A diesel hydrodesulfurization catalyst and its preparation method and sulfurization method
By controlling the sulfurization temperature and gas phase conditions during the sulfurization process of the hydrodesulfurization catalyst, a highly active Co-Mo-S phase is formed, which solves the problem of Co and Ni being sulfurized before Mo and W, and improves the hydrodesulfurization performance of the catalyst. and activity.
Patent Information
- Application Number
- CN202111260937.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2041-10-28
AI Technical Summary
During the sulfurization process of existing hydrodesulfurization catalysts, Co and Ni are sulfurized before Mo and W, resulting in insufficient activity and insufficient sulfurization of the multi-layer stacked second-type active phase, which affects the hydrodesulfurization performance of the catalyst.
By introducing hydrogen sulfide at a higher temperature, heating and roasting a mixture of molybdenum trioxide, cobalt sulfate and phosphoric acid with an alumina carrier in a specific proportion to form a Co-Mo-S active phase, avoiding the low-temperature separate sulfidation of Co and Ni , and vulcanized under specific conditions to generate a highly active Co-Mo-S phase.
The generated catalyst has higher hydrodesulfurization activity, appropriate pore volume and specific surface area, and appropriate packing density. The Co-Mo-S phase ratio after sulfidation reaches 90% to 100%, which significantly improves the hydrodesulfurization performance of the catalyst.
Smart Images

Figure 776119DEST_PATH_IMAGE002 
Figure 834205DEST_PATH_IMAGE004 
Figure DEST_PATH_IMAGE001
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalyst preparation, and specifically relates to a diesel hydrodesulfurization catalyst and a preparation method and a sulfurization method thereof. Background Art
[0002] The deep hydrodesulfurization of petroleum fractions has higher and higher requirements on the activity of hydrodesulfurization catalysts. Hydrogenation catalysts usually use Group VIB and Group VIII metals as active components. Group VIB metals are generally Mo and W, and Group VIII metals are generally Co and Ni. Before the catalyst is used, the oxidized active metal needs to be converted into a sulfided active substance before it becomes active. Therefore, the sulfidation of the catalyst has an important influence on the performance of the catalyst.
[0003] Studies have shown that after sulfidation, the active phase crystals of the catalyst with the second type of active center are not in a monodisperse state, but are stacked Co-Mo-S or Ni-Mo-S species with an appropriate number of layers. This multi-layer stack of the second type of active phase is fully sulfided, and its edge position (Rim-edge) has a high adsorption hydrodesulfurization activity. At the same time, the study also found that the sulfidation temperature of Co and Ni is lower than that of Mo and W. Therefore, the goal of the sulfidation process of the catalyst with the second type of active center is to generate as many highly active multi-layer Co-Mo-S or Ni-Mo-S species as possible to avoid Co and Ni from sulfiding before Mo and W.
[0004] CN201110321357 discloses a method for sulfurizing a hydrorefining catalyst. In this method, hydrogen sulfide and a sulfurizing agent are introduced into the system at a relatively high temperature, so that the low-temperature sulfurization of Co and Ni can be avoided. Thus, at a relatively high temperature and in the presence of hydrogen sulfide, Mo and W are simultaneously sulfurized with Co and Ni to form a highly active Mo(W)-Co(Ni)-S active phase. Summary of the invention
[0005] In order to overcome the deficiencies of the prior art, the present invention provides a diesel hydrodesulfurization catalyst and a preparation method and a sulfurization method thereof. The catalyst of the present invention generates more Co-Mo-S phases after sulfurization, has higher hydrodesulfurization activity, is simple in operation process, and is easy to promote and apply.
[0006] The diesel hydrodesulfurization catalyst of the present invention comprises the following components based on the total weight of the catalyst: 17.0wt%-25.0wt% of molybdenum oxide, 6.0wt%-10.0wt% of cobalt sulfate, 2.5wt%-3.3wt% of P2O5, and 61.7wt%-74.5wt% of Al2O3.
[0007] The diesel hydrodesulfurization catalyst of the present invention has the following properties: pore volume 0.25-0.55 mL / g, specific surface area 120-250 m2 / g, bulk density 0.70~1.0g / cm 3 .
[0008] The alumina carrier is γ-Al2O3, with a pore volume of 0.50~0.90mL / g and a specific surface area of 180~350m 2 / g, bulk density 0.45~0.65g / cm 3 .
[0009] The preparation method of the diesel hydrodesulfurization catalyst of the present invention comprises the following contents:
[0010] (1) mixing and heating a certain proportion of molybdenum trioxide, cobalt sulfate, phosphoric acid and water to obtain a clear solution;
[0011] (2) Then, the clarified solution obtained in step (1) is used to saturate the alumina carrier, followed by drying and calcining to obtain a diesel hydrodesulfurization catalyst.
[0012] In the method of the present invention, the mass ratio of molybdenum trioxide, cobalt sulfate and phosphoric acid in step (1) is (18-23): (6-10): (2-6).
[0013] In the method of the present invention, the solution is prepared in step (1) and heated to a temperature of 80-95° C. and maintained at the constant temperature for 30-90 minutes.
[0014] In the method of the present invention, the drying conditions of step (1) are: drying temperature is 100° C. to 150° C., and drying time is 3 to 5 hours.
[0015] In the method of the present invention, the calcination conditions of step (1) are: the calcination temperature is 350° C. to 450° C., the calcination time is 3 to 5 hours, and the calcination is carried out in an air atmosphere.
[0016] The present invention also provides a sulfurization method for a diesel hydrodesulfurization catalyst, comprising the following contents: a diesel hydrodesulfurization catalyst is loaded into a reactor, and after the reactor is airtight, sulfurized oil is introduced into the reactor, and after the catalyst bed is wetted, sulfurization treatment is performed, and after the sulfurization is completed, the raw material oil is switched to perform normal operation; the sulfurization treatment conditions are: hydrogen partial pressure 3.0-8.0MPa, hydrogen-to-oil volume ratio 300-800, space velocity 1.5-3.0h -1 , keep the temperature at 80~120℃ for 6~10 hours, keep the temperature at 180~250℃ for 6~10 hours, keep the temperature at 280~340℃ for 6~10 hours, and keep the temperature at 350~450℃ for 6~10 hours.
[0017] The airtight process is well known in the art, and generally includes nitrogen airtightness, hydrogen replacement and hydrogen airtightness.
[0018] The sulfided oil is straight-run gasoline, straight-run kerosene, refined gasoline or refined kerosene. The sulfiding agent can be one or more of the commonly used sulfiding agents in the art, such as carbon disulfide, dimethyl disulfide, thiophene and elemental sulfur. The liquid phase sulfiding agent or elemental sulfur is added to the sulfided oil when used.
[0019] The Co-Mo-S phase ratio of the diesel hydrodesulfurization catalyst after the sulfurization method of the present invention is 90% to 100%, and the Co-Mo-S phase ratio is the molar ratio of Co-Mo-S to Mo.
[0020] The present invention first sulfides the molybdenum oxide on the catalyst to form MoS2. After the molybdenum oxide on the catalyst is completely converted into MoS2, cobalt sulfate is decomposed to form cobalt oxide species within a certain temperature range, and the cobalt oxide begins to be sulfided to form cobalt sulfide. The newly generated cobalt sulfide is distributed on the molybdenum sulfide grains to form a Co-Mo-S active phase structure. The cobalt oxide after the decomposition of cobalt sulfate is sulfided to almost form a Co-Mo-S active phase structure. The sulfided catalyst has excellent hydrodesulfurization activity. DETAILED DESCRIPTION
[0021] The present invention is further described in detail below in conjunction with the examples. In the present invention, the specific surface area and pore volume are measured by low temperature liquid nitrogen adsorption method. The Co-Mo-S phase ratio is tested by X-ray photoelectron spectroscopy (XPS). The properties of the carrier and catalyst are shown in Table 1, the properties of the sulfurized oil and the raw oil are shown in Table 2, the results of the in-situ infrared characterization of the catalyst after sulfurization are shown in Table 3, and the properties of the generated oil are shown in Table 4.
[0022] Example 1
[0023] (1) Add 140 mL of deionized water and 15 g of phosphoric acid to a 400 mL conical flask, start a magnetic stirrer, and then add 40 g of molybdenum trioxide and 28 g of cobalt sulfate heptahydrate. Heat the mixture in the conical flask at 90°C for 2 hours, then cool it naturally to 30°C, dilute the solution to 200 mL, and filter out the insoluble matter for later use;
[0024] (2) 75 mL of the solution prepared in step (1) was used to saturate 100 g of the carrier. After curing for 8 hours, the catalyst was dried at 110° C. for 4 hours and calcined at 430° C. for 3 hours to obtain a finished catalyst, numbered C-01.
[0025] (3) Catalyst sulfidation conditions: hydrogen partial pressure 6.0 MPa, hydrogen to oil volume ratio 500, space velocity 2.0 h -1, C-01 catalyst was loaded with 10mL, and after catalyst drying, nitrogen airtightness, hydrogen replacement and hydrogen airtightness, the airtightness was qualified; sulfide oil was introduced into the reactor to wet the catalyst bed, and then the temperature was increased to 110℃ at 3℃ / min, kept at a constant temperature for 8 hours, increased to 230℃ at 1℃ / min, kept at a constant temperature for 8 hours, increased to 320℃ at 1℃ / min, kept at a constant temperature for 8 hours, increased to 380℃ at 1℃ / min, and kept at a constant temperature for 8 hours.
[0026] After the vulcanization, the feedstock oil was switched. The evaluation conditions were: hydrogen partial pressure 6.0 MPa, hydrogen-to-oil volume ratio 500, and space velocity 1.5 h -1 The reaction temperature was 365°C. After stabilization for 24 hours, sampling was performed to analyze trace sulfur. The sample number was Y-01.
[0027] Example 2
[0028] Same as Example 1, except that the catalyst sulfurization conditions were: hydrogen partial pressure 6.0 MPa, hydrogen to oil volume ratio 500, space velocity 2.0 h -1 , C-01 catalyst was loaded with 10mL, and the catalyst was dried, nitrogen-tight, hydrogen-substituted, and hydrogen-tight, and the airtightness was qualified; sulfurized oil was introduced into the reactor to wet the catalyst bed. After the sulfurization was completed, the temperature was raised to 110°C at 3°C / min, and the temperature was kept constant for 8 hours, and the temperature was raised to 230°C at 1°C / min, and the temperature was kept constant for 8 hours, and the temperature was raised to 320°C at 1°C / min and the temperature was kept constant for 8 hours;
[0029] After the vulcanization, the feedstock oil was switched. The evaluation conditions were: hydrogen partial pressure 6.0 MPa, hydrogen-to-oil volume ratio 500, and space velocity 1.5 h -1 The reaction temperature was 365°C. After stabilization for 24 hours, sampling was performed to analyze trace sulfur. The sample number was Y-02.
[0030] Example 3
[0031] Same as Example 1, except that the catalyst sulfurization conditions were: hydrogen partial pressure 6.0 MPa, hydrogen to oil volume ratio 500, space velocity 2.0 h -1 , C-01 catalyst was loaded with 10mL, and the catalyst was dried, nitrogen-tight, hydrogen-substituted, and hydrogen-tight, and the airtightness was qualified; sulfurized oil was introduced into the reactor to wet the catalyst bed. After the sulfurization was completed, the temperature was raised to 110°C at 3°C / min, and the temperature was kept constant for 8 hours, and the temperature was raised to 230°C at 1°C / min, and the temperature was kept constant for 8 hours, and the temperature was raised to 420°C at 1°C / min and the temperature was kept constant for 8 hours;
[0032] After the vulcanization, the feedstock oil was switched. The evaluation conditions were: hydrogen partial pressure 6.0 MPa, hydrogen-to-oil volume ratio 500, and space velocity 1.5 h -1 The reaction temperature was 365°C. After stabilization for 24 hours, sampling was performed to analyze trace sulfur. Sample number was Y-03.
[0033] Example 4
[0034] Same as Example 1, except that the catalyst sulfurization conditions were: hydrogen partial pressure 6.0 MPa, hydrogen to oil volume ratio 500, space velocity 2.0 h -1 , C-01 catalyst was loaded with 10mL, and the catalyst was dried, nitrogen-tight, hydrogen-substituted, and hydrogen-tight, and the airtightness was qualified; sulfurized oil was introduced into the reactor to wet the catalyst bed. After the sulfurization was completed, the temperature was raised to 110°C at 3°C / min, and the temperature was kept constant for 8 hours, and the temperature was raised to 230°C at 1°C / min, and the temperature was kept constant for 8 hours, and the temperature was raised to 460°C at 1°C / min and the temperature was kept constant for 8 hours;
[0035] After the vulcanization, the feedstock oil was switched. The evaluation conditions were: hydrogen partial pressure 6.0 MPa, hydrogen-to-oil volume ratio 500, and space velocity 1.5 h -1 The reaction temperature was 365°C. After stabilization for 24 hours, sampling was performed to analyze trace sulfur. Sample number was Y-04.
[0036] Comparative Example 1
[0037] (1) Preparation of impregnation solution
[0038] Add 140 mL of deionized water and 15 g of phosphoric acid to a 400 mL conical flask, start a magnetic stirrer, and then add 40 g of molybdenum trioxide and 14.9 g of basic cobalt carbonate. Heat the mixture in the conical flask at 90°C for 2 hours, then cool it naturally to 30°C, dilute the solution to 200 mL, and filter out the insoluble matter for later use;
[0039] (2) 75 mL of the impregnation solution from step (1) was used to saturate 100 g of the carrier. After curing for 8 hours, the catalyst was dried at 110° C. for 4 hours and calcined at 430° C. for 3 hours to obtain a finished catalyst, numbered C-02.
[0040] (3) Catalyst sulfidation conditions: hydrogen partial pressure 6.0 MPa, hydrogen to oil volume ratio 500, space velocity 2.0 h -1 , C-03 catalyst was loaded with 10mL, and the catalyst was dried, nitrogen-tight, hydrogen-substituted, and hydrogen-tight, and the airtightness was qualified; sulfide oil was introduced into the reactor, and the catalyst bed was wetted, and the temperature was raised to 110°C at 3°C / min, and kept at this temperature for 8 hours, and then raised to 230°C at 1°C / min, and kept at this temperature for 8 hours, and then raised to 320°C at 1°C / min, and kept at this temperature for 8 hours, and then raised to 380°C at 1°C / min, and kept at this temperature for 8 hours;
[0041] After the vulcanization, the feedstock oil was switched. The evaluation conditions were: hydrogen partial pressure 6.0 MPa, hydrogen-to-oil volume ratio 500, and space velocity 1.5 h -1 The reaction temperature was 365°C. After stabilization for 24 hours, sampling was performed to analyze trace sulfur. Sample number was Y-05.
[0042] Table 1 Physical and chemical properties of carrier and catalyst
[0043]
[0044] Table 2 Properties of sulfurized oil and crude oil
[0045]
[0046] Table 3 In situ infrared characterization results of the sulfided catalyst at different temperatures
[0047]
[0048] Table 4 Properties of generated oil
[0049]
Claims
1. A method for sulfurizing a diesel hydrodesulfurization catalyst, Features: The catalyst, based on the total weight of the catalyst, comprises the following components: 17.0 wt% to 25.0 wt% of molybdenum oxide, 6.0 wt% to 10.0 wt% of cobalt sulfate, 2 O 5 2.5wt%~3.3wt%,Al 2 O 3 61.7wt%~74.5wt%; The sulfurization method comprises: loading a diesel hydrodesulfurization catalyst into a reactor, introducing sulfurized oil into the reactor after the reactor is airtight, and performing sulfurization after the catalyst bed is wetted. After the sulfurization is completed, a sulfurized diesel hydrodesulfurization catalyst is obtained, and the raw material oil is switched to perform normal operation. The sulfurization treatment conditions are: hydrogen partial pressure of 3.0-8.0 MPa, hydrogen-to-oil volume ratio of 300-800, and space velocity of 1.5-3.0 h -1 , the temperature is kept constant at 80~120℃ for 6~10 hours, the temperature is kept constant at 180~250℃ for 6~10 hours, the temperature is kept constant at 280~340℃ for 6~10 hours, and the temperature is kept constant at 350~450℃ for 6~10 hours; the Co-Mo-S phase ratio of the diesel hydrodesulfurization catalyst after sulfurization is 90%~100%, and the Co-Mo-S phase ratio is the molar ratio of Co-Mo-S to Mo.
2. The vulcanization method according to claim 1, Features: The catalyst has a pore volume of 0.25-0.55 mL / g and a specific surface area of 120-250 m 2 / g, bulk density 0.70~1.0g / cm 3 .
3. The vulcanization method according to claim 1, Features: Alumina carrier is γ-Al 2 O 3 , pore volume 0.50~0.90mL / g, specific surface area 180~350m 2 / g, bulk density 0.45~0.65g / cm 3 .
4. A vulcanization method according to any one of claims 1 to 3, Features: The preparation method of the catalyst comprises the following steps: (1) mixing and heating a certain proportion of molybdenum trioxide, cobalt sulfate, phosphoric acid and water to obtain a clear solution; (2) then using the clear solution obtained in step (1) to saturate an alumina carrier, drying and calcining to obtain a diesel hydrodesulfurization catalyst.
5. The vulcanization method according to claim 4, Features: In step (1), the mass ratio of molybdenum trioxide, cobalt sulfate and phosphoric acid is 18-23:6-10:2-6.
6. The vulcanization method according to claim 4, Features: Step (1) The solution is heated to 80-95°C and kept at this temperature for 30-90 minutes.
7. The vulcanization method according to claim 4, Features: The drying conditions of step (1) are: drying temperature is 100°C to 150°C, and drying time is 3 to 5 hours.
8. The vulcanization method according to claim 4, Features: The calcination conditions of step (1) are as follows: the calcination temperature is 350° C. to 450° C., the calcination time is 3 to 5 hours, and the calcination is carried out in an air atmosphere.
9. The vulcanization method according to claim 1, Features: The airtightness is achieved through nitrogen airtightness, hydrogen replacement and hydrogen airtightness processes.
10. The vulcanization method according to claim 1, Features: The sulfided oil is straight-run gasoline, straight-run kerosene, refined gasoline or refined kerosene; the sulfiding agent is one or more of carbon disulfide, dimethyl disulfide, thiophene and elemental sulfur; and the sulfiding agent is added to the sulfided oil when in use.