A heterojunction solar cell and its fabrication method

By using a tin oxide layer instead of an ITO layer in a crystalline silicon heterojunction solar cell and connecting the buffer layer to the doped layer, the problem of high indium usage cost is solved, achieving more efficient photoelectric conversion and reduced production costs.

CN116031323BActive Publication Date: 2026-11-17SUZHOU MAXWELL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310067168.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-18
Publication Date
2026-11-17
Estimated Expiration
2043-01-18

AI Technical Summary

Technical Problem

In existing crystalline silicon heterojunction solar cells, the use of rare metal indium (In) in the transparent conductive film results in high costs, and the stability and conductivity of tin oxide transparent conductive film are insufficient, affecting cell efficiency.

Method used

A tin oxide layer is used to replace the ITO layer, and a buffer layer is used to contact the doped layer to reduce the contact resistance. The gate line is formed by electroplating copper, which reduces the use of indium.

Benefits of technology

It reduces production costs, improves photoelectric conversion efficiency and light utilization, simplifies the process, and enhances the corrosion resistance of the transparent conductive film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116031323B_ABST
    Figure CN116031323B_ABST
Patent Text Reader

Abstract

This application relates to a heterojunction solar cell and a method for fabricating the same. The method includes: providing a silicon wafer; the silicon wafer including a first surface and a second surface disposed opposite to each other; depositing a first passivation layer and a first doped layer on the first surface, and depositing a second passivation layer and a second doped layer on the second surface; depositing a first buffer layer on the surface of the first doped layer away from the silicon wafer; depositing a second buffer layer on the surface of the second doped layer away from the silicon wafer; depositing a first tin oxide layer on the surface of the first buffer layer away from the silicon wafer, and depositing a second tin oxide layer on the surface of the second buffer layer away from the silicon wafer, to obtain a first sample of the cell; and electroplating copper onto the first sample to obtain a first cell. This method can reduce production costs, has high reliability, and improves light utilization.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the fields of new energy, photovoltaic and semiconductor technology, and in particular to a heterojunction solar cell and its preparation method. Background Technology

[0002] Due to their higher open-circuit voltage and conversion efficiency, crystalline silicon heterojunction solar cells have attracted significant investment from major domestic photovoltaic companies in recent years. Among these components, the transparent conducting oxide (TCO) film, serving as a lateral carrier transport layer, is an essential part of heterojunction solar cells.

[0003] Currently, the fabrication of double-sided transparent conductive films in crystalline silicon heterojunction solar cells commonly employs magnetron sputtering of ITO (Indium Tin Oxide) targets. As heterojunction solar cell manufacturers continue to expand, the demand for the rare metal indium is increasing, inevitably raising production costs. Furthermore, research has found that during copper electroplating, the plating solution and stripping solution can damage the ITO film, while tin oxide transparent conductive films offer higher stability and lower cost, making them an ideal replacement for ITO. However, due to its low mobility and high bulk resistivity, tin oxide exhibits significant contact resistance with the doped layer, which can significantly reduce the photoelectric conversion efficiency of solar cells, hindering the continued development of heterojunction solar cells.

[0004] To reduce the cost of heterojunction solar cells and decrease the use of indium, there is an urgent need to find a low-cost TCO film with abundant indium content to replace the transparent conductive film containing indium. Summary of the Invention

[0005] Therefore, it is necessary to provide a heterojunction solar cell and its fabrication method to address the above-mentioned technical problems, which can reduce the use of indium and silver and lower costs.

[0006] In a first aspect, this application provides a method for fabricating a heterojunction solar cell. The method includes:

[0007] A silicon wafer is provided; the silicon wafer includes a first surface and a second surface disposed opposite to each other;

[0008] A first passivation layer and a first doped layer are deposited on the first surface, and a second passivation layer and a second doped layer are deposited on the second surface.

[0009] A first buffer layer is deposited on the surface of the first doped layer away from the silicon wafer; a second buffer layer is deposited on the surface of the second doped layer away from the silicon wafer.

[0010] A first tin oxide layer is deposited on the surface of the first buffer layer away from the silicon wafer, and a second tin oxide layer is deposited on the surface of the second buffer layer away from the silicon wafer to obtain the first battery sample;

[0011] The first sample was electroplated with copper to obtain the first battery.

[0012] In one embodiment, the method further includes:

[0013] Masking the main grid of the first cell;

[0014] A first antireflection layer is deposited on the surface of the first tin oxide layer away from the silicon wafer;

[0015] A second antireflection layer is deposited on the surface of the first antireflection layer away from the silicon wafer to obtain the second sample;

[0016] The second sample was surface-treated and encapsulated to obtain the second battery.

[0017] In one embodiment, the thickness of the second buffer layer is less than the thickness of the first buffer layer.

[0018] In one embodiment, the first buffer layer and the second buffer layer are made of different materials.

[0019] In one embodiment, the first antireflective layer is composed of multiple layers of silicon oxide, and the different silicon oxide layers have different refractive indices.

[0020] In one embodiment, the first antireflective layer is composed of multiple layers of silicon oxide, and the different silicon oxide layers have different refractive indices, including:

[0021] The refractive index of the first antireflective layer changes linearly from the side closest to the silicon wafer to the side furthest from the silicon wafer.

[0022] In one embodiment, depositing a first antireflection layer on the surface of the first tin oxide layer away from the silicon wafer includes:

[0023] A first silicon oxide film is deposited on the surface of the first tin oxide layer away from the silicon wafer;

[0024] A second silicon oxide film is deposited on the surface of the first silicon oxide film away from the silicon wafer;

[0025] A third silicon oxide film is deposited on the surface of the second silicon oxide film away from the silicon wafer;

[0026] The refractive indices of the first, second, and third silicon oxide films decrease sequentially.

[0027] In one embodiment, masking the main grid of the first battery includes:

[0028] The main grid of the first cell can be masked by encapsulating tape, or by printing photosensitive adhesive on screen to mask the main grid.

[0029] In one embodiment, surface treatment and encapsulation of the second sample includes:

[0030] Remove the tape or photosensitive adhesive from the surface of the copper grid lines of the second sample.

[0031] Secondly, this application also provides a heterojunction solar cell, which includes:

[0032] A silicon wafer, comprising a first surface and a second surface disposed opposite to each other;

[0033] The first passivation layer is deposited on the first surface;

[0034] The first doped layer is deposited on the surface of the first passivation layer away from the silicon wafer;

[0035] A second passivation layer is deposited on the second surface;

[0036] The second doped layer is deposited on the surface of the second passivation layer away from the silicon wafer;

[0037] The first buffer layer is deposited on the surface of the first doped layer away from the silicon wafer;

[0038] The second buffer layer is deposited on the surface of the second doped layer away from the silicon wafer;

[0039] The first tin oxide layer is deposited on the surface of the first buffer layer away from the silicon wafer;

[0040] A second tin oxide layer is deposited on the surface of the second buffer layer away from the silicon wafer;

[0041] The first electroplated copper electrode is deposited on the surface of the first tin oxide layer away from the silicon wafer;

[0042] The second electroplated copper electrode is deposited on the surface of the second tin oxide layer away from the silicon wafer.

[0043] In one embodiment, the battery further includes:

[0044] The first antireflection layer is deposited on the surface of the first tin oxide layer away from the silicon wafer;

[0045] The second antireflection layer is deposited on the surface of the first antireflection layer away from the silicon wafer.

[0046] The above-described method for preparing a heterojunction solar cell provides a silicon wafer. The silicon wafer includes a first surface and a second surface disposed opposite to each other. A first passivation layer and a first doped layer are deposited on the first surface, and a second passivation layer and a second doped layer are deposited on the second surface. A first buffer layer is deposited on the surface of the first doped layer away from the silicon wafer. A second buffer layer is deposited on the surface of the second doped layer away from the silicon wafer. A first tin oxide layer is deposited on the surface of the first buffer layer away from the silicon wafer, and a second tin oxide layer is deposited on the surface of the second buffer layer away from the silicon wafer, to obtain a first cell sample. The first sample is then electroplated with copper to obtain a first cell. Both the first and second buffer layers serve a buffering function. As a cell buffer layer, by using the buffer layer to contact the double-sided doped layers, the contact resistance is reduced, which is more conducive to the transport of charge carriers. Combined with the tin oxide-based transparent conductive layer (TCO layer), the corrosion resistance is more stable during the copper electroplating process. This not only reduces the use of ITO, but also allows the grid lines to be formed by electroplating, eliminating the need for screen printing silver paste to prepare the grid lines. This reduces production costs, increases reliability, and improves light utilization. Attached Figure Description

[0047] Figure 1 This is a schematic flowchart of a method for fabricating a heterojunction solar cell in one embodiment;

[0048] Figure 2 This is a comparison chart of the effective total transmittance of a heterojunction solar cell and a conventional heterojunction solar cell TCO film in one embodiment.

[0049] Figure 3 This is a schematic flowchart of a method for fabricating a heterojunction solar cell in another embodiment;

[0050] Figure 4 This is a flowchart of a method for fabricating a heterojunction solar cell in one embodiment;

[0051] Figure 5 This is an internal structural diagram of a heterojunction solar cell in one embodiment;

[0052] Figure 6 This is an internal structural diagram of a heterojunction solar cell in another embodiment. Detailed Implementation

[0053] To make the above-mentioned objects, features, and advantages of the present invention more apparent and understandable, specific embodiments of the present invention will be described in detail below with reference to the accompanying drawings. Many specific details are set forth in the following description to provide a thorough understanding of the present invention. However, the present invention can be practiced in many other ways different from those described herein, and those skilled in the art can make similar modifications without departing from the spirit of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0054] In the description of this invention, it should be understood that the terms "center," "longitudinal," "lateral," "length," "width," "thickness," "upper," "lower," "front," "rear," "left," "right," "vertical," "horizontal," "top," "bottom," "inner," "outer," "clockwise," "counterclockwise," "axial," "radial," and "circumferential" indicate the orientation or positional relationship based on the orientation or positional relationship shown in the accompanying drawings. They are used only for the convenience of describing this invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, or be constructed and operated in a specific orientation. Therefore, they should not be construed as limitations on this invention.

[0055] Furthermore, the terms "first" and "second" are used for descriptive purposes only and should not be construed as indicating or implying relative importance or implicitly specifying the number of technical features indicated. Thus, a feature defined as "first" or "second" may explicitly or implicitly include at least one of that feature. In the description of this invention, "a plurality of" means at least two, such as two, three, etc., unless otherwise explicitly specified.

[0056] In this invention, unless otherwise explicitly specified and limited, the terms "installation," "connection," "linking," and "fixing," etc., should be interpreted broadly. For example, they can refer to a fixed connection, a detachable connection, or an integral part; they can refer to a mechanical connection or an electrical connection; they can refer to a direct connection or an indirect connection through an intermediate medium; they can refer to the internal communication of two components or the interaction between two components, unless otherwise explicitly limited. Those skilled in the art can understand the specific meaning of the above terms in this invention according to the specific circumstances.

[0057] In this invention, unless otherwise explicitly specified and limited, "above" or "below" the second feature can mean that the first feature is in direct contact with the second feature, or that the first feature is in indirect contact with the second feature through an intermediate medium. Furthermore, "above," "over," and "on top" of the second feature can mean that the first feature is directly above or diagonally above the second feature, or simply that the first feature is at a higher horizontal level than the second feature. "Below," "below," and "under" the second feature can mean that the first feature is directly below or diagonally below the second feature, or simply that the first feature is at a lower horizontal level than the second feature.

[0058] It should be noted that when an element is referred to as being "fixed to" or "set on" another element, it can be directly on the other element or there may be an intervening element. When an element is considered to be "connected to" another element, it can be directly connected to the other element or there may be an intervening element. The terms "vertical," "horizontal," "upper," "lower," "left," "right," and similar expressions used herein are for illustrative purposes only and do not represent the only possible implementation.

[0059] The main process of heterojunction solar cell fabrication includes: cleaning and texturing the silicon wafer, depositing intrinsic amorphous silicon and doped layers by PECVD (Plasma-enhanced chemical vapor deposition), depositing ITO layers with a thickness of about 80 nm on both sides of the cell, and finally screen printing silver grid line electrodes or electroplating copper electrodes.

[0060] This method requires a large amount of rare metal indium, which increases the process cost in production. In addition, the plating solution and the stripping solution can damage the ITO film during the copper electroplating process. Therefore, there is a need for a method to prepare heterojunction solar cells that can reduce the cost of heterojunction solar cells and reduce the use of indium.

[0061] See Figure 1 , Figure 1 A schematic flowchart of a method for preparing a heterojunction solar cell according to an embodiment of the present invention is shown.

[0062] like Figure 1 As shown, in one embodiment, a method for fabricating a heterojunction solar cell is provided, comprising the following steps:

[0063] Step 102, providing a silicon wafer; the silicon wafer includes a first surface and a second surface disposed opposite to each other.

[0064] In one embodiment, the silicon wafer comprises an n-type monocrystalline silicon wafer.

[0065] In one embodiment, the first surface of the silicon wafer can be the n-side of the silicon wafer, and the second surface of the silicon wafer can be the p-type doped surface of the silicon wafer.

[0066] Step 104: Deposit a first passivation layer and a first doped layer on the first surface, and deposit a second passivation layer and a second doped layer on the second surface.

[0067] In one embodiment, a first passivation layer and a first doped layer are sequentially deposited on a first surface using chemical vapor deposition, and a second passivation layer and a second doped layer are sequentially deposited on a second surface. The materials of the first passivation layer and the second passivation layer can be intrinsic amorphous silicon, intrinsic microcrystalline silicon, or other material layers with passivation effects, as long as the passivation effect is achieved.

[0068] In one embodiment, the conditions required for depositing the first passivation layer and the second passivation layer include: a power supply of 500W, a hydrogen to silane gas flow rate ratio (hydrogen dilution ratio) of 9.5:1, a pressure of 50Pa, and a substrate temperature of 220°C during deposition.

[0069] In one embodiment, the conditions for depositing the first doped layer include: a power supply range of 200W to 500W, a hydrogen to silane gas flow rate ratio (hydrogen dilution ratio) set in the range of 4 to 7, a silane to phosphine gas flow rate ratio (silicon-phosphorus ratio) of 80 to 120, a pressure adjusted in the range of 100 Pa to 130 Pa, and a substrate temperature of 200°C to 230°C during deposition.

[0070] In one embodiment, the conditions for depositing the second doped layer include: a power supply range of 300W to 700W, a hydrogen to silane gas flow rate ratio (hydrogen dilution ratio) of 1 to 4, a silane to phosphine gas flow rate ratio (silicon-phosphorus ratio) of 40 to 70, a pressure range of 45 Pa to 65 Pa, and a substrate temperature range of 200°C to 220°C during deposition.

[0071] In one embodiment, preferably, within the above-mentioned range, the optimal process matching doped layer deposition conditions are preferred.

[0072] In one embodiment, the deposition step may be: depositing a second passivation layer on the second surface of the silicon wafer, performing wafer flipping, sequentially depositing a first passivation layer and a first doped layer on the first surface of the silicon wafer, performing wafer flipping again, and finally depositing a second doped layer on the second passivation layer on the second surface of the silicon wafer.

[0073] Step 106: Deposit a first buffer layer on the surface of the first doped layer away from the silicon wafer; deposit a second buffer layer on the surface of the second doped layer away from the silicon wafer.

[0074] In one embodiment, the first buffer layer and the second buffer layer function as buffer layers.

[0075] In one embodiment, a first buffer layer is deposited on the surface of the first doped layer away from the silicon wafer using an RPD (Reactive Plasma Deposition) apparatus.

[0076] In one embodiment, the first buffer layer includes an ICO (indium cerium oxide) film, an IWO (indium tungsten oxide) film, an IHfO (indium hafnium oxide) film, an ITiO (indium titanium oxide) film, an IMO (indium molybdenum oxide) film, etc., wherein the ICO film ratio (CeO2:In2O3) is adjusted within the range of 0.5wt% to 3wt%, and the IWO film ratio (WO3:In2O3) is adjusted within the range of 1wt% to 5wt%. Considering the influence of the work function of the first buffer layer and the first doped layer on the contact resistance between them, preferably, the material of the first buffer layer is an ICO (In2O3:CeO2 = 99:1wt%) film with a doping ratio of 1% or an IWO (In2O3:WO3 = 97:3wt%) film with a doping ratio of 3%.

[0077] In one embodiment, the thickness of the first buffer layer is 20nm to 30nm. Optionally, the thickness of the first buffer layer can be 20nm, 22nm, 25nm, 28nm, or 30nm.

[0078] In one embodiment, the conditions for depositing the first buffer layer on the surface of the first doped layer away from the silicon wafer include: at room temperature, introducing 30 sccm of argon gas and 1 sccm of argon-hydrogen mixture (hydrogen ratio of 30%), maintaining the chamber pressure at 0.32 Pa, and using a power supply of 2.4 kW.

[0079] In one embodiment, a second buffer layer is deposited on the surface of the second doped layer away from the silicon wafer using a magnetron sputtering deposition apparatus.

[0080] In one embodiment, the second buffer layer comprises an ITO (indium tin oxide) film, wherein the ratio of indium oxide to tin dioxide (In₂O₃:SnO₂) in the ITO film can range from 90:10wt% to 99:1wt%. Considering the influence of the work function of the second buffer layer and the second doped layer on the contact resistance between them, preferably, the material of the second buffer layer is a 5% ITO (In₂O₃:SnO₂ = 95:5wt%) film.

[0081] In one embodiment, the thickness of the second buffer layer is 10nm to 20nm, and the thickness of the second buffer layer can be 10nm, 12nm, 15nm, 18nm, or 20nm.

[0082] In one embodiment, the conditions for depositing a second buffer layer on the surface of the second doped layer away from the silicon wafer include: introducing a mixture of argon, oxygen and hydrogen at room temperature, maintaining the chamber pressure at 0.1 Pa to 5 Pa, and using a power density of 1 kW / m to 10 kW / m.

[0083] Step 108: Deposit a first tin oxide layer on the surface of the first buffer layer away from the silicon wafer, and deposit a second tin oxide layer on the surface of the second buffer layer away from the silicon wafer to obtain the first battery sample.

[0084] In one embodiment, a first tin oxide layer is deposited on the surface of the first buffer layer away from the silicon wafer using a magnetron sputtering deposition apparatus, and a second tin oxide layer is deposited on the surface of the second buffer layer away from the silicon wafer.

[0085] In one embodiment, tin oxide includes various doped tin oxides, including tantalum-doped tin oxide, antimony-doped tin oxide, magnesium-doped tin oxide, etc.

[0086] In one embodiment, the thickness of the first tin oxide layer is 50nm to 60nm, and the thickness of the second tin oxide layer is 60nm to 70nm; optionally, the thickness of the first tin oxide layer can be 50nm, 52nm, 55nm, 58nm, or 60nm; optionally, the thickness of the second tin oxide layer can be 60nm, 62nm, 65nm, 68nm, or 70nm.

[0087] In one embodiment, the first buffer layer and the first tin oxide layer are collectively referred to as the first transparent oxide film, and the second buffer layer and the second tin oxide layer are collectively referred to as the second transparent oxide film. Both the first transparent oxide film and the second transparent oxide film are transparent conductive oxide films.

[0088] In one embodiment, the total thickness of the first buffer layer and the first tin oxide layer is maintained at 80 nm, and the total thickness of the second buffer layer and the second tin oxide layer is maintained at 80 nm.

[0089] In one embodiment, a first tin oxide layer is deposited on the surface of the first buffer layer away from the silicon wafer, a second tin oxide layer is deposited on the surface of the second buffer layer away from the silicon wafer, and a third specified gas is introduced, the third specified gas including argon and an argon-oxygen mixture.

[0090] In one embodiment, the conditions for depositing a first tin oxide layer on the surface of the first buffer layer away from the silicon wafer and depositing a second tin oxide layer on the surface of the second buffer layer away from the silicon wafer include: introducing a mixture of argon and oxygen at room temperature, maintaining the cavity pressure at 0.1 Pa-5 Pa, and having a power density of 1 KW / m-10 KW / m.

[0091] Step 110: Electroplating copper onto the first sample to obtain the first battery.

[0092] In one embodiment, the first sample is annealed under the following conditions: in an air environment, at a temperature of 190°C for 30 minutes.

[0093] In one embodiment, the first sample is subjected to an electroplating copper process.

[0094] In one embodiment, the copper electroplating process includes: first forming a copper seed layer, then spraying photosensitive ink onto both sides of a first sample, wherein the ink thickness is 12 μm; exposing the ink on the first and second surfaces of the first sample using an exposure machine, wherein the linewidth after exposure is 15 μm; developing the sample to obtain the desired pattern, wherein the desired pattern has a linewidth of 15 μm and a depth of 12 μm; the sample entering an electroplating device, electroplating copper electrodes according to the designed pattern to generate copper electrode grid lines with a linewidth of 15 μm and a height of 10 μm; immersing the sample in an ink removal solution to remove all residual ink; then immersing the first sample in an acidic solution for removing the copper seed layer to remove the seed layer copper film, wherein the pH value of the acidic solution is 1-2, the reaction time is 35 seconds, and the reaction solution temperature is 25°C.

[0095] In one embodiment, due to the protective covering of the copper electrode, the seed layer copper film directly beneath the copper electrode, which has a thickness and width of micrometers, can be preserved, while the seed layer copper film with a thickness of nanometers in the remaining area is removed, exposing the first tin oxide layer and the second tin oxide layer.

[0096] In the prior art, the transparent conductive layer material is an ITO layer, on which copper grid lines are directly electroplated. The adhesion between the copper grid lines and the ITO layer is poor, and the film is easy to peel off. Therefore, before the copper electroplating process, a copper seed layer needs to be deposited on the ITO layer using PVD (Physical Vapor Deposition) equipment to improve the adhesion between the subsequent electroplated copper grid lines and the ITO layer.

[0097] In one embodiment, after forming the copper seed layer and performing the copper electroplating process, it is necessary to remove the copper seed layer outside the copper gate lines. This requires an etching process, which can damage the transparent conductive layer and increase the process steps and costs. Therefore, in one embodiment, preferably, due to the presence of the tin oxide layer, it is not necessary to prepare a copper seed layer on the tin oxide layer, and the copper electroplating process can be performed directly. In this embodiment, performing the copper electroplating process directly on the tin oxide layer results in better bonding performance between the copper gate lines and tin oxide, thereby reducing the need for the copper seed layer formation process and subsequent etching process, simplifying the process, and further avoiding damage to the transparent conductive layer caused by the copper seed removal process.

[0098] In the above method for preparing a heterojunction solar cell, a silicon wafer is provided; the silicon wafer includes a first surface and a second surface disposed opposite to each other; a first passivation layer and a first doped layer are deposited on the first surface, and a second passivation layer and a second doped layer are deposited on the second surface; a first buffer layer is deposited on the surface of the first doped layer away from the silicon wafer; a second buffer layer is deposited on the surface of the second doped layer away from the silicon wafer; a first tin oxide layer is deposited on the surface of the first buffer layer away from the silicon wafer, and a second tin oxide layer is deposited on the surface of the second buffer layer away from the silicon wafer, to obtain a first sample of the cell; copper is electroplated onto the first sample to obtain a first cell. By setting the first buffer layer, it is more conducive to the migration of electrons from the N-type microcrystalline silicon layer to the TCO layer. Optionally, the first buffer layer includes an ICO film or an IWO film. The ICO / IWO film has good transmittance and conductivity, and its transmittance combined with the first tin oxide layer is still better than that of the ITO film, which is more conducive to improving the utilization rate of photons.

[0099] Reference Figure 2 This illustrates a comparison of the effective total transmittance of a heterojunction solar cell in one embodiment with that of a conventional heterojunction solar cell. For example... Figure 2 As shown in the figure, the solid line represents the transmittance of the first cell using a combination of the first buffer layer and the first tin oxide layer, while the dashed line represents the transmittance of the cell using the ITO film. It can be seen from the figure that the transmittance of the first cell using the combination of the first buffer layer and the first tin oxide layer exceeds that of the ITO film for different wavelengths.

[0100] Furthermore, the second buffer layer, which is in contact with the second doped layer, further facilitates the migration of holes from microcrystalline silicon to the TCO layer, minimizing the loss caused by light attenuation in the film. Optionally, the second buffer layer includes an ITO film. Contacting the second buffer layer with the second tin oxide layer helps reduce the contact resistance between the tin oxide film and the doped layer, and further improves the fill factor of the heterojunction solar cell. While reducing contact resistance, it also increases mobility, achieving efficient carrier collection. During the copper plating process, the corrosion resistance of the tin oxide transparent conductive film is better than that of the ITO film, which can greatly reduce the degradation of the solar cell. At the same time, the copper plating electrode replaces the silver electrode, reducing production costs.

[0101] In one embodiment, such as Figure 3 As shown, the method for fabricating heterojunction solar cells also includes:

[0102] Step 302: Mask the main grid of the first cell.

[0103] In one embodiment, the main grid of the first battery is masked by a fully automatic tape machine; or photosensitive adhesive is printed using screen printing technology to mask the main grid of the first battery.

[0104] In one embodiment, the main grid of the first cell is masked to prepare for the deposition of the first and second antireflection layers, in order to prevent the main components of the first or second antireflection layers from covering the electrodes and affecting the transport of charge carriers.

[0105] Step 304: Deposit a first antireflection layer on the surface of the first tin oxide layer away from the silicon wafer.

[0106] In one embodiment, a first antireflection layer with a different refractive index is deposited on the surface of the first tin oxide layer away from the silicon wafer using chemical vapor deposition.

[0107] Step 306: Deposit a second antireflection layer on the surface of the first antireflection layer away from the silicon wafer to obtain the second sample.

[0108] In one embodiment, a second antireflective layer is deposited using a vacuum evaporation apparatus.

[0109] In one embodiment, the second antireflective layer comprises a magnesium fluoride film.

[0110] In one embodiment, the step of depositing a second antireflection layer on the surface of the first antireflection layer away from the silicon wafer includes: first evacuating the chamber pressure to 1×10⁻⁶. -3 Pa, turn on the power supply, and pass current through the molybdenum boat. After the deposition rate of the second antireflection layer stabilizes, open the baffle. The deposition rate is 0.5 nm / s, and the deposition thickness is 80 nm to 110 nm. The thickness can be finely adjusted according to the requirements. Specifically, the material of the second antireflection layer can be magnesium fluoride.

[0111] Step 308: Perform surface treatment on the second sample and encapsulate it to obtain the second battery.

[0112] In one embodiment, the adhesive tape or photosensitive adhesive on the surface of the copper grid lines of the second sample is removed by a process to expose the main grid lines. The sample is then placed in an ultra-high temperature sintering furnace and finally encapsulated with a POE (Polyolyaltha Olfin) film.

[0113] In one embodiment, the photosensitive emulsion can be removed using designated equipment, including an exposure machine.

[0114] In one embodiment, the thickness of the first buffer layer is 10nm to 20nm. Optionally, the thickness of the first buffer layer is 10nm, 12nm, 15nm, 18nm, or 20nm.

[0115] During the encapsulation process, the presence of the antireflective layer can better prevent moisture in the air from entering the transparent conductive layer, thus extending the lifespan of the component. At the same time, the contact between the silicon oxide layer and the POE film is better than that between the transparent conductive film and the POE film, resulting in a superior encapsulation effect.

[0116] Compared to the first cell, the second cell includes a double-sided buffer layer and a tin oxide layer, while the second cell includes a thinned first buffer layer, a first tin oxide layer, and two anti-reflection layers. The normalized comparison results of the cell efficiency, open-circuit voltage, short-circuit current, and fill factor of the first cell, the second cell, and the comparative example are shown in Table 1. Compared with the comparative example, the first cell has higher cell efficiency, short-circuit current, and fill factor. Similarly, the second cell is also more advantageous than the comparative example. Both cells have improved in short-circuit current and fill factor, and the second cell performs better. It has significant advantages in cost reduction and improvement of high-efficiency heterojunction solar cell technology.

[0117] Table 1

[0118] project Battery efficiency (%) Open circuit voltage (%) Short-circuit current (%) Fill factor (%) Comparative Example 100 100 100 100 First Battery 101.52 100 101.42 100.10 Second battery 102.76 100 102.58 100.18

[0119] In one embodiment, the thickness of the second buffer layer is less than the thickness of the first buffer layer.

[0120] In one embodiment, a suitable gas pressure, power, and gas ratio are required when depositing a TCO membrane.

[0121] In one embodiment, the thickness of the first buffer layer is 20nm to 30nm, and optionally, the thickness of the first buffer layer is 20nm, 22nm, 24nm, 26nm, 28nm and 30nm; the thickness of the second buffer layer is 10nm to 20nm, and optionally, the thickness of the second buffer layer is 10nm, 12nm, 14nm, 16nm, 18nm and 20nm.

[0122] In one embodiment, the provision of a first buffer layer is more conducive to the migration of electrons from the N-type microcrystalline silicon layer to the TCO layer. The first buffer layer has good transmittance and conductivity, and its transmittance combined with the first tin oxide layer is better than that of the second buffer layer, which is more conducive to improving the utilization rate of photons.

[0123] In one embodiment, a second buffer layer is provided to enable the migration of holes from microcrystalline silicon to the TCO layer, minimizing the loss caused by the attenuation of light by the film layer; the second buffer layer is in contact with the second tin oxide layer, which helps to reduce the contact resistance between the tin oxide film and the doped layer, and is more conducive to improving the fill factor of the heterojunction solar cell. While reducing the contact resistance, the mobility is improved, achieving efficient collection of charge carriers.

[0124] In one embodiment, a mixture of argon and hydrogen is introduced when the first buffer layer is deposited on the surface of the first doped layer away from the silicon wafer.

[0125] In one embodiment, the mobility of the TCO membrane is increased by introducing hydrogen gas.

[0126] In one embodiment, a second buffer layer is deposited on the surface of the second doped layer away from the silicon wafer, and a mixture of argon, oxygen and hydrogen is introduced.

[0127] In one embodiment, the permeability of the TCO membrane is increased by introducing oxygen, and the migration rate of the TCO membrane is increased by introducing hydrogen.

[0128] In one embodiment, using an RPD device requires only argon and hydrogen, while using a magnetron sputtering device to prepare an indium-containing buffer layer requires argon, oxygen, and hydrogen.

[0129] In one embodiment, the first buffer layer and the second buffer layer are made of different materials.

[0130] In one embodiment, the first buffer layer includes an indium cerium oxide film, an indium tungsten oxide film, an indium hafnium oxide film, an indium titanium oxide film, and an indium molybdenum oxide film; the second buffer layer includes an indium tin oxide film.

[0131] In one embodiment, the first antireflective layer is composed of multiple layers of silicon oxide, and the different silicon oxide layers have different refractive indices.

[0132] In one embodiment, the first antireflective layer is composed of multiple layers of silicon oxide, and the different silicon oxide layers have different refractive indices, including:

[0133] The refractive index of the first antireflective layer changes linearly from the side closest to the silicon wafer to the side furthest from the silicon wafer.

[0134] In one embodiment, the conditions for depositing a first antireflection layer with different refractive indices on the surface of the first tin oxide layer away from the silicon wafer include: a substrate temperature of 200°C, a radio frequency of 13.56 MHz, introducing silane and carbon dioxide for reaction, setting the gas flow ratio of silane to carbon dioxide to 1:20, and a radio frequency power of 30W to 200W. By adjusting different gas pressures and gas flow rates, silicon oxide films with different refractive indices are deposited.

[0135] In one embodiment, depositing a first antireflection layer on the surface of the first tin oxide layer away from the silicon wafer includes:

[0136] A first silicon oxide film is deposited on the surface of the first tin oxide layer away from the silicon wafer.

[0137] A second silicon oxide film is deposited on the surface of the first silicon oxide film away from the silicon wafer.

[0138] A third silicon oxide film is deposited on the surface of the second silicon oxide film away from the silicon wafer.

[0139] The refractive indices of the first, second, and third silicon oxide films decrease sequentially.

[0140] In one embodiment, the refractive indices of the first, second, and third silicon oxide films decrease sequentially to meet the requirements of different refractive indices. Through a multilayer antireflection process, silicon oxide is combined with vacuum-deposited magnesium fluoride material, which can further increase the light absorption efficiency of the battery.

[0141] In one embodiment, the refractive index of the first antireflection layer changes linearly from the side closer to the silicon wafer to the side farther away from the silicon wafer. Specifically, by adjusting different gas pressures and gas flow rates, a silicon oxide film with a linearly changing refractive index is deposited, thereby causing the refractive index of the first antireflection layer to gradually decrease from the side closer to the silicon wafer to the side farther away from the silicon wafer.

[0142] In one embodiment, the first antireflective layer comprises three silicon oxide films. The first silicon oxide film has a refractive index of 1.8 and a thickness of 20 nm to 30 nm. Optionally, the thickness of the first silicon oxide film is 20 nm, 22 nm, 24 nm, 26 nm, 28 nm, or 30 nm. The second silicon oxide film has a refractive index of 1.7 and a thickness of 30 nm to 50 nm. Optionally, the thickness of the second silicon oxide film is 30 nm, 32 nm, 34 nm, 36 nm, 38 nm, 40 nm, 42 nm, or 40 nm. The thicknesses are 4nm, 46nm, 48nm, and 50nm; the third silicon oxide film has a refractive index of 1.6 and a thickness of 40nm to 70nm. Optionally, the thickness of the third silicon oxide film is 40nm, 42nm, 44nm, 46nm, 48nm, 50nm, 52nm, 54nm, 56nm, 58nm, 60nm, 62nm, 64nm, 66nm, 68nm, and 50nm; the thickness of the three silicon oxide films is adjusted according to the total thickness of the first buffer layer and the first tin oxide layer.

[0143] In one embodiment, masking the main grid of the first battery includes:

[0144] The main grid of the first cell can be masked by encapsulating tape, or by printing photosensitive adhesive on screen to mask the main grid.

[0145] In one embodiment, surface treatment and encapsulation of the second sample includes:

[0146] Remove the tape or photosensitive adhesive from the surface of the copper grid lines of the second sample.

[0147] In one embodiment, the main grid of the first battery is masked by a fully automatic tape machine; or photosensitive adhesive is printed using screen printing technology to mask the main grid of the first battery.

[0148] In one embodiment, the adhesive tape or photosensitive adhesive on the surface of the copper grid lines of the second sample is removed by a process to expose the main grid lines, which are then placed in an ultra-high temperature sintering furnace and finally encapsulated with a POE film.

[0149] In another embodiment, such as Figure 4 As shown, a method for fabricating a heterojunction solar cell is provided, characterized in that the method includes:

[0150] Step 402, providing a silicon wafer; the silicon wafer includes a first surface and a second surface disposed opposite to each other.

[0151] Step 404: Deposit a first passivation layer and a first doped layer on the first surface, and deposit a second passivation layer and a second doped layer on the second surface.

[0152] Step 406: Deposit a first buffer layer on the surface of the first doped layer away from the silicon wafer; deposit a second buffer layer on the surface of the second doped layer away from the silicon wafer.

[0153] Step 408: Deposit a first tin oxide layer on the surface of the first buffer layer away from the silicon wafer, and deposit a second tin oxide layer on the surface of the second buffer layer away from the silicon wafer to obtain the first battery sample.

[0154] Step 410: Electroplating copper onto the first sample to obtain the first battery.

[0155] Step 412: Mask the main grid of the first cell.

[0156] Step 414: Deposit a first antireflection layer on the surface of the first tin oxide layer away from the silicon wafer.

[0157] Step 416: Deposit a second antireflection layer on the surface of the first antireflection layer away from the silicon wafer to obtain the second sample.

[0158] Step 418: Perform surface treatment on the second sample and encapsulate it to obtain the second battery.

[0159] This method uses PVD equipment to sputter tin oxide-based targets (including all doped tin oxide targets such as tin oxide, tantalum-doped tin oxide, gallium-doped tin oxide, magnesium-doped tin oxide, antimony-doped tin oxide, zirconium-doped tin oxide, etc.), and by adjusting the oxygen / argon ratio, a target with a mobility of 22 cm⁻¹ is prepared. 2 / Vs tin oxide single film. In the electroplating process, tin oxide film is more corrosion resistant and has higher stability than ITO film, making it more suitable as a TCO material for electroplating.

[0160] Furthermore, tin oxide, as a window layer, exhibits higher average transmittance than ITO in the visible light band. However, experimental verification has shown that the interface between tin oxide and the doped layer has a large contact resistance, severely hindering carrier transport and affecting the photoelectric conversion efficiency of the solar cell. Therefore, this method employs PVD to prepare an ultrathin ITO buffer layer of approximately 10 nm to 30 nm, followed by RPD reactive plasma deposition to prepare an ultrathin ICO / IWO buffer layer of approximately 10 nm to 30 nm, and then PVD deposition of a tin oxide film with a thickness of approximately 50 nm to 70 nm. This buffer layer significantly improves the interfacial contact between the doped layer and the tin oxide layer, reducing the production cost of the process.

[0161] In some embodiments, the thickness of the transparent conductive film on the first surface of the light-receiving surface, i.e., the sum of the thicknesses of the buffer layer and the tin oxide layer, can be further reduced. Specifically, while maintaining the conversion efficiency of the solar cell, the thickness of the transparent conductive film on the first surface can be reduced to 20nm-40nm.

[0162] In one embodiment, the thickness of the transparent conductive film on the first surface is 20nm to 40nm. Optionally, the thickness of the transparent conductive film on the first surface can be 20nm, 22nm, 25nm, 28nm, 30nm, 33nm, 35nm, 37nm, or 40nm.

[0163] In one embodiment, the thickness of the buffer layer can be 5nm-15nm, and optionally, the thickness of the buffer layer can be 5nm, 7nm, 10nm, 12nm, or 15nm.

[0164] In this embodiment, a buffer layer of 5nm-15nm and a tin oxide stack structure of varying thicknesses are used, with the total thickness of the buffer layer and tin oxide layer controlled between 20nm-40nm. This significantly reduces the use of target materials and lowers production process costs. After electroplating copper electrodes, an antireflective layer of appropriate thickness and refractive index is deposited. Optimal process conditions are matched with the transparent conductive film on the first surface to further enhance sunlight absorption. Furthermore, the presence of the antireflective layer facilitates POE film encapsulation, with significantly better results than ITO and POE film encapsulation. In the above method, the total thickness of the first buffer layer and the first tin oxide layer is reduced to 20nm-40nm while retaining the first buffer layer. Reducing the thickness of the first buffer layer and the first tin oxide layer improves the longitudinal transport capability of charge carriers. Combined with different antireflective layers, this further enhances photon utilization and facilitates the realization of high current in heterojunction solar cells.

[0165] It should be understood that although the steps in the flowcharts of the embodiments described above are shown sequentially according to the arrows, these steps are not necessarily executed in the order indicated by the arrows. Unless explicitly stated herein, there is no strict order restriction on the execution of these steps, and they can be executed in other orders. Moreover, at least some steps in the flowcharts of the embodiments described above may include multiple steps or multiple stages. These steps or stages are not necessarily completed at the same time, but can be executed at different times. The execution order of these steps or stages is not necessarily sequential, but can be performed alternately or in turn with other steps or at least some of the steps or stages of other steps.

[0166] Based on the same inventive concept, this application also provides a heterojunction solar cell. The implementation scheme for the preparation of this cell is similar to the implementation scheme described in the above method. Therefore, the specific limitations of one or more heterojunction solar cell embodiments provided below can be found in the limitations of the method for preparing heterojunction solar cells above, and will not be repeated here.

[0167] In one embodiment, such as Figure 5 As shown, a heterojunction solar cell is provided, which includes: a silicon wafer 502, a first passivation layer 504, a second passivation layer 506, a first doped layer 508, a second doped layer 510, a first buffer layer 512, a second buffer layer 514, a first tin oxide layer 516, a second tin oxide layer 518, a first electroplated copper electrode 520, and a second electroplated copper electrode 522.

[0168] Silicon wafer 502 includes a first surface and a second surface disposed opposite to each other;

[0169] A first passivation layer 504 and a first doped layer 508 are sequentially deposited on the first surface;

[0170] The second passivation layer 506 and the second doped layer 510 are sequentially deposited on the second surface;

[0171] The first buffer layer 512 is deposited on the surface of the first doped layer 508 away from the silicon wafer;

[0172] The second buffer layer 514 is deposited on the surface of the second doped layer 510 away from the silicon wafer;

[0173] The first tin oxide layer 516 is deposited on the surface of the first buffer layer 512 away from the silicon wafer;

[0174] The second tin oxide layer 518 is deposited on the surface of the second buffer layer 514 away from the silicon wafer;

[0175] The first electroplated copper electrode 520 is deposited on the surface of the first tin oxide layer 516 away from the silicon wafer;

[0176] The second electroplated copper electrode 522 is deposited on the surface of the second tin oxide layer 518 away from the silicon wafer.

[0177] The first electroplated copper electrode 520, the first tin oxide layer 516, the first buffer layer 512, the first doped layer 508, and the first passivation layer 504 constitute the first surface of the battery, and the second passivation layer 506, the second doped layer 510, the second buffer layer 514, the second tin oxide layer 518, and the second electroplated copper electrode 522 constitute the second surface of the battery.

[0178] Furthermore, such as Figure 6 As shown, the heterojunction solar cell also includes: a first antireflection layer, a second antireflection layer 602, a first electroplated copper electrode, and a second electroplated copper electrode.

[0179] The first antireflection layer is deposited on the surface of the first tin oxide layer 516 away from the silicon wafer;

[0180] The second antireflection layer 602 is deposited on the surface of the first antireflection layer away from the silicon wafer;

[0181] The first electroplated copper electrode 520 is deposited on the surface of the first tin oxide layer 516 away from the silicon wafer;

[0182] The second electroplated copper electrode 522 is deposited on the surface of the second tin oxide layer 518 away from the silicon wafer.

[0183] In one embodiment, the first antireflective layer includes a first silicon oxide film 604, a second silicon oxide film 606, and a third silicon oxide film 608.

[0184] The aforementioned heterojunction solar cell designs a transparent conductive layer (TCO) film. An ITO film prepared by PVD or an ICO / IWO film prepared by RPD is used as a buffer layer. This buffer layer, in contact with the doped layer, significantly reduces contact resistance. A PVD-sputtered tin oxide target is then used as a window layer. Because tin oxide films have higher transmittance in the visible light region, the transmittance of a normal-thickness buffer layer and an 80nm tin oxide layer is better than that of an ITO layer. Furthermore, the 80nm tin oxide layer has a mobility of only 22cm⁻¹. 2 / Vs, and with the use of a buffer layer and a tin oxide layer, its mobility can reach as high as 56cm. 2 / Vs, which is close to the mobility of ITO films.

[0185] The TCO film ratio for the first surface (n-layer) and the second surface (p-layer), which serves as the backlight, is optimized. Specifically, the TCO film on the n-layer side can be designed as a 20nm–30nm buffer layer and a 50nm–60nm tin oxide layer, while the TCO film on the p-layer side can be designed as a 10nm–20nm buffer layer and a 60nm–70nm tin oxide layer. Furthermore, in existing technologies, directly electroplating copper electrodes on the ITO layer side presents technological challenges. Based on this, due to the presence of the tin oxide layer, copper electrodes can be electroplated on the tin oxide layer side, thereby reducing the use of silver in the electrodes and achieving both high efficiency and cost reduction.

[0186] Furthermore, the battery incorporates a first and second buffer layer, thereby reducing the thickness of the ITO layer. After electroplating the copper grid lines, the main grid of the battery is masked using a fully automated tape machine, or by screen printing photosensitive adhesive to mask the main grid, depositing antireflective layer materials of varying thicknesses. Adjustments to the silicon oxide antireflective layer process can achieve different refractive indices from 1.5 to 1.8. Through a multi-layer antireflective process, silicon oxide is combined with vacuum-deposited magnesium fluoride material to further increase light absorption efficiency. Finally, the tape or photosensitive adhesive is removed, achieving a high-efficiency and cost-effective heterojunction solar cell. Adding an antireflective layer not only improves sunlight absorption but also facilitates encapsulation with a POE film, resulting in better encapsulation performance than direct encapsulation of ITO with a POE film.

[0187] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0188] The embodiments described above are merely illustrative of several implementation methods of this application, and while the descriptions are specific and detailed, they should not be construed as limiting the scope of this patent application. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of this application, and these all fall within the protection scope of this application. Therefore, the protection scope of this application should be determined by the appended claims.

Claims

1. A method for fabricating a heterojunction solar cell, characterized in that, The method includes: A silicon wafer is provided; the silicon wafer includes a first surface and a second surface disposed opposite to each other; A first passivation layer and a first doped layer are deposited on the first surface, and a second passivation layer and a second doped layer are deposited on the second surface; A first buffer layer is deposited on the surface of the first doped layer away from the silicon wafer using an RPD device; a second buffer layer is deposited on the surface of the second doped layer away from the silicon wafer using a magnetron sputtering deposition device, wherein the first buffer layer comprises an ICO film or an IWO film, and the second buffer layer comprises an ITO film. A first tin oxide layer was deposited on the surface of the first buffer layer away from the silicon wafer using a magnetron sputtering coating device, and a second tin oxide layer was deposited on the surface of the second buffer layer away from the silicon wafer to obtain a first battery sample; The first sample was electroplated with copper to obtain the first battery. The first doped layer is an N-type doped layer, and the second doped layer is a P-type doped layer. The thickness of the second buffer layer is less than that of the first buffer layer, with the first buffer layer having a thickness of 20-30 nm and the second buffer layer having a thickness of 10-20 nm. The thickness of the first tin oxide layer is 50-60 nm, and the thickness of the second tin oxide layer is 60-70 nm. The transmittance of the first buffer layer is better than that of the second buffer layer.

2. The method according to claim 1, characterized in that, The method further includes: Masking the main grid of the first battery; A first antireflection layer is deposited on the surface of the first tin oxide layer away from the silicon wafer; A second antireflection layer is deposited on the surface of the first antireflection layer away from the silicon wafer to obtain a second sample; The second sample is surface-treated and encapsulated to obtain a second battery.

3. The method according to claim 2, characterized in that, The first antireflective layer is composed of multiple layers of silicon oxide, and the refractive indices of the different silicon oxide layers are different.

4. The method according to claim 3, characterized in that, The first antireflective layer is composed of multiple layers of silicon oxide, and the different silicon oxide layers have different refractive indices, including: The refractive index of the first antireflection layer changes linearly from the side closer to the silicon wafer to the side farther away from the silicon wafer.

5. The method according to claim 2, characterized in that, The deposition of the first antireflection layer on the surface of the first tin oxide layer away from the silicon wafer includes: A first silicon oxide film is deposited on the surface of the first tin oxide layer away from the silicon wafer; A second silicon oxide film is deposited on the surface of the first silicon oxide film away from the silicon wafer; A third silicon oxide film is deposited on the surface of the second silicon oxide film away from the silicon wafer; The refractive indices of the first silicon oxide film, the second silicon oxide film, and the third silicon oxide film decrease sequentially.

6. The method according to claim 2, characterized in that, The masking of the main grid of the first battery includes: The main grid of the first battery can be masked by encapsulating tape, or by printing photosensitive adhesive on screen to mask the main grid.

7. The method according to claim 2, characterized in that, The surface treatment and encapsulation of the second sample includes: Remove the tape or photosensitive adhesive from the surface of the copper grid lines of the second sample.

8. A heterojunction solar cell, characterized in that, The battery includes: A silicon wafer, the silicon wafer including a first surface and a second surface disposed opposite to each other; A first passivation layer is deposited on the first surface; The first doped layer is deposited on the surface of the first passivation layer away from the silicon wafer; A second passivation layer is deposited on the second surface; The second doped layer is deposited on the surface of the second passivation layer away from the silicon wafer; A first buffer layer is deposited on the surface of the first doped layer away from the silicon wafer using an RPD device. The first buffer layer includes an ICO film or an IWO film. A second buffer layer is deposited on the surface of the second doped layer away from the silicon wafer using a magnetron sputtering device, and the second buffer layer includes an ITO film; a first tin oxide layer is deposited on the surface of the first buffer layer away from the silicon wafer using a magnetron sputtering deposition device; The second tin oxide layer is deposited on the surface of the second buffer layer away from the silicon wafer using a magnetron sputtering deposition apparatus; The first electroplated copper electrode is deposited on the surface of the first tin oxide layer away from the silicon wafer; The second electroplated copper electrode is deposited on the surface of the second tin oxide layer away from the silicon wafer; The first doped layer is an N-type doped layer, and the second doped layer is a P-type doped layer. The thickness of the second buffer layer is less than that of the first buffer layer, with the first buffer layer having a thickness of 20-30 nm and the second buffer layer having a thickness of 10-20 nm. The thickness of the first tin oxide layer is 50-60 nm, and the thickness of the second tin oxide layer is 60-70 nm. The transmittance of the first buffer layer is better than that of the second buffer layer.

9. The battery according to claim 8, characterized in that, The battery also includes: The first antireflection layer is deposited on the surface of the first tin oxide layer away from the silicon wafer; The second antireflection layer is deposited on the surface of the first antireflection layer away from the silicon wafer.

Citation Information

Patent Citations

  • Silicon-based heterojunction solar cell and preparation method thereof

    CN111653644A

  • Heterojunction solar cell and preparation method thereof

    CN114447152A