A carbon-nitrogen-boron ternary negative electrode material, preparation method and application
The carbon-nitrogen-boron ternary anode material is prepared through a CVD rotary coating furnace, which solves the shortcomings of lithium-ion battery anode materials in rate performance and cycle life, achieves high energy density and long cycle life, and is suitable for industrial production.
Patent Information
- Application Number
- CN202310077569.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-08
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-02-08
AI Technical Summary
Existing lithium-ion battery anode materials often sacrifice energy density and cycle life when improving rate performance, and traditional preparation methods have problems with hydrochloric acid corrosiveness and low first Coulombic efficiency, making it difficult to meet the needs of industrial production.
A CVD rotary coating furnace is used to prepare a porous artificial graphite precursor, and ammonia borane is introduced to form a carbon-nitrogen-boron (CNB) ternary anode material. A carbon-nitrogen-boron ternary anode material with a surface porous structure is formed through high-temperature reaction.
It achieves high specific capacity, excellent rate performance and long cycle life. The process is simple, environmentally friendly and low-cost. It is suitable for industrial production and avoids the use of toxic solvents and high-temperature protective gases.
Smart Images

Figure CN116014140B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of battery materials, and in particular to a carbon-nitrogen-boron (CNB) ternary negative electrode material, a preparation method and an application thereof. Background Art
[0002] In today's society, the environmental friendliness and sustainable development of energy storage are receiving more and more attention. So far, lithium-ion battery technology has been considered an important form of energy storage due to its advantages such as high specific capacity, long cycle life, environmental friendliness, and no memory effect. Studies have shown that the key to determining the electrochemical performance of lithium-ion batteries is the electrode material, especially the negative electrode material as the main contributor to capacity. With the popularization of new energy vehicles equipped with lithium-ion batteries, users also have higher requirements for driving range and fast charging. Therefore, it is urgent to explore negative electrode materials with high capacity, high rate performance and long cycle life.
[0003] However, in order to obtain better rate performance, lithium-ion batteries often sacrifice the energy density of the negative electrode material. At the same time, under rate charging conditions, lithium deposition and various problems inherent in the electrochemical system are very likely to occur on the electrode surface, causing irreversible damage to the battery's capacity and service life.
[0004] In order to overcome these defects, technicians have adopted methods such as reducing the particle size of negative electrode materials and carbonizing the surface of materials to improve the rate performance of negative electrode materials. However, the above methods still have the problem of reducing the specific capacity of materials and poor rate performance in high energy density design systems during actual application. In order to further improve the energy density and rate performance of materials, Chinese patent CN110911665B discloses a boron- and nitrogen-doped lithium-ion battery negative electrode material and a preparation method thereof, which is to mix melamine, ammonium borate, tetraethyl orthosilicate, hydrochloric acid, deionized water and ethanol to obtain a colloidal precursor solution, and the product after heating and carbonization is doped with graphite for ball milling. This method uses hydrochloric acid, which has the problem of hydrochloric acid corrosiveness, and the material is seriously reduced in the first coulomb efficiency by ball milling. Chinese patent CN108807876A discloses a method for preparing a modified carbon negative electrode material for a lithium-ion battery. The method first uses a hard carbon precursor to soak in a boric acid solution, and then uses asphalt to coat and graphitize it after drying to obtain a composite material. When the graphitization temperature rises to 2300°C, the protective gas is replaced with chlorine. Chlorine is a highly toxic gas and is not conducive to industrial production. At the same time, the first coulomb efficiency of the negative electrode material prepared by this method is low, which is difficult to meet the requirements of commercial high-energy power sources.
[0005] To this end, the present invention intends to compound carbon, nitrogen and boron into a carbon-nitrogen-boron (CNB) ternary negative electrode material to give it higher capacity characteristics and rate performance, thereby achieving higher energy density, better rate performance and longer cycle life for lithium-ion batteries. Summary of the invention
[0006] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing a carbon-nitrogen-boron ternary negative electrode material with a simple and environmentally friendly preparation process, low cost, and suitable for industrial production; and to provide a negative electrode material that can improve the material specific capacity and has excellent rate performance, thereby improving the energy density and rate performance of lithium-ion batteries.
[0007] In order to solve the above technical problems, the present invention provides a porous artificial graphite precursor prepared by a CVD rotary coating furnace, and ammonia borane containing nitrogen and boron elements is introduced into the porous artificial graphite precursor to form a carbon-nitrogen-boron ternary negative electrode material after a high-temperature reaction, and the carbon-nitrogen-boron ternary negative electrode material is used to make a battery negative electrode and a lithium-ion battery.
[0008] The present invention first provides a carbon-nitrogen-boron ternary negative electrode material. A porous artificial graphite negative electrode material precursor is first prepared with artificial graphite micropowder, and then ammonia borane is mixed with the porous artificial graphite negative electrode material precursor. After high-temperature reaction, a carbon-nitrogen-boron ternary negative electrode material with a porous surface structure is formed. The porosity of the carbon-nitrogen-boron ternary negative electrode material is 1% to 35%, graphite is 80wt% to 95wt%, boron element is 2wt% to 15wt%, and nitrogen element is 2wt% to 15wt%.
[0009] The present invention also provides a method for preparing a carbon-nitrogen-boron ternary negative electrode material, comprising the following steps:
[0010] Step 1: artificial graphite powder is selected as raw material, the artificial graphite powder is placed in a CVD rotary coating furnace, protective gas and surface pore-forming carbon source gas are introduced, the furnace body is heated and rotated, and after the reaction is completed, the furnace is cooled to obtain a porous artificial graphite precursor;
[0011] Step 2: adding the porous artificial graphite precursor and the ammonia borane solution into a reaction kettle in proportion, stirring and dispersing them, so that the ammonia borane is introduced into the mesopores on the surface of the porous artificial graphite precursor;
[0012] Step 3: The reactor is continuously stirred and heated, and the porous artificial graphite precursor and ammonia borane blend in step 2 are continuously stirred, dispersed and carbonized at high temperature, so that ammonia borane undergoes a series of dehydrogenation reactions, and ammonia borane decomposes nitrogen and boron elements to obtain a carbon-nitrogen-boron (CNB) ternary negative electrode material.
[0013] As a preferred preparation method of the present invention, in step 1, the artificial graphite powder accounts for 100%wt, as a raw material for making a porous artificial graphite precursor, the median particle size D50: 2um~6um, the specific surface area is 3㎡ / g~8㎡ / g, the purity is ≥99.9%, the first coulomb efficiency is 85%~92%, the first discharge gram capacity is 340mAh / g~350mAh / g, and the tap density is 0.7g / cm 3 ~1.0g / cm 3 .
[0014] Preferably, the equipment for making the porous graphite negative electrode precursor is a CVD vapor deposition carbon coating rotary furnace, the CVD rotary coating furnace has a specification of φ300*1000, a volume of 70L, a furnace speed of 0.1r / min~10r / min, a maximum operating temperature of 1200°C, and the equipment is suitable for the following gases: nitrogen, argon, methane, acetylene, ammonia;
[0015] Preferably, the micron-sized artificial graphite powder is placed in a CVD vapor deposition carbon coating rotary kiln.
[0016] As a preferred embodiment of the preparation method of the present invention, in step 1, the surface pore-forming carbon source gas is one of acetylene, acetylene, methane, and carbon monoxide, and the purity of the surface pore-forming carbon source is ≥98%; the protective gas is nitrogen or argon, and the purity of the protective gas is ≥99.9%.
[0017] As a preferred preparation method of the present invention, the furnace speed is 0.1r / min~1r / min, the furnace temperature is 850℃~1200℃, the constant temperature time is 1h~3h, the amount of surface pore-forming carbon source gas introduced is 1L / min~8L / min, the amount of protective gas introduced is 1L / min~8L / min, and a porous artificial graphite precursor is obtained after the material is cooled.
[0018] As a preferred embodiment of the preparation method of the present invention, in step 2, the porous artificial graphite precursor accounts for 65wt% to 90wt%.
[0019] As a preferred preparation method of the present invention, in step 2, the ammonia borane solution is prepared according to the following method: ammonia borane and N-methylpyrrolidone solvent are mixed, stirred and dissolved to obtain an ammonia borane solution, wherein the proportion of ammonia borane in the ammonia borane solution is 2wt% to 40wt%, and the porous artificial graphite precursor and the ammonia borane solution are added to the reactor and stirred and dispersed.
[0020] As a preferred preparation method of the present invention, in step three, it is preferred to use a reactor with a rotation speed of 1r / min to 110r / min, a maximum heating temperature of 1000°C, and a function of introducing protective gases such as nitrogen and argon. The porous artificial graphite precursor and the ammonia borane solution can be continuously stirred and dispersed at the same time. The high-speed stirring can fully disperse the porous artificial graphite and the ammonia borane blend evenly, and the ammonia borane is dissolved and infiltrated into the mesopores on the surface of the porous artificial graphite precursor. The continuous stirring and dispersing process is assisted by heating. During the process, high-purity nitrogen or argon is introduced, and the gas introduction rate is 1000L / h to 3500L / h, so that the kettle is in a slightly positive pressure state, so that the ammonia borane undergoes a series of dehydrogenation reactions, and the ammonia borane decomposes nitrogen and boron elements and is enriched on the surface of the porous artificial graphite. As the temperature of the reactor continues to rise to 1000°C, the materials in the reactor are carbonized to obtain a carbon-nitrogen-boron (CNB) ternary negative electrode material.
[0021] As a preferred embodiment of the preparation method of the present invention, the continuous heating temperature curve and the stirring and dispersing speed are as follows: uniformly heating from room temperature to 150°C for 60 minutes, maintaining the temperature for 60 minutes, and stirring and dispersing at a speed of 100 r / min; uniformly heating from 150°C to 350°C for 120 minutes, maintaining the temperature for 180 minutes, and stirring and dispersing at a speed of 80 r / min; uniformly heating from 350°C to 850°C for 120 minutes, maintaining the temperature for 200 minutes, and stirring and dispersing at a speed of 45 r / min.
[0022] The present invention also provides a battery negative electrode, the active material of which adopts the carbon-nitrogen-boron ternary negative electrode material as described above or the carbon-nitrogen-boron ternary negative electrode material prepared by the preparation method.
[0023] The present invention also provides a lithium ion battery, the negative electrode of which adopts the battery negative electrode as described above.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The preparation method is simple and environmentally friendly. The porous artificial graphite precursor is prepared by using a CVD vapor deposition carbon-coated rotary kiln, and the reactor simultaneously completes the stirring, dispersion, heating decomposition, and high-temperature carbonization of the ammonia borane solution and the porous artificial graphite precursor, avoiding the use of corrosive or toxic solvent raw materials, which will cause pollution. The process of the present invention only requires three steps, in which stirring, dispersion, heating, and high-temperature carbonization are carried out in the same equipment, and the process is simple and easy to implement.
[0026] 2. Low cost and suitable for industrial production. Only three raw materials are used in the preparation, and the raw materials for making porous artificial graphite precursors are by-products in the production process of lithium battery negative electrode materials. They are low-cost and easy to obtain. The process preferably uses CVD vapor deposition carbon-coated rotary kilns and reactors, which are commercially available equipment. General battery material manufacturing companies have the above equipment, and no special customized equipment is required, making it suitable for industrial production.
[0027] 3. Greatly improve the specific capacity and rate performance of the material. The carbon-nitrogen-boron ternary negative electrode material prepared by the present invention increases the active sites in the negative electrode and the electronegativity of the material by introducing nitrogen and boron elements, and also enhances the negative electrode's ability to resist Li + The material has excellent adsorption capacity and excellent conductivity. Due to its abundant pores, unique structure and co-doping of nitrogen and boron elements, CNB exhibits excellent lithium storage performance, especially the long cycle performance under high current density is significantly improved. Compared with traditional graphite negative electrode materials, it shows higher specific capacity and excellent rate performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the specific implementation of the present invention or the technical solution in the prior art, the drawings required for describing the specific implementation or the prior art will be briefly introduced below. Obviously, the drawings described below are only one implementation of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0029] Figure 1 This is a SEM image of the material obtained in Example 1 of the present invention;
[0030] Figure 2 This is a SEM image of the material obtained in Example 2 of the present invention;
[0031] Figure 3 This is a SEM image of the material obtained in Example 3 of the present invention;
[0032] Figure 4 It is the SEM picture of the comparative material in the comparative example of the present invention. DETAILED DESCRIPTION
[0033] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the technical scheme in the specific implementation mode of the present invention is clearly and completely described below to further illustrate the present invention. Obviously, the specific implementation mode described is only a part of the implementation mode of the present invention, rather than all styles.
[0034] In order to further illustrate the advantages of the method of the present invention, the present invention uses the following methods and equipment to test the conventional materials prepared in the examples and comparative examples respectively:
[0035]
[0036] In the embodiment, the specifications of the CVD vapor deposition carbon-coated rotary furnace are: φ300*1000, the volume is 70L, the furnace speed is 0.1r / min~10r / min, the maximum working temperature is 1200℃, and the equipment is suitable for the following gases: nitrogen, argon, methane, acetylene, and ammonia.
[0037] In the embodiment, the specifications of the reactor are: vertical, with a rotation speed of 1 r / min to 110 r / min, a maximum heating temperature of 1000° C., and a function of introducing protective gases such as nitrogen and argon.
[0038] Comparative Example
[0039] The graphite negative electrode material used in the comparative example of the present invention adopts the LT-PSH product produced by Rongtan Technology (hereinafter referred to as comparative material). The test results of the comparative material discharge specific capacity, initial coulomb efficiency, and powder compaction density are shown in Table 1. The cycle capacity retention rate of the full battery pole at 3C charge and 1C discharge rate is shown in Table 2. The SEM image of the comparative material is shown in Figure 4 shown.
[0040] Example 1
[0041] A carbon-nitrogen-boron ternary negative electrode material, the preparation method of which mainly comprises the following steps:
[0042] Step 1, preparation of porous artificial graphite precursor: artificial graphite powder is placed in a CVD rotary coating furnace, the furnace speed is set to 0.5r / min, the furnace temperature is uniformly increased from room temperature to 850°C for 120min and then kept constant for 120min, nitrogen and acetylene gas are introduced simultaneously during the whole process, the gas flow rate is 3L / min, acetylene purity: ≥98%, nitrogen purity ≥99.9%.
[0043] Among them, artificial graphite powder accounts for 100%wt. As the raw material for making porous stone artificial graphite precursor, the median particle size D50: 4um, the specific surface area is 3㎡ / g, the purity is ≥99.9%, the first coulomb efficiency is 92%, the first discharge capacity is 342mAh / g, and the tap density is 0.94g / cm 3 .
[0044] Step 2: prepare a blend of porous stone artificial ink precursor and ammonia borane solution: add ammonia borane and N-methylpyrrolidone solvent into a reactor and stir at a speed of 70 r / min for 90 min to dissolve and obtain an ammonia borane solution, wherein the ammonia borane accounts for 20 wt % of the ammonia borane solution.
[0045] Subsequently, the porous artificial graphite precursor was added into the ammonia borane solution, the proportion of the porous artificial graphite precursor was 50wt%, and the reactor was rotated at 90r / min and stirred for 120min to obtain a blend.
[0046] Among them, the density of ammonia borane is 0.78g / cm 3 ; N-methylpyrrolidone solvent purity ≥99.9%.
[0047] Step 3, high temperature carbonization: The porous stone artificial ink precursor prepared in step 2 and the ammonia borane solution mixture are continuously stirred and heated until carbonized. During the process, high-purity nitrogen is introduced at a gas flow rate of 2500 L / h, so that the reactor is in a slightly positive pressure state. The high temperature carbonization parameters are as follows:
[0048] The room temperature was raised uniformly to 150°C for 60 min, and kept at this temperature for 60 min, with a stirring and dispersion speed of 100 r / min;
[0049] Heating at a constant speed of 150℃ for 120min to 350℃, maintaining constant temperature for 180min; stirring and dispersing at a speed of 80r / min;
[0050] Rise the temperature at a constant speed from 350°C for 120 min to 850°C, and keep the temperature constant for 200 min; stir and disperse at a speed of 45 r / min.
[0051] After high-temperature carbonization is completed, the carbon-nitrogen-boron ternary negative electrode material is prepared.
[0052] The porosity of the prepared carbon-nitrogen-boron ternary negative electrode material is 15%, graphite is 92wt%, boron element is 4wt%, and nitrogen element is 4wt%.
[0053] After testing, the discharge specific capacity, first coulomb efficiency, and powder compaction density test results of the carbon-nitrogen-boron ternary negative electrode material prepared in this embodiment are shown in Table 1, and the cycle capacity retention rate of the full battery at a 3C charge and 1C discharge rate is shown in Table 2. Its SEM image is shown in Figure 1 shown.
[0054] Example 2
[0055] A carbon-nitrogen-boron ternary negative electrode material, the preparation method of which mainly comprises the following steps:
[0056] Step 1, preparation of porous artificial graphite precursor: artificial graphite powder is placed in a CVD rotary coating furnace, the furnace speed is set to 1r / min, the furnace temperature is uniformly increased from room temperature to 900°C for 150min and then kept constant for 90min, nitrogen and acetylene gas are introduced simultaneously during the whole process, the gas flow rate is 4L / min, acetylene purity: ≥98%, nitrogen purity ≥99.9%.
[0057] Among them, artificial graphite powder accounts for 100%wt. As the raw material for making porous stone artificial graphite precursor, the median particle size D50: 3um, the specific surface area is 5㎡ / g, the purity is ≥99.9%, the first coulomb efficiency is 90%, the first discharge capacity is 343mAh / g, and the tap density is 0.90g / cm 3 .
[0058] Step 2: prepare a blend of porous stone artificial ink precursor and ammonia borane solution: add ammonia borane and N-methylpyrrolidone solvent into a reactor and stir at a speed of 80 r / min for 100 min to dissolve and obtain an ammonia borane solution, wherein the ammonia borane accounts for 25 wt % of the ammonia borane solution.
[0059] Subsequently, the porous artificial graphite precursor was added into the ammonia borane solution, the porous artificial graphite precursor accounted for 55 wt %, and the reactor was stirred at a speed of 95 r / min for 150 min to obtain a blend.
[0060] Among them, the density of ammonia borane is 0.78g / cm 3 ; N-methylpyrrolidone solvent purity ≥99.9%.
[0061] Step 3, high temperature carbonization: The porous stone artificial graphite precursor prepared in step 2 and the ammonia borane solution mixture are continuously stirred and heated until carbonized. During the process, high-purity nitrogen is introduced at a gas flow rate of 3000 L / h, so that the reactor is in a slightly positive pressure state. The high temperature carbonization parameters are as follows:
[0062] The room temperature was raised uniformly to 150°C for 60 min, and kept at this temperature for 60 min, with a stirring and dispersion speed of 100 r / min;
[0063] Heating at a constant speed of 150℃ for 120min to 350℃, maintaining constant temperature for 180min; stirring and dispersing at a speed of 80r / min;
[0064] Rise the temperature at a constant speed from 350°C for 120 min to 850°C, and keep the temperature constant for 200 min; stir and disperse at a speed of 45 r / min.
[0065] After high-temperature carbonization is completed, the carbon-nitrogen-boron ternary negative electrode material is prepared.
[0066] The porosity of the prepared carbon-nitrogen-boron ternary negative electrode material is 18%, graphite is 94%, boron element is 3wt%, and nitrogen element is 3wt%.
[0067] After testing, the discharge specific capacity, first coulomb efficiency, and powder compaction density test results of the carbon-nitrogen-boron ternary negative electrode material prepared in this embodiment are shown in Table 1, and the cycle capacity retention rate of the full battery at a 3C charge and 1C discharge rate is shown in Table 2. Its SEM image is shown in Figure 2 shown.
[0068] Example 3
[0069] A carbon-nitrogen-boron ternary negative electrode material, the preparation method of which mainly comprises the following steps:
[0070] Step 1, preparation of porous artificial graphite precursor: artificial graphite powder is placed in a CVD rotary coating furnace, the furnace speed is set to 1.5r / min, the furnace temperature is uniformly increased from room temperature to 950°C for 150min and then kept constant for 60min, nitrogen and acetylene gas are introduced simultaneously during the whole process, the gas flow rate is 5L / min, acetylene purity: ≥98%, nitrogen purity ≥99.9%.
[0071] Among them, artificial graphite powder accounts for 100%wt. As the raw material for making porous stone artificial graphite precursor, the median particle size D50: 5um, the specific surface area is 3㎡ / g, the purity is ≥99.9%, the first coulomb efficiency is 92%, the first discharge capacity is 345mAh / g, and the tap density is 0.97g / cm 3 .
[0072] Step 2: prepare a blend of porous stone artificial ink precursor and ammonia borane solution: add ammonia borane and N-methylpyrrolidone solvent into a reactor and stir at a speed of 90 r / min for 60 min to dissolve and obtain an ammonia borane solution, wherein the ammonia borane accounts for 30 wt % of the ammonia borane solution.
[0073] Subsequently, the porous artificial graphite precursor was added into the ammonia borane solution, the porous artificial graphite precursor accounted for 60wt%, and the reactor was stirred at a speed of 100r / min for 180min to obtain a blend.
[0074] Among them, the density of ammonia borane is 0.78g / cm 3 ; N-methylpyrrolidone solvent purity ≥99.9%.
[0075] Step 3, high temperature carbonization: The porous stone artificial ink precursor prepared in step 2 and the ammonia borane solution mixture are continuously stirred and heated until carbonized. During the process, high-purity nitrogen is introduced at a gas flow rate of 3500 L / h, so that the reactor is in a slightly positive pressure state. The high temperature carbonization parameters are as follows:
[0076] The room temperature was raised uniformly to 150°C for 60 min, and kept at this temperature for 60 min, with a stirring and dispersion speed of 100 r / min;
[0077] Heating at a constant speed of 150℃ for 120min to 350℃, maintaining constant temperature for 180min; stirring and dispersing at a speed of 80r / min;
[0078] Rise the temperature at a constant speed from 350°C for 120 min to 850°C, and keep the temperature constant for 200 min; stir and disperse at a speed of 45 r / min.
[0079] After high-temperature carbonization is completed, the carbon-nitrogen-boron ternary negative electrode material is prepared.
[0080] The porosity of the prepared carbon-nitrogen-boron ternary negative electrode material is 25%, graphite is 95wt%, boron element is 2.5wt%, and nitrogen element is 2.5wt%.
[0081] After testing, the discharge specific capacity, first coulomb efficiency, and powder compaction density test results of the carbon-nitrogen-boron ternary negative electrode material prepared in this embodiment are shown in Table 1, and the cycle capacity retention rate of the full battery at a 3C charge and 1C discharge rate is shown in Table 2. Its SEM image is shown in Figure 3 shown.
[0082] Table 1 Test results of discharge specific capacity, first coulombic efficiency and powder compaction density
[0083]
[0084] Table 2 Full battery 3C charge 1C discharge rate cycle capacity retention rate
[0085]
[0086] From Table 1, Table 2 and Figure 1-3 It can be seen that the carbon-nitrogen-boron ternary negative electrode material prepared in the embodiment of the present invention has significantly better specific capacity and compaction density than the comparative material, and is significantly better than the comparative material in rate cycle life, indicating that the carbon-nitrogen-boron ternary negative electrode material prepared by the method of the present invention meets the expected requirements.
[0087] The above describes the main technical features and basic principles of the present invention and the related advantages. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the concept or basic features of the present invention. Therefore, no matter from which point of view, the above specific embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention.
[0088] In addition, it should be understood that although the present specification is described according to various implementation methods, not every implementation method contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation method may also be appropriately combined to form other implementation methods that can be understood by those skilled in the art.
Claims
1. A carbon-nitrogen-boron ternary negative electrode material, It is characterized in that First, a porous artificial graphite negative electrode material precursor is prepared with artificial graphite micropowder, and then ammonia borane is mixed with the porous artificial graphite negative electrode material precursor, and a carbon-nitrogen-boron ternary negative electrode material with a porous surface structure is formed after a high-temperature reaction. The porosity of the carbon-nitrogen-boron ternary negative electrode material is 1% to 35%, graphite is 80wt% to 95wt%, boron is 2wt% to 15wt%, and nitrogen is 2wt% to 15wt%.
2. A method for preparing a carbon-nitrogen-boron ternary negative electrode material, It is characterized in that The steps include: Step 1: Put artificial graphite powder into a CVD rotary coating furnace, introduce protective gas and surface pore-forming carbon source gas, heat up and rotate the furnace, cool after the reaction is completed, and obtain a porous artificial graphite precursor; Step 2: adding the porous artificial graphite precursor and the ammonia borane solution into a reaction kettle in proportion, stirring and dispersing them, so that the ammonia borane is introduced into the mesopores on the surface of the porous artificial graphite precursor; Step 3: The porous artificial graphite precursor and ammonia borane blend in step 2 are continuously stirred, dispersed and carbonized at high temperature, so that ammonia borane undergoes a series of dehydrogenation reactions to decompose nitrogen and boron elements, thereby obtaining a carbon-nitrogen-boron ternary negative electrode material.
3. The method for preparing a carbon-nitrogen-boron ternary negative electrode material according to claim 2, It is characterized in that In step 1, the artificial graphite powder accounts for 100%wt, the median particle size D50: 2um~6um, the specific surface area is 3㎡ / g~8㎡ / g, the purity is ≥99.9%, the first coulomb efficiency is 85%~92%, the first discharge capacity is 340mAh / g~350mAh / g, and the tap density is 0.7g / cm 3 ~1.0g / cm 3 .
4. The method for preparing a carbon-nitrogen-boron ternary negative electrode material according to claim 2, It is characterized in that In step one, The surface pore-forming carbon source gas is one of acetylene, methane and carbon monoxide, and the purity of the surface pore-forming carbon source is ≥98%; The protective gas is nitrogen or argon, and the purity of the protective gas is ≥99.9%.
5. The method for preparing a carbon-nitrogen-boron ternary negative electrode material according to claim 2, It is characterized in that The furnace speed is 0.1r / min~1r / min, the furnace temperature is 850℃~1200℃, the constant temperature time is 1h~3h, the amount of surface pore-forming carbon source gas introduced is 1L / min~8L / min, and the amount of protective gas introduced is 1L / min~8L / min.
6. The method for preparing a carbon-nitrogen-boron ternary negative electrode material according to claim 2, It is characterized in that In step 2, the porous artificial graphite precursor accounts for 65wt% to 90wt%; The ammonia borane solution is prepared by mixing and stirring ammonia borane and N-methyl pyrrolidone solvent to dissolve the ammonia borane, and the proportion of ammonia borane in the ammonia borane solution is 2 wt% to 40 wt%.
7. The method for preparing a carbon-nitrogen-boron ternary negative electrode material according to claim 2, It is characterized in that In step three, high-purity nitrogen or argon is introduced to place the reactor in a slightly positive pressure state, and the gas introduction rate is 1000L / h to 3500L / h.
8. The method for preparing a carbon-nitrogen-boron ternary negative electrode material according to claim 7, It is characterized in that The continuous heating temperature curve and stirring and dispersing speed are: The room temperature was raised uniformly to 150°C for 60 min, and kept at this temperature for 60 min, with a stirring and dispersion speed of 100 r / min; Heating at a constant speed of 150°C for 120 min to 350°C, maintaining constant temperature for 180 min, stirring and dispersing at a speed of 80 r / min; Rise the temperature at a constant speed from 350°C for 120 min to 850°C, keep the temperature constant for 200 min, and stir and disperse at a speed of 45 r / min.
9. A negative electrode of a battery, It is characterized in that The active material of the negative electrode adopts a carbon-nitrogen-boron ternary negative electrode material as claimed in claim 1 or a carbon-nitrogen-boron ternary negative electrode material prepared by any preparation method as claimed in any one of claims 2 to 8.
10. A lithium ion battery, It is characterized in that The negative electrode thereof adopts the negative electrode of the battery as claimed in claim 9.
Citation Information
Patent Citations
Method for preparing modified carbon cathode material for lithium ion battery
CN108807876A
A boron- and nitrogen-doped lithium-ion battery anode material and its preparation method
CN110911665B
Method for producing carbon cathode material of composite coated lithium ion battery
CN103441251A
A boron-doped negative electrode material with good high-temperature performance and a solid-phase preparation method thereof
CN109148843A