High-density and high-conductivity lithium-ion positive electrode material and preparation method thereof
By using glucose to coat large particles and graphene/carbon nanotube composites to coat small particles in the lithium iron phosphate cathode material to form a bridge structure, the problem of low density of the lithium iron phosphate cathode material is solved and significantly improved Energy density and electronic conduction properties of lithium-ion batteries.
Patent Information
- Application Number
- CN202310074002.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-16
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-01-16
AI Technical Summary
The density of the electrode sheet formed by pressing the existing lithium iron phosphate cathode material is too low, resulting in a low energy density of the lithium-ion battery.
By mixing FePO4, Li2CO3 and glucose in a water medium, grinding, spray drying and sintering, large particles are formed, and cracked into graphitized carbon in a high temperature environment to coat the surface of lithium iron phosphate particles, while using graphene/ The carbon nanotube composite coats small particles to form multiple tentacle-like bridge structures to improve electronic conduction, fills small particles between large particles, and optimizes the particle ratio to increase compaction density.
It significantly increases the compaction density of the cathode material, which is more than 20% higher than the existing technology. It also improves the electronic conductivity and increases the energy density of lithium-ion batteries.
Smart Images

Figure CN116031387B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a high-density and high-conductivity lithium ion positive electrode material and a preparation method thereof. Background Art
[0002] Lithium-ion batteries are a new generation of green high-energy batteries that have a wide range of uses in various fields. Among them, the positive electrode material of lithium-ion batteries determines the performance and price of lithium batteries. At present, the most studied and applied positive electrode materials are LiCoO 2 、LiNiO 2 、LiMn 2 O 4 、LiFePO 4 Among them, lithium iron phosphate cathode material has good stability and safety performance, and has gradually become a hot topic of research.
[0003] However, the existing lithium iron phosphate has a more obvious disadvantage, that is, the compaction density of the electrode sheet formed by pressing is too low and the conductivity deviation can only reach 2.1-2.3g / cm 3 , which directly leads to the low energy density of the battery prepared therefrom. To this end, the present invention provides a lithium ion positive electrode material and a preparation method thereof, which can effectively solve the technical problem of low energy density. Summary of the invention
[0004] The present invention is achieved in that:
[0005] A method for preparing a high-density and high-conductivity positive electrode material comprises the following steps:
[0006] S1, FePO 4 , Li 2 CO 3 and glucose, grinding in an aqueous medium, spray drying, and sintering; and finally air flow crushing to form first size particles with a particle size of 1 micron to 5 microns, wherein the glucose accounts for 4% to 7% of the total mixture mass;
[0007] S2, FePO 4 , Li 2 CO 3 and the graphene / carbon nanotube composite are uniformly mixed, ground in an aqueous medium, spray dried, and sintered; and finally air flow crushed to form second size particles with a particle size of 100 nanometers to 400 nanometers, wherein the graphene / carbon nanotube composite accounts for 0.1% to 1% of the total mixture mass;
[0008] S3, mixing the first-sized particles and the second-sized particles in a mass ratio of 2:0.8-1.2 to form the positive electrode material.
[0009] The present invention further provides a high-density and high-conductivity positive electrode material, which is obtained according to the above method.
[0010] The beneficial effects of the present invention are as follows: the high-density and high-conductivity positive electrode material and the preparation method thereof, the positive electrode sheet and the lithium-ion battery provided by the present invention are obtained by coating LiFePO with glucose. 4 Large particles are formed, and then they are cracked into graphitized carbon under high temperature and evenly coated on the surface of lithium iron phosphate particles. However, the graphene / carbon nanotube composite will coat the surface of small particles, so that multiple tentacle-like bridge structures are formed on the surface of small particles, and the bridge structure can form good electronic conduction with large particles. In addition, small particles are filled between large particles, so as to further improve the compaction density, which can be increased by more than 20% compared with the existing technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0011] Figure 1 It is a flow chart of the method for preparing the positive electrode material provided in an embodiment of the present invention. DETAILED DESCRIPTION
[0012] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention. Therefore, the following detailed description of the embodiments of the present invention provided in the drawings is not intended to limit the scope of the invention claimed for protection, but merely represents the selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0013] The content of the present invention is described in detail below with reference to embodiments.
[0014] Reference Figure 1 As shown, an embodiment of the present invention provides a method for preparing a high-density and high-conductivity positive electrode material, comprising the following steps:
[0015] S1, FePO 4 , Li 2 CO 3 and glucose, ground in an aqueous medium, spray dried, and sintered; and finally subjected to air flow crushing to form first-size particles with a particle size of 1 micron to 5 microns, wherein the glucose accounts for 4% to 7% of the mass of the total mixture.
[0016] In step S1, the grinding, spray drying, sintering and other steps are all prior art and will not be described here. Specifically, the general temperature of the spray drying is controlled between 220-250°C; the general temperature of the atmosphere sintering is controlled between 810-840°C. 4 , Li 2 CO 3 Generally, it is mixed according to the reaction ratio, which will not be repeated here. Furthermore, the final particle size can be controlled by the intensity and time of air flow crushing. Preferably, air flow crushing is performed to form first size particles with a particle size of 2 microns to 4 microns. In addition, since glucose will eventually decompose and evenly coat the surface of lithium iron phosphate, the total amount of glucose also needs to be optimized and controlled. Preferably, glucose accounts for 5% to 6% of the total mixture mass. As the amount of glucose added increases, the thickness of the subsequently decomposed carbon shell also increases.
[0017] S2, FePO 4 , Li 2 CO 3 The graphene / carbon nanotube composite is uniformly mixed, ground in an aqueous medium, spray dried, and sintered; and finally air flow crushing is performed to form second size particles with a particle size of 100 nanometers to 400 nanometers, wherein the graphene / carbon nanotube composite accounts for 0.1% to 1% of the total mixture mass.
[0018] In step S2, the grinding, spray drying, sintering and other steps are all prior art and will not be described here. Specifically, the general temperature of the spray drying is controlled between 220-250°C; the general temperature of the atmosphere sintering is controlled between 710-750°C. 4 , Li 2 CO 3 Generally, the mixture is mixed according to the reaction ratio, which will not be repeated here. Furthermore, the final particle size can be controlled by the intensity and time of air flow crushing. Preferably, air flow crushing is performed to form second size particles with a particle size of 150 nanometers to 200 nanometers. In addition, since the graphene / carbon nanotube composite is a nanoscale material, it will be evenly coated on the surface of lithium iron phosphate. Therefore, it is also necessary to optimize and control the total amount of the graphene / carbon nanotube composite. Preferably, the graphene / carbon nanotube composite is 0.5% to 0.8% of the total mixture mass. The graphene / carbon nanotube composite will be coated on the surface of the small particles, so that a plurality of tentacle-like bridging structures are formed on the surface of the small particles, and the bridging structure can form good electronic conduction with the large particles.
[0019] The method for preparing the graphene / carbon nanotube composite specifically comprises:
[0020] S21, mixing carbon nanotube powder and graphene powder and dispersing them in an acetone solvent by ultrasonic dispersion, wherein the carbon nanotube powder comprises a plurality of carbon nanotubes with both ends open;
[0021] S22, filtering the carbon nanotube powder and the graphene powder to form a mixed powder;
[0022] S23, heating the mixed powder, so that the openings of the carbon nanotubes are partially melted and composited with the graphene.
[0023] In step S21, the two ends of the carbon nanotube powder can be corroded by strong acid to open. On the one hand, after the corrosion, the two ends of the carbon nanotube are easily functionalized, which is conducive to dispersion in the solvent; on the other hand, after functionalization, it is easy to adsorb with graphene. Further, by opening the two ends of the carbon nanotube, the temperature of subsequent heating and melting can also be reduced.
[0024] The weight ratio of the carbon nanotube to graphene is 2 to 5: 1. The length of the carbon nanotube may be between 100 nanometers and 1000 nanometers. Preferably, the length of the carbon nanotube is between 500 nanometers and 800 nanometers.
[0025] In step S23, the temperature can be raised to above 1500° C. by laser ablation or other heating methods in an inert atmosphere, so that the carbon nanotube openings are partially melted and composited with graphene. In one embodiment, the temperature is raised to above 1500° C. by laser ablation or other methods, so that the carbon nanotube openings are partially melted and composited with graphene.
[0026] S3, mixing the first-sized particles and the second-sized particles in a mass ratio of 2:0.8-1.2 to form the positive electrode material.
[0027] In step S3, glucose is coated on LiFePO 4 Large particles are formed, and then they are cracked into graphitized carbon under high temperature and uniformly coated on the surface of lithium iron phosphate particles. However, the graphene / carbon nanotube composite will be coated on the surface of the small particles, so that a plurality of tentacle-like bridging structures are formed on the surface of the small particles, and the bridging structure can form good electron conduction with the large particles. In addition, the small particles are filled between the large particles, so that the compaction density can be further improved. As a further improvement, in order to increase the compaction density of the positive electrode material as much as possible, it is necessary to appropriately adjust the mixing ratio of the first size particles and the second size particles. Preferably, the first size particles and the second size particles are mixed in a mass ratio of 2:0.9 to 1.1 to form the positive electrode material. In one embodiment, the first size particles and the second size particles are mixed in a mass ratio of 2:1 to form the positive electrode material.
[0028] Embodiment 1:
[0029] FePO 4 , Li 2 CO 3 and glucose, wherein glucose is added at 5.5% by weight of the total raw material mixture, and ground in a deionized water medium; spray dried at about 230°C; sintered and kept at 820°C for about 14 hours in a nitrogen atmosphere; formed into first-size particles by air flow crushing and other methods, the mean particle size of which is about 2 microns and the standard deviation is 500nm; FePO 4 , Li 2 CO 3 and a graphene / carbon nanotube composite material uniformly mixed, wherein the graphene / carbon nanotube composite material (the weight ratio of carbon nanotube to graphene is 3:1) is added at 0.8% of the weight of the total raw material mixture, and ground in a deionized water medium; spray dried at about 210° C.; sintered and kept warm at 730° C. in a nitrogen atmosphere for about 10 hours; formed second-size particles by methods such as air flow crushing, wherein the mean particle size is about 300 nanometers and the standard deviation is 50 nm; finally, the first-size particles and the second-size particles are mixed at a mass ratio of 2:1 to form the positive electrode material.
[0030] Embodiment 2:
[0031] FePO 4 , Li 2 CO 3 and glucose, wherein glucose is added at 5.5% by weight of the total raw material mixture, and ground in a deionized water medium; spray dried at about 230°C; sintered and kept at 820°C for about 14 hours in a nitrogen atmosphere; formed into first-size particles by air flow crushing and other methods, the mean particle size of which is about 2 microns and the standard deviation is 500nm; FePO 4 , Li 2 CO 3 and a graphene / carbon nanotube composite material uniformly mixed, wherein the graphene / carbon nanotube composite material (the weight ratio of carbon nanotube to graphene is 3:1) is added at 0.8% of the weight of the total raw material mixture, and ground in a deionized water medium; spray dried at about 210°C; sintered and kept warm at 730°C in a nitrogen atmosphere for about 10 hours; formed second-size particles by methods such as air flow crushing, the mean particle size of which is about 300 nanometers and the standard deviation is 50nm; finally, the first-size particles and the second-size particles are mixed at a mass ratio of 2:0.8 to form the positive electrode material.
[0032] Embodiment 3:
[0033] FePO 4, Li 2 CO 3 and glucose, wherein glucose is added at 5.5% by weight of the total raw material mixture, and ground in a deionized water medium; spray dried at about 230°C; sintered and kept at 820°C for about 14 hours in a nitrogen atmosphere; formed into first-size particles by air flow crushing and other methods, the mean particle size of which is about 2 microns and the standard deviation is 500nm; FePO 4 , Li 2 CO 3 and a graphene / carbon nanotube composite material uniformly mixed, wherein the graphene / carbon nanotube composite material (the weight ratio of carbon nanotube to graphene is 3:1) is added at 0.8% of the weight of the total raw material mixture, and ground in a deionized water medium; spray dried at about 210°C; sintered and kept warm at 730°C in a nitrogen atmosphere for about 10 hours; formed second-size particles by methods such as air flow crushing, the mean particle size of which is about 300 nanometers and the standard deviation is 50nm; finally, the first-size particles and the second-size particles are mixed at a mass ratio of 2:1.2 to form the positive electrode material.
[0034] Comparative Example 1:
[0035] FePO 4 , Li 2 CO 3 and glucose, wherein glucose is added at 5.5% by weight of the total raw material mixture, and ground in a deionized water medium; spray dried at about 230°C; sintered and kept at 820°C for about 14 hours in a nitrogen atmosphere; formed into first-size particles by air flow crushing and other methods, the mean particle size of which is about 2 microns and the standard deviation is 500nm; FePO 4 , Li 2 CO 3 and a graphene / carbon nanotube composite material uniformly mixed, wherein the graphene / carbon nanotube composite material (the weight ratio of carbon nanotube to graphene is 3:1) is added at 0.8% of the weight of the total raw material mixture, and ground in a deionized water medium; spray dried at about 210°C; sintered and kept warm at 730°C in a nitrogen atmosphere for about 10 hours; formed second-sized particles by methods such as air flow crushing, with a mean particle size of about 300 nanometers and a standard deviation of 50 nm; finally, the first-sized particles and the second-sized particles are mixed at a mass ratio of 2:0.5 to form the positive electrode material.
[0036] Comparative Example 2:
[0037] FePO 4 , Li 2 CO 3and glucose, wherein glucose is added at 5.5% by weight of the total raw material mixture, and ground in a deionized water medium; spray dried at about 230°C; sintered and kept at 820°C for about 14 hours in a nitrogen atmosphere; formed into first-size particles by air flow crushing and other methods, the mean particle size of which is about 2 microns and the standard deviation is 500nm; FePO 4 , Li 2 CO 3 and a graphene / carbon nanotube composite material uniformly mixed, wherein the graphene / carbon nanotube composite material (the weight ratio of carbon nanotube to graphene is 3:1) is added at 0.8% of the weight of the total raw material mixture, and ground in a deionized water medium; spray dried at about 210°C; sintered and kept warm at 730°C in a nitrogen atmosphere for about 10 hours; formed second-size particles by methods such as air flow crushing, the mean particle size of which is about 300 nanometers and the standard deviation is 50nm; finally, the first-size particles and the second-size particles are mixed at a mass ratio of 2:0.3 to form the positive electrode material.
[0038] Comparative Example 3:
[0039] FePO 4 , Li 2 CO 3 and glucose, wherein glucose is added at 5.5% by weight of the total raw material mixture, and ground in a deionized water medium; spray dried at about 230°C; sintered and kept at 820°C for about 14 hours in a nitrogen atmosphere; formed into first-size particles by air flow crushing and other methods, the mean particle size of which is about 2 microns and the standard deviation is 500nm; FePO 4 , Li 2 CO 3 and a graphene / carbon nanotube composite material uniformly mixed, wherein the graphene / carbon nanotube composite material (the weight ratio of carbon nanotube to graphene is 3:1) is added at 0.8% of the weight of the total raw material mixture, and ground in a deionized water medium; spray dried at about 210°C; sintered and kept warm at 730°C in a nitrogen atmosphere for about 10 hours; formed second-size particles by methods such as air flow crushing, wherein the mean particle size is about 300 nanometers and the standard deviation is 50nm; finally, the first-size particles and the second-size particles are mixed at a mass ratio of 2:1.5 to form the positive electrode material.
[0040] Comparative Example 4:
[0041] FePO 4 , Li 2 CO 3and glucose, wherein glucose is added at 5.5% by weight of the total raw material mixture, and ground in a deionized water medium; spray dried at about 230°C; sintered and kept at 820°C for about 14 hours in a nitrogen atmosphere; formed into first-size particles by air flow crushing and other methods, the mean particle size of which is about 2 microns and the standard deviation is 500nm; FePO 4 , Li 2 CO 3 and a graphene / carbon nanotube composite material uniformly mixed, wherein the graphene / carbon nanotube composite material (the weight ratio of carbon nanotube to graphene is 3:1) is added at 0.8% of the weight of the total raw material mixture, and ground in a deionized water medium; spray dried at about 210°C; sintered and kept warm at 730°C in a nitrogen atmosphere for about 10 hours; formed second-size particles by methods such as air flow crushing, wherein the mean particle size is about 300 nanometers and the standard deviation is 50nm; finally, the first-size particles and the second-size particles are mixed at a mass ratio of 2:1.8 to form the positive electrode material.
[0042] Tablet pressing: Mix the lithium iron phosphate positive electrode active material, conductive agent and PVDF binder in a mass ratio of 8:1:1 to form a slurry; coat the slurry on aluminum foil, dry and compact it to obtain a tablet. Then cut the tablet into equal round pieces, weigh and measure the thickness, and finally calculate the compaction density of the tablet.
[0043] The positive electrode materials in Examples 1-3 and Comparative Examples 1-2 were prepared into positive electrode sheets, and the compaction density of the positive electrode sheets was tested. The test results are shown in Table 1.
[0044] Table 1 is a table of test data of Examples 1-3 and Comparative Examples 1-2
[0045] project <![CDATA[Compaction density (g / cm 3 )]]> Resistivity(Ω*cm) Example 1 2.81 9.6 Example 2 2.70 12.7 Example 3 2.75 11.4 Comparative Example 1 2.59 18.4 Comparative Example 2 2.50 20.1 Comparative Example 3 2.61 16.7 Comparative Example 4 2.53 19.5
[0046] It can be seen from the figure that different proportions of large-sized lithium iron phosphate particles and small-sized lithium iron phosphate particles have a significant effect on the compaction density, among which the compaction density can reach 2.70g / cm 3 When the ratio is about 2:1, it has the highest compaction density of 2.81g / cm 3 , significantly higher than the current 2.1-2.3g / cm 3 , the compaction density can be increased by about 20% compared with the existing materials. Further, the resistivity of the electrode sheet in Example 1 is as low as 9.6Ω*cm; while the resistivity of the comparative example 1 is as low as 18.4Ω*cm.
[0047] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a high-density and high-conductivity positive electrode material, characterized in that: The following steps are involved: S1, FePO4, Li2CO3 and glucose are mixed, ground, spray-dried and sintered in an aqueous medium; finally, air flow crushing is performed to form first-size particles with a particle size of 1 micron to 5 microns, wherein the glucose accounts for 4% to 7% of the total mixture mass; S2, FePO4, Li2CO3 and graphene / carbon nanotube composite are uniformly mixed, ground, spray-dried and sintered in an aqueous medium; finally, air flow crushing is performed to form second-size particles with a particle size of 100 nanometers to 400 nanometers, wherein the graphene / carbon nanotube composite accounts for 0.1% to 1% of the total mixture mass; S3, the first-size particles and the second-size particles are mixed in a mass ratio of 2:0.8 to 1.2 to form the positive electrode material; In step S2, the preparation method of the graphene / carbon nanotube composite comprises the following steps: S21, mixing carbon nanotube powder and graphene powder and dispersing them in an acetone solvent by ultrasonication, wherein the carbon nanotube powder comprises a plurality of carbon nanotubes with openings at both ends; S22, filtering the carbon nanotube powder and graphene powder to form a mixed powder; S23, heating the mixed powder so that the openings of the carbon nanotubes are partially melted to form a composite with the graphene; In step S21, two ends of the carbon nanotube powder are corroded by strong acid to form openings; the weight ratio of the carbon nanotube to graphene is 2-5:
1.
2. The method for preparing a high-density and high-conductivity positive electrode material according to claim 1, characterized in that: In step S3, the first-sized particles and the second-sized particles are mixed in a mass ratio of 2:0.9-1.1 to form the positive electrode material.
3. The method for preparing a high-density and high-conductivity positive electrode material according to claim 1, characterized in that: In step S1, the temperature of the spray drying is between 220-250°C; the temperature of the atmosphere sintering is controlled between 810-840°C.
4. The method for preparing a high-density and high-conductivity positive electrode material according to claim 1, characterized in that: In step S2, the temperature of the spray drying is between 220-250°C; the temperature of the atmosphere sintering is controlled between 710-750°C.
5. A high-density and high-conductivity lithium-ion positive electrode material prepared by the method according to any one of claims 1 to 4.