A method for preparing micro-nano structure in one step, micro-nano structure and application thereof

Through the hydrothermal reaction of liquid metal in the micro-pit array structure, the one-step preparation of micro-nano structures is achieved, which solves the problem of multi-step process, reduces the cost and controls the particle size, and is suitable for the fields of superhydrophobicity and light absorption.

CN116022839BActive Publication Date: 2024-10-22TECHNICAL INST OF PHYSICS & CHEMISTRY - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111248338.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-26
Publication Date
2024-10-22
Estimated Expiration
2041-10-26

AI Technical Summary

Technical Problem

The existing technology usually requires a multi-step process when preparing micro-nano structures, which increases experimental steps and costs, making it difficult to achieve one-time preparation.

Method used

By placing liquid metal in a micro-pit array structure and performing a hydrothermal reaction in a metal salt solution, the phase change of the liquid metal and the volume expansion caused by hydrogen production are used to achieve the one-step preparation of micro-nano structures.

Benefits of technology

It achieves rapid and low-cost preparation of micro-nanostructures, can control the size of solid particles, and has applications in the fields of superhydrophobicity and light absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116022839B_ABST
    Figure CN116022839B_ABST
Patent Text Reader

Abstract

The present invention provides a preparation method for preparing a micro-nano structure, a micro-nano structure and an application thereof. The preparation method of the present invention comprises: 1) placing liquid metal in micro-pits of a micro-pit array structure; 2) placing the micro-pit array structure with liquid metal in step 1) in a metal salt aqueous solution, performing a hydrothermal reaction, and obtaining solid particles having a micro-nano structure. The preparation method of the present invention can prepare micro-nano structures in one step, can effectively improve the preparation speed of micro-nano structures, and reduce the preparation cost of micro-nano materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of material preparation, and in particular to a method for preparing a micro-nano structure in one step, the micro-nano structure and applications thereof. Background Art

[0002] The special structural effects of micro-nano structures play an irreplaceable role in many fields. For example, the self-cleaning function of the lotus leaf surface is mainly caused by the surface micro-nano structure. In the process of preparing micro-nano structures, many studies first prepare micron-scale structures and then design nanostructures, which increases the steps and costs of the experiment. Summary of the invention

[0003] In order to simplify the experimental process and realize the one-step preparation of micro-nano structures, the present invention provides a one-step preparation method of micro-nano structures, micro-nano structures and applications thereof. Through this method, micro-nano structures can be quickly prepared.

[0004] The present invention provides a method for preparing a micro-nano structure, which comprises: 1) placing liquid metal in micro-pits of a micro-pit array structure; 2) placing the micro-pit array structure with liquid metal in step 1) in a metal salt aqueous solution, performing a hydrothermal reaction, and obtaining solid particles with a micro-nano structure.

[0005] According to an embodiment of the present invention, in step 2), the liquid metal expands in situ in the micropits to obtain solid particles having a micro-nano structure.

[0006] According to an embodiment of the present invention, when liquid metal is heated in a metal salt aqueous solution to undergo a hydrothermal reaction, the liquid metal reacts with hydrogen ions in the aqueous solution to generate metal hydroxides and oxides, thereby producing a phase change from liquid to solid; during the phase change of the liquid metal, the generation of hydrogen will also cause the internal porous structure to form. The phase change of the liquid metal and the generation of hydrogen will both cause the liquid metal to expand in volume during the hydrothermal reaction, thereby expanding out of the micro-pits. The surface of this expanded microsphere then provides a seed for the growth of the nanostructure, thereby generating a nanostructure on its surface.

[0007] Preferably, the microspheres have a hollow porous spherical structure.

[0008] According to an embodiment of the present invention, the liquid metal is selected from a gallium-based liquid metal alloy or a bismuth-based liquid metal alloy. For example, the gallium-based liquid metal is selected from a gallium-indium liquid metal alloy, wherein the mass ratio of gallium metal to indium metal is, for example, 10:1 to 3:1. For example, the gallium-based liquid metal may also be gallium-indium-tin, wherein the mass ratio of gallium metal, indium metal, and tin metal may be 10:1:0.1 to 10:1:1 or 75:25:0.1 to 75:25:1.

[0009] Exemplarily, the gallium-indium liquid metal alloy is GaIn10 or GaIn24.5, and its melting point is 15°C±2°C.

[0010] According to an embodiment of the present invention, the size of the micropits in the micropit array structure and the amount of liquid metal in the micropits can determine the particle size of the prepared solid particles with micro-nano structures.

[0011] According to an embodiment of the present invention, the size of the micropits is not particularly limited. Those skilled in the art can appropriately select the size of the micropits based on the size of the micro-nanoparticles to be prepared. For example, the average diameter of the micropits can be 1 μm-8 mm, such as 2 μm-5 mm, for example, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 200 μm, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, 1 mm.

[0012] Preferably, the average diameter of the micropits is 5-200 μm.

[0013] According to an embodiment of the present invention, the spacing of the micropits is not particularly limited, for example, it can be 0.1 μm-8 mm, such as 0.5 μm-5 mm, such as 1 μm-1 mm. Preferably, the spacing of the micropits is 0.1-200 μm. The spacing of the micropits in the present invention refers to the average distance between the center points of two adjacent micropits in the micropit array structure.

[0014] According to an embodiment of the present invention, the micro-pit array structure can be prepared by methods known in the prior art, for example, by replicating, machining or 3D printing technology.

[0015] According to an embodiment of the present invention, the replica method can replicate the structure of a lotus leaf, for example, by spreading a replica material (such as silica gel and a curing agent) on the surface of a lotus leaf and curing it to obtain a micro-pit array structure.

[0016] According to an embodiment of the present invention, in step 1), liquid metal is spread on the surface of the micro-pit array structure above its melting point, and the liquid metal enters the micro-pits.

[0017] According to an embodiment of the present invention, in step 2), the temperature of the hydrothermal reaction is, for example, 60-150°C, preferably 70-120°C, for example, 70°C, 80°C, 90°C, 100°C, 110°C, 120°C.

[0018] According to an embodiment of the present invention, in step 2), the time of the hydrothermal reaction is 1-20 hours, for example, 1-10 hours. The pressure of the hydrothermal reaction is, for example, atmospheric pressure.

[0019] According to an embodiment of the present invention, in step 2), the metal salt is selected from at least one of zinc salts, silver salts or copper salts, for example, selected from at least one of zinc nitrate, silver nitrate or copper nitrate, preferably zinc nitrate.

[0020] According to an embodiment of the present invention, the aqueous metal salt solution may further contain hexamethylenetetramine.

[0021] According to an embodiment of the present invention, the concentration of the aqueous metal salt solution is, for example, 0.001-0.016 g / mL.

[0022] According to an exemplary embodiment of the present invention, the preparation method comprises: placing the micro-pit array structure with liquid metal in step 1) in an aqueous solution containing zinc salt for hydrothermal reaction, and growing zinc oxide with a petal-like structure on the surface of the solid microspheres formed by the liquid metal.

[0023] According to an embodiment of the present invention, the preparation method further comprises: performing surface hydrophobic treatment on the solid particles of the micro-nano structure.

[0024] According to an embodiment of the present invention, the method for treating the surface hydrophobicity includes, for example: treating the micro-nanostructured solid particles with fluorosilane to obtain micro-nanostructured solid particles with super-hydrophobic surfaces. Exemplarily, the fluorosilane is selected from FAS-17.

[0025] Exemplarily, the fluorosilane treatment specifically includes: placing FAS-17 fluorosilane and the micro-nanostructured solid particles in a vacuum dryer, evacuating the vacuum, and then heating while maintaining the vacuum state. For example, the vacuum dryer is 1-10L. For example, the vacuuming time is 5-30 minutes. For example, the heating condition is maintained at 60-90°C for 3-9 hours.

[0026] The present invention also provides solid particles with micro-nano structure prepared by the above method.

[0027] According to an embodiment of the present invention, the solid particles include a hollow porous spherical structure.

[0028] According to an embodiment of the present invention, the surface of the solid particles has a petal-shaped structure.

[0029] According to an embodiment of the present invention, the average particle size of the solid particles is determined by the size of the micropits in the micropit array structure and the amount of liquid metal in the micropits, for example, 1 μm-8 mm, such as 2 μm-5 mm, for example, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, 200 μm, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, 1 mm. Exemplarily, the average particle size of the solid particles is 10-500 μm.

[0030] The present invention also provides applications of the micro-nano structure in the fields of super-hydrophobicity and light absorption.

[0031] Beneficial Effects

[0032] The present invention provides a preparation method for preparing micro-nano structures in one step, which can effectively improve the preparation speed of micro-nano structures, reduce the preparation cost of micro-nano materials, and control the size of solid particles of the prepared micro-nano structures. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of preparing micro-nanospheres by liquid metal in the present invention;

[0034] Figure 2 This is an electron microscope image of the micropore array structure of Example 1;

[0035] Figure 3 This is an electron microscope image of the micro-nanospheres prepared in Example 1;

[0036] Figure 4 The electron microscope images of the micro-nano structures prepared in Examples 2 and 3 are shown. DETAILED DESCRIPTION

[0037] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0038] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0039] Example 1

[0040] (1) First, prepare a micro-pit array structure to replicate the structure of a lotus leaf. Mix the silica gel and curing agent at a mass ratio of 10:1, stir evenly, and spread on the surface of the lotus leaf. Store at 70°C for 50 minutes and solidify. Peel off the lotus leaf to obtain a micro-hole array surface, such as Figure 2 As shown;

[0041] (2) Spreading GaIn10 liquid metal alloy at a melting point of 15°C above the surface of the hole array, and the liquid metal enters the interior of the micropits in the micropit array;

[0042] (3) The micro-pit array structure with liquid metal obtained in step (2) is placed in a reaction kettle, and then a zinc nitrate aqueous solution with a concentration of 0.7 g / 100 mL is added and heated to 90° C. and maintained for 4 hours. The liquid metal expands inside the micro-pit array to obtain micro-nano structured solid particles, whose surface is petal-shaped, such as Figure 3 As shown; EDS test shows that the petal-like structure includes zinc oxide;

[0043] (4) Surface hydrophobic treatment: The micro-nano structured solid particles obtained in step (3) are treated with fluorosilane to obtain micro-nano structured solid particles with super hydrophobic surfaces. The fluorosilane treatment specifically includes:

[0044] 1-3 drops of FAS-17 fluorosilane and the micro-nanostructure obtained in step (3) are placed in a vacuum dryer (1-10 L), evacuated for 5-30 minutes, and then placed in an oven under vacuum and heated at 60-90° C. for 3-9 hours.

[0045] Example 2

[0046] The preparation method of the micro-nanostructured solid particles of this embodiment is the same as that of Embodiment 1, except that the micro-pit array structure is prepared by 3D printing technology, the diameter of the micro-pits is 5 μm, and the average spacing between the micro-pits is 5 μm.

[0047] Example 3

[0048] (1) Micropit array structures with different micropit diameters were prepared by mechanical processing, where the micropit diameters were 200 μm, 120 μm, 80 μm, and 50 μm, respectively; the corresponding average spacing of the micropits was 500 μm.

[0049] (2) spreading GaIn24.5 liquid metal alloy at a melting point of 15° C. or higher on the surface of the micropit array prepared above, and the liquid metal enters the interior of the micropits in the micropit array;

[0050] (3) placing the micro-pit array structure with liquid metal obtained in step (2) into a reaction kettle, adding a 0.7 g / 100 mL zinc nitrate aqueous solution and 0.3 g hexamethylenetetramine, heating to 100° C., and maintaining for 2 hours to obtain solid particles of micro-nano structure;

[0051] (4) Surface hydrophobic treatment: The solid particles of the micro-nano structure obtained in step (3) are treated with fluorosilane to obtain a micro-nano structure with a super-hydrophobic surface. The fluorosilane treatment step is the same as that in Example 1.

[0052] Figure 4 The solid particles with micro-nano structure prepared in Example 2-3 are shown, wherein: Figure 4 The corresponding micropit diameters of ae are 200μm, 120μm, 80μm, 50μm, and 5μm, respectively. Figure 4 f is a partial enlarged view of Figure e.

[0053] The exemplary embodiments of the present invention are described above. However, the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing solid particles with micro-nano structure, characterized in that: The preparation method comprises: 1) placing liquid metal in micropits of a micropit array structure; 2) placing the micropit array structure with liquid metal in step 1) in a metal salt aqueous solution to perform a hydrothermal reaction, wherein the liquid metal expands in volume during the hydrothermal reaction, and a nanostructure is generated on the surface of the expanded microspheres to obtain solid particles with a micro-nanostructure; The metal salt is selected from at least one of zinc salt, silver salt or copper salt; The solid particles include a hollow porous spherical structure; and the surface of the solid particles has a petal-shaped structure.

2. The preparation method according to claim 1, characterized in that: The liquid metal is selected from a gallium-based liquid metal alloy or a bismuth-based liquid metal alloy; The gallium-based liquid metal is selected from gallium-indium liquid metal alloy.

3. The preparation method according to claim 1, characterized in that: The average diameter of the micropits is 1 μm-8 mm.

4. The preparation method according to claim 1, characterized in that The spacing between the micro pits is 0.1 μm-8 mm.

5. The preparation method according to claim 1, characterized in that: In step 1), liquid metal is spread on the surface of the micro-pit array structure above its melting point, and the liquid metal enters the micro-pits; And / or, in step 2), the temperature of the hydrothermal reaction is 60-150°C; And / or, the hydrothermal reaction time is 1-20 hours; And / or, the pressure of the hydrothermal reaction is atmospheric pressure.

6. The preparation method according to claim 1, characterized in that: In step 2), the concentration of the metal salt aqueous solution is 0.001-0.016 g / mL.

7. The preparation method according to claim 1, characterized in that: In step 2), the metal salt is selected from at least one of zinc nitrate, silver nitrate or copper nitrate.

8. The preparation method according to any one of claims 1 to 7, characterized in that: The preparation method further comprises: performing surface hydrophobic treatment on the solid particles having the micro-nano structure; The method for surface hydrophobic treatment comprises: treating the solid particles with micro-nano structure with fluorosilane to obtain solid particles with micro-nano structure whose surface is super-hydrophobic.

9. The preparation method according to claim 1, characterized in that: The preparation method comprises: placing the micro-pit array structure with liquid metal in step 1) in an aqueous solution containing zinc salt for hydrothermal reaction, and growing zinc oxide with a petal-shaped structure on the surface of the solid microspheres formed by the liquid metal.

10. A solid particle with a micro-nano structure, wherein the solid particle with a micro-nano structure is prepared by the method according to any one of claims 1 to 9.