053] The performance of the impermeable concrete in Examples 1-7 and Comparative Examples 1-2 of the present invention was tested:

[0054] Compressive strength test: According to GB / T50081-2019 "Standard for Test Methods for Physical and Mechanical Properties of Concrete", the 7d compressive strength (MPa) and 28d compressive strength (MPa) of the concrete of each embodiment and comparative example were tested.

[0055] Anti-permeability performance test: According to the water penetration test in GB / T50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete", the water penetration resistance of the concrete in each embodiment and comparative example was tested.

[0056] Cracking index test: The cracking index of the concrete of each embodiment and comparative example was tested according to GB / T29417-2012 “Test method for drying shrinkage cracking performance of cement mortar and concrete”.

[0057] The test results are shown in Table 2.

[0058] Table 2 Test results of various properties of concrete

[0059] 7d compressive strength / MPa 28d compressive strength / MPa Maximum water seepage pressure / MPa Cracking index Example 1 52 68 2.0 1% Example 2 54 70 2.2 1% Example 3 55 73 2.4 1% Example 4 51 69 1.9 1% Example 5 50 67 1.8 1% Example 6 52 71 2.1 1% Example 7 53 72 2.3 1% Comparative Example 1 41 54 1.3 2% Comparative Example 2 46 58 1.4 2%

[0060] It can be seen from the data in Table 2 that the concrete prepared in Examples 1-7 of the present invention has high compressive strength, a small cracking index, a small possibility of cracking of the concrete under drying shrinkage conditions, and excellent anti-permeability performance;

[0061] From the data comparison between Comparative Example 1 and Example 3 in Table 2, it can be seen that the composite fiber added to the concrete in the present invention contains epoxy-modified polypropylene fiber, which will significantly improve the compressive strength of the concrete. The reason may be that the epoxy-modified polypropylene fiber can be more easily dispersed in the cement colloid, coarse aggregate and other components in the concrete, and the interfacial effect with the cement colloid is enhanced, becoming a bridge connecting the cement colloid and the aggregate, enhancing the bonding effect, making it less likely for the concrete to be damaged or broken when under pressure, thereby improving the overall stability of the concrete; at the same time, the anti-permeability performance of the concrete is also improved.

[0062] From the data comparison between Comparative Example 2 and Example 3 in Table 2, it can be seen that the adsorption of melamine and graphene oxide on the surface of sepiolite in the sustained-release expansion agent has a significant effect on the compressive strength and anti-seepage performance of the concrete; the reason may be that melamine and graphene oxide are adsorbed on the surface of sepiolite in a lamellar structure through π-π stacking, which changes the surface composition of sepiolite, controls the expansion rate of sepiolite, and makes the water absorption, expansion, anti-seepage and anti-cracking performance of sepiolite fully and effectively exerted; at the same time, it also enhances the effect between sepiolite and cement colloid; on the other hand, it may be that melamine and the lamellar structure of graphene oxide themselves also have the effect of blocking capillary channels to achieve the effect of waterproofing and anti-seepage.

[0063] The above embodiments are only preferred specific implementation methods of the present invention, and the protection scope of the present invention is not limited thereto. Any simple changes or equivalent replacements of the technical solutions that can be obviously obtained by any technician familiar with the technical field within the technical scope disclosed in the present invention all fall within the protection scope of the present invention.

Claims

1. An impermeable concrete, characterized in that: The invention comprises the following raw materials in parts by weight: 280-300 parts of cement, 1000-1050 parts of coarse aggregate, 40-50 parts of fly ash, 30-38 parts of expansion agent, 5.6-7.5 parts of water reducer, 20-26 parts of composite fiber and 160-180 parts of water; the composite fiber comprises lignin fiber, basalt fiber and epoxy-modified polypropylene fiber; the expansion agent is a slow-release expansion agent; the slow-release expansion agent is composed of a core layer and a coating layer, the core layer is composed of the expansion agent and a melamine / graphene oxide / sepiolite composite, and the coating layer is composed of guar gum and boric acid; The preparation method of the melamine / graphene oxide / sepiolite composite is as follows: melamine and graphene oxide are dispersed in ethanol, sepiolite is added thereto under stirring conditions for adsorption and assembly, and then taken out and dried to obtain the melamine / graphene oxide coated sepiolite composite; The preparation method of the sustained-release swelling agent is specifically as follows: the swelling agent and the melamine / graphene oxide / sepiolite composite are uniformly mixed and placed in a granulator as a core layer, and the guar gum solution and the boric acid solution are sprayed into the core layer at the same time, and granulation is performed to obtain the sustained-release swelling agent; The mass ratio of melamine, graphene oxide and sepiolite is 1:1:

10.

2. The impermeable concrete according to claim 1, characterized in that: The weight ratio of the lignin fiber, the basalt fiber and the epoxy-modified polypropylene fiber is 1:1:5-7.

3. The impermeable concrete according to claim 1, characterized in that: The preparation method of the epoxy-modified polypropylene fiber is as follows: heating the polypropylene fiber resin to a molten state, adding an epoxy silane coupling agent thereto, stirring evenly and degassing, and then spinning to obtain the epoxy-modified polypropylene fiber.

4. The impermeable concrete according to claim 1, characterized in that: The weight ratio of the expander to the melamine / graphene oxide / sepiolite composite is 1:

5.

5. The impermeable concrete according to claim 1, characterized in that: The coarse aggregate is crushed stone and fine sand; the particle size of the crushed stone is 6-8 mm; the fineness modulus of the fine sand is 2.2-1.

6.

6. The impermeable concrete according to claim 1, characterized in that: The cement is P042.5; the water reducer is polycarboxylic acid water reducer.

7. The impermeable concrete according to claim 1, characterized in that: The preparation method of the impermeable concrete specifically comprises the following steps: (1) Material preparation: weigh the materials in the above-mentioned weight proportions; and uniformly mix the water reducer with water to obtain a water reducer solution; (2) placing cement and fly ash in a mixer and stirring them uniformly, and then adding a water reducing agent solution thereto under stirring conditions to obtain cement slurry; (3) After the coarse aggregate, expansion agent and composite fiber are mixed evenly, they are added to the cement slurry under stirring conditions. After stirring evenly, impermeable concrete can be obtained.