Polymorphic phosphorus adsorbent and preparation method thereof
By subjecting biochar to acid activation, ball milling, impregnation and hydrothermal reaction, a polymorphic phosphorus adsorbent is prepared, which solves the problems of low utilization rate of phosphorus removal agents and poor treatment of organic phosphorus in the existing technology, and achieves efficient and economical Phosphate adsorption effect.
Patent Information
- Application Number
- CN202410900025.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-15
AI Technical Summary
When existing sewage treatment plants pursue efficient phosphorus removal, the utilization rate of chemical phosphorus removal agents is low, resulting in high operating costs and increased sludge production, and the treatment effect on organic phosphorus is poor.
Using the preparation method of polymorphic phosphorus adsorbent, the biochar material is subjected to acid activation, ball milling, impregnation and hydrothermal reaction to form positively charged sites and functional groups to enhance the adsorption capacity of phosphate radicals and through organic Nitrogen quaternary ammonium salts reduce the interference effects of silicates.
It significantly improves the adsorption effect of orthophosphate, dimethoate, glyphosate and other polymorphic phosphorus, reduces the competitive effect of silicate on phosphorus removal agents, and improves phosphorus removal efficiency and economy.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of water treatment, and in particular to a polymorphic phosphorus adsorbent and a preparation method thereof. Background Art
[0002] Water pollution is one of the major environmental problems facing my country, among which phosphorus pollution has a serious impact on water ecology and human life. Phosphorus is an essential element for the growth and metabolism of organisms, but excessive phosphorus input into water bodies will lead to eutrophication of water bodies, which will lead to a series of serious ecological problems. Total phosphorus has become the main pollutant in my country's surface water environment. In order to control phosphorus pollution, some regions or river basins in my country have formulated more stringent sewage discharge standards based on their own water environment conditions and pollution prevention and control needs, raising the total phosphorus discharge standard to 0.3mg / L or 0.2mg / L. The implementation of these standards is of great significance for reducing phosphorus pollution and improving water environment quality.
[0003] The implementation of the above standards has put forward higher requirements on the phosphorus treatment capacity of sewage treatment plants. When pursuing higher standards of total phosphorus removal, sewage treatment plants tend to increase the dosage of chemical phosphorus removal agents, especially coagulants such as iron salts or aluminum salts. This method is simple to operate and easy to implement. However, its actual effect is affected by many factors. Anions such as silicate, bicarbonate and sulfate, which are commonly present in sewage, will compete with phosphate for the active binding sites of phosphorus removal agents, reducing the effective adsorption of phosphate by the agent. In addition, chemical phosphorus removal agents mainly target inorganic phosphorus and have poor treatment effects on organic phosphorus. These factors together lead to a problem: in the pursuit of deep phosphorus removal, a large amount of agents must be invested, while the effective utilization rate of the agents is relatively low. This not only increases operating costs, but also leads to a significant increase in sludge production. The treatment and disposal of large amounts of sludge not only increases the environmental burden, but also increases operating costs. Therefore, how to improve the efficiency and economy of sewage phosphorus removal has attracted more and more attention from technicians in this field. Summary of the invention
[0004] In order to solve or partially solve the problems existing in the related art, the present invention provides a polymorphic phosphorus adsorbent and a preparation method thereof.
[0005] The present invention provides a method for preparing a polymorphic phosphorus adsorbent, which comprises:
[0006] Step a), placing the biochar material in an acid solution for stirring and activation; washing and drying the activated biochar material in sequence to obtain activated biochar;
[0007] Step b), ball milling the activated biochar material to obtain powdered biochar with a diameter less than 0.1 mm;
[0008] Step c), adding the powdered biochar into a metal salt solution for impregnation treatment to obtain an impregnation treatment solution; the metal salt solution includes divalent or trivalent metal ions;
[0009] Step d), adding an organic nitrogen quaternary ammonium salt to the impregnation treatment solution for hydrothermal reaction; washing and drying the reaction product to obtain a polymorphic phosphorus adsorbent.
[0010] Furthermore, in the step a), the acid solution is a 1-4 mol / L nitric acid solution, and the mixing ratio of the biochar material to the nitric acid solution is 10 ml-50 ml: 1 g.
[0011] Furthermore, in step c), the metal ions in the metal salt solution include: Ca 2+ ,Mg 2+ , Mn 2+ and Fe 3+ One or more of the following; the concentration of metal ions in the metal salt solution is 1-2 mol / L, and the solvent is water.
[0012] Furthermore, in the step c), the metal salt solution is a mixed solution of calcium chloride, magnesium chloride and manganese chloride.
[0013] Furthermore, in the step c), the mixing ratio of the metal salt solution to the biochar is 10 ml to 30 ml: 1 g.
[0014] Furthermore, in the step c), the immersion treatment is carried out under stirring conditions, the stirring speed is 150 to 350 r / min, and the immersion time is 20 to 30 hours.
[0015] Furthermore, in the step d), the organic nitrogen quaternary ammonium salt is a short-chain organic nitrogen quaternary ammonium salt of C3 to C6; the mass ratio of the added amount of the organic nitrogen quaternary ammonium salt to the biochar material is 2 to 5:1.
[0016] Furthermore, the organic nitrogen quaternary ammonium salt is 3-chloropropyltrimethylammonium chloride, tetramethylammonium chloride or tetraethylammonium chloride.
[0017] Furthermore, in the step d), the temperature of the hydrothermal reaction is 70-80° C., and the reaction time is 4-8 hours.
[0018] The present invention also provides a polymorphic phosphorus adsorbent, characterized in that it is prepared according to any one of the methods described above.
[0019] The preparation method of the polymorphic phosphorus adsorbent provided by the present invention may have the following beneficial effects:
[0020] This method uses biochar as raw material, first performs acid activation, and forms groups such as hydroxyl and carboxyl groups while increasing its porosity and specific surface area, providing active sites for subsequent coordination with metal ions. Then, ball milling is performed to further increase its specific surface area and improve adsorption efficiency. Subsequently, a metal salt solution is added for impregnation treatment. During the impregnation process, metal ions form positively charged sites on the surface of biochar, that is, charge regulation is achieved, thereby enhancing the adsorption capacity of biochar for negatively charged phosphate ions (such as phosphate, hydrogen phosphate and dihydrogen phosphate); at the same time, metal complexes are introduced as functional groups. These complexes can form coordination bonds with phosphate ions, thereby enhancing the adsorption of phosphorus, that is, functional group loading is achieved. Finally, organic nitrogen quaternary ammonium salt is added for hydrothermal reaction. Under high temperature and high pressure, quaternary ammonium cations are formed on the surface of biochar and deposited on the surface of biochar, further playing a role in charge regulation. In addition, the quaternary ammonium salt group has an adsorption effect on silicate ion organic phosphorus in wastewater that interferes with phosphorus adsorption. When used in conjunction with chemical phosphorus removal, it reduces the competition of silicates for the active sites of iron salt and aluminum salt chemical phosphorus removal agents, thereby reducing the interference effect of phosphorus adsorption.
[0021] Experiments have shown that the polymorphic phosphorus adsorbent prepared by this method has a good adsorption effect on polymorphic phosphorus such as orthophosphate, dimethoate and glyphosate.
[0022] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the invention. DETAILED DESCRIPTION
[0023] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] The terms used in the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The singular forms "a", "the" and "the" used in the present invention and the appended claims are also intended to include plural forms unless the context clearly indicates other meanings. It should also be understood that the term "and / or" used herein refers to and includes any or all possible combinations of one or more associated listed items.
[0025] It should be understood that although the terms "first", "second", "third", etc. may be used to describe various information in the present invention, such information should not be limited to these terms. These terms are only used to distinguish the same type of information from each other. For example, without departing from the scope of the present invention, the first information may also be referred to as the second information, and similarly, the second information may also be referred to as the first information. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "multiple" is two or more, unless otherwise clearly and specifically defined.
[0026] At present, phosphorus removal in sewage treatment mainly adopts chemical precipitation method and biological phosphorus removal method. Compared with other processes, the adsorption method is simple to operate and the raw materials are easily available. In particular, the carbon-rich porous biochar produced by high-temperature pyrolysis of agricultural and forestry waste biomass under oxygen-limited conditions has the characteristics of wide sources, low cost, diverse functional groups, and rich porous structure, and has great potential for removing pollutants in water. At the same time, biochar itself can be used as a soil conditioner, and the adsorbed phosphorus is not only a pollutant, but also a nutrient. The biochar after phosphorus adsorption can be used as a fertilizer in agriculture, which can realize resource recycling. Therefore, the inventors of this application considered using biochar as a raw material to treat phosphorus adsorption in sewage.
[0027] However, the inventors of this application have found through research that although biochar has adsorption properties, its adsorption capacity for phosphate and organic phosphorus is poor, and even negative adsorption occurs. The inventors further analyzed the reasons and found that this is related to the presence of oxygen-containing functional groups in biochar that are easy to adsorb cations and the electronegativity of the surface. Directly applying it to phosphorus adsorption has the following disadvantages: the surface is electronegative, the adsorption capacity is low, and anions such as silicates compete with phosphates for adsorption sites.
[0028] Therefore, the inventors of the present application considered regulating the surface charge of biochar and loading functional groups on it to enhance its adsorption performance for phosphorus in wastewater, especially organic phosphorus.
[0029] Based on the above inventive concept, an embodiment of the present invention provides a method for preparing a polymorphic phosphorus adsorbent, which comprises the following steps:
[0030] Step a), placing the biochar material in an acid solution for stirring and activation; washing and drying the activated biochar material in sequence to obtain activated biochar;
[0031] Step b), ball milling the activated biochar material to obtain powdered biochar with a diameter less than 0.1 mm;
[0032] Step c), adding the powdered biochar into a metal salt solution for impregnation treatment to obtain an impregnation treatment solution; the metal salt solution includes divalent or trivalent metal ions;
[0033] Step d), adding an organic nitrogen quaternary ammonium salt to the impregnation treatment solution for hydrothermal reaction; washing and drying the reaction product to obtain a polymorphic phosphorus adsorbent.
[0034] The polymorphic phosphorus adsorbent provided in the present application is obtained by sequentially performing acid activation, ball milling, impregnation and hydrothermal reaction using biochar material as raw material. The biochar material can be carbon-rich porous biochar produced by high-temperature pyrolysis of wood, coal or waste biomass under oxygen-limited conditions.
[0035] The above step a) is a step of acid activation. The function of this step is: on the one hand, to remove inorganic minerals and some organic substances in the biochar material, increase its porosity and specific surface area, and thus improve the adsorption performance. On the other hand, to introduce or change the functional groups on the surface of the biochar; for example, the acid can react with the hydrocarbons in the biochar to generate hydroxyl and carboxyl groups, which can provide active sites for the subsequent coordination with metal ions. The acid solution in this step preferably uses a 1-4 mol / L nitric acid solution, and the mixing ratio of the biochar material and the nitric acid solution is preferably 10ml-50ml:1g. More preferably, the acid solution uses a 2-3 mol / L nitric acid solution, and the mixing ratio of the biochar material and the nitric acid solution is 30ml-40ml:1g. Most preferably, the acid solution uses a 2 mol / L nitric acid solution, and the mixing ratio of the biochar material and the nitric acid solution is 35ml:1g. Stirring helps to improve the activation efficiency. In this step, the stirring activation time is preferably 4-8h, and the stirring speed is preferably 150-350r / min. After stirring and activating, the activated biochar material is washed and dried in sequence to obtain activated biochar. Specifically, the activated biochar material is washed with deionized water until neutral and then placed in an oven at 105°C for drying.
[0036] The above step b) is a step of ball milling, which is used to further refine the biochar material, increase its specific surface area, and improve the adsorption efficiency. This step can be specifically: ball milling the activated biochar material, sieving it with a 200-mesh sieve, and obtaining a powdered biochar with a diameter of less than 0.1 mm.
[0037] The above step c) is a step of impregnating the powdered biochar with a metal salt solution. This is preferably carried out under stirring conditions, the stirring speed of the impregnation treatment is preferably 150 to 350 r / min, and the impregnation time is preferably 20 to 30 hours. The role of this step is that during the impregnation process, metal ions are easily adsorbed by biochar powder; metal ions will coordinate or chemically react with functional groups on the surface and inside of biochar (such as hydroxyl groups, carboxyl groups, etc.) to form metal complexes. These metal ions form positively charged sites on the surface of biochar, thereby changing the surface charge properties of biochar. This change in charge can enhance the adsorption capacity of biochar for negatively charged phosphate ions (such as phosphate, hydrogen phosphate and dihydrogen phosphate), that is, charge regulation is achieved. The reaction of metal ions with functional groups on the surface of biochar not only changes the surface charge, but also introduces metal complexes as functional groups. These complexes can form coordination bonds with phosphate ions, thereby enhancing the adsorption of phosphorus, that is, functional group loading is achieved.
[0038] Furthermore, the inventors of the present application have found through research that the metal valence of the metal salt has an important influence on the performance of the product. When divalent and / or trivalent metal salts (i.e., the metal salt solution includes divalent or trivalent metal ions) are used, the phosphorus adsorption performance of the product is relatively excellent. In this step, the metal ions of the metal salt solution preferably include: Ca 2+ ,Mg 2+ , Mn 2+ and Fe 3+ One or more of the following: the concentration of metal ions in the metal salt solution is 1-2 mol / L, and the solvent is water. Furthermore, the mixing ratio of the metal salt solution to the biochar is preferably 10ml-30ml:1g. More preferably, the concentration of metal ions in the metal salt solution is 1.5 mol / L, and the mixing ratio is 20ml:1g. As a preferred embodiment of this embodiment, the metal ions in the metal salt solution include Ca 2 + Mg 2+ and Mn 2+ The product obtained in this way has the highest phosphorus adsorption rate. The metal salt solution can specifically be a mixed solution of calcium chloride, magnesium chloride and manganese chloride.
[0039] Step d) is a step of adding an organic nitrogen quaternary ammonium salt to the impregnation treatment solution (solid-liquid mixture) obtained in step c) for hydrothermal reaction. In this step, the impregnated biochar and the quaternary ammonium salt form quaternary ammonium cations on the surface of the biochar under high temperature and high pressure, and are deposited on the surface of the biochar, further playing a role in charge regulation; in addition, the quaternary ammonium salt group has an adsorption effect on the silicate ion organic phosphorus in the wastewater that interferes with phosphorus adsorption, thereby reducing the interference effect of phosphorus adsorption.
[0040] Specifically, when the impregnated biochar undergoes a hydrothermal reaction with an organic nitrogen quaternary ammonium salt solution, the following reaction processes may occur:
[0041] 1. Interaction between metal ions and organic nitrogen quaternary ammonium salts:
[0042] Organic nitrogen quaternary ammonium salts may undergo pyrolysis under hydrothermal conditions to produce nitrogen-containing groups such as amino and pyridine. These nitrogen-containing groups may react with metal ions already present on the surface of activated carbon to form new metal-nitrogen complexes or ionic bond structures, further changing the surface chemical properties of activated biochar.
[0043] 2. Formation of metal oxides:
[0044] Under hydrothermal conditions, metal ions may undergo oxidation reactions to generate metal oxide nanoparticles, which may adhere to the surface and pore structure of activated carbon, changing the physical properties of activated carbon.
[0045] 3. Catalytic effect:
[0046] Some transition metal ions (such as Fe 3+ , Mn 2+ etc.) may show catalytic activity under hydrothermal conditions. They can promote the thermal decomposition and chemical reaction of organic nitrogen quaternary ammonium salts and accelerate the introduction of nitrogen-containing functional groups. At the same time, metal ions may also participate in the redox reaction on the surface of activated carbon and induce other chemical changes.
[0047] 4. Composite structure formation:
[0048] Metal ions and nitrogen-containing functional groups may combine through coordination bonds, ionic bonds, etc. to form new composite structures. This composite structure may change the electronic properties, pore structure and surface chemical properties of activated carbon.
[0049] In summary, when biochar impregnated with metal ions continues to undergo hydrothermal reaction with organic nitrogen quaternary ammonium salts, a series of reaction processes may occur, including the formation of metal-nitrogen species, the generation of metal oxides, catalytic effects, and the formation of composite structures. These reaction processes can further optimize the physical and chemical properties of biochar and improve its adsorption performance for phosphorus pollutants.
[0050] The above-mentioned organic nitrogen quaternary ammonium salt is preferably a short-chain organic nitrogen quaternary ammonium salt of C3 to C6; the mass ratio of the addition amount of the organic nitrogen quaternary ammonium salt to the biochar material is 2 to 5:1; more preferably 3 to 4:1, and most preferably 3.5:1. The modified biochar obtained by hydrothermal reaction with short-chain organic nitrogen quaternary ammonium salts of C3 to C6 has relatively good hydrophilicity and is easy to adsorb interfering ions such as silicate. The short-chain organic nitrogen quaternary ammonium salt can specifically be 3-chloropropyltrimethylammonium chloride, tetramethylammonium chloride or tetraethylammonium chloride. 3-chloropropyltrimethylammonium chloride is most preferably used in this embodiment. The temperature of the hydrothermal reaction is preferably 70 to 80°C, and the reaction time is preferably 4 to 8h. More preferably, the temperature of the hydrothermal reaction is 80°C and the reaction time is 6h.
[0051] After the hydrothermal reaction, the reaction product is washed and dried to obtain a polymorphic phosphorus adsorbent. Specifically, the reaction product is washed with deionized water after the hydrothermal reaction, and the operation is repeated until the last washing liquid is neutral, and then placed in an oven at 105°C for drying to obtain a powder, which is the polymorphic phosphorus adsorbent.
[0052] From the above content, it can be seen that the preparation method of the multi-morphological phosphorus adsorbent provided by the embodiment of the present invention has the following advantages:
[0053] This method uses biochar as raw material, first performs acid activation, and forms groups such as hydroxyl and carboxyl groups while increasing its porosity and specific surface area, providing active sites for subsequent coordination with metal ions. Then, ball milling is performed to further increase its specific surface area and improve adsorption efficiency. Subsequently, a metal salt solution is added for impregnation treatment. During the impregnation process, metal ions form positively charged sites on the surface of biochar, that is, charge regulation is achieved, thereby enhancing the adsorption capacity of biochar for negatively charged phosphate ions (such as phosphate, hydrogen phosphate and dihydrogen phosphate); at the same time, metal complexes are introduced as functional groups. These complexes can form coordination bonds with phosphate ions, thereby enhancing the adsorption of phosphorus, that is, functional group loading is achieved. Finally, organic nitrogen quaternary ammonium salt is added for hydrothermal reaction. Under high temperature and high pressure, quaternary ammonium cations are formed on the surface of biochar and deposited on the surface of biochar, further playing a role in charge regulation. In addition, the quaternary ammonium salt group has an adsorption effect on silicate ion organic phosphorus in wastewater that interferes with phosphorus adsorption. When used in conjunction with chemical phosphorus removal, it reduces the competition of silicates for the active sites of iron salt and aluminum salt chemical phosphorus removal agents, thereby reducing the interference effect of phosphorus adsorption.
[0054] Experiments have shown that the polymorphic phosphorus adsorbent prepared by this method has a good adsorption effect on polymorphic phosphorus such as orthophosphate, dimethoate and glyphosate.
[0055] Another embodiment of the present invention further provides a polymorphic phosphorus adsorbent, which is prepared according to the method of the above embodiment. The specific implementation process and beneficial effects are the same as those of the above embodiment, and will not be described in detail in this embodiment.
[0056] The technical solution of the present invention is further described below in conjunction with specific embodiments:
[0057] Example 1
[0058] (1) Take 1g of wood biochar and place it in 50ml of 2.5mol / L nitric acid solution. Stir it at 150r / min for 4h, then wash it with deionized water until it is neutral, and then place it in a 105℃ oven to dry for later use;
[0059] (2) ball-milling the material obtained in step (1) and sieving it with a 200-mesh sieve to obtain powdered biochar;
[0060] (3) The powdered biochar obtained in step (2) is placed in 30 ml of a metal salt solution and stirred at 350 r / min for 24 hours. The metal salt solution is a mixed solution of calcium chloride, magnesium chloride and manganese chloride, and the concentrations of calcium chloride, magnesium chloride and manganese chloride are all 2 mol / L; then 5 g of 3-chloropropyltrimethylammonium chloride is slowly added to the solution and mixed evenly, and then poured into a hydrothermal reactor, and placed in an oven at 80°C for 6 hours to complete the hydrothermal reaction. After the reaction is completed, the reaction product is filtered and washed with deionized water, and the operation is repeated until the last washing liquid is neutral, and then placed in an oven at 105°C for drying. The obtained powder is a polymorphic phosphorus adsorbent.
[0061] Example 2
[0062] (1) Take 1g of coal-based biochar and place it in 10ml of 3.5mol / L nitric acid solution. Stir it at 150r / min for 8h, then wash it with deionized water until it is neutral, and then place it in a 105℃ oven to dry for later use;
[0063] (2) ball-milling the material obtained in step (1) and sieving it with a 200-mesh sieve to obtain powdered biochar;
[0064] (3) The powdered biochar obtained in step (2) is placed in 10 ml of a metal salt solution and stirred at 250 r / min for 24 hours. The metal salt solution is a mixed solution of calcium chloride, magnesium chloride and manganese chloride, and the concentrations of calcium chloride, magnesium chloride and manganese chloride are all 1 mol / L; then 2 g of 3-chloropropyltrimethylammonium chloride is slowly added to the solution and mixed evenly, and then poured into a hydrothermal reactor, and placed in an oven at 80°C for 6 hours to complete the hydrothermal reaction. After the reaction is completed, the reaction product is filtered and washed with deionized water, and the operation is repeated until the last washing liquid is neutral, and then placed in an oven at 105°C for drying. The obtained powder is a polymorphic phosphorus adsorbent.
[0065] Example 3
[0066] (1) Take 1g of biochar made from dewatered sludge from a sewage plant and place it in 35ml of 2mol / L nitric acid solution. Stir it at 150r / min for 4h, then wash it with deionized water until it is neutral and place it in a 105℃ oven to dry for later use;
[0067] (2) ball-milling the material obtained in step (1) and sieving it with a 200-mesh sieve to obtain powdered biochar;
[0068] (3) The powdered biochar obtained in step (2) is placed in 20 ml of a metal salt solution and stirred at 150 r / min for 24 hours. The metal salt solution is a mixed solution of calcium chloride, magnesium chloride and manganese chloride, and the concentrations of calcium chloride, magnesium chloride and manganese chloride are all 1.5 mol / L; then 3.5 g of 3-chloropropyltrimethylammonium chloride is slowly added to the solution, mixed evenly, and poured into a hydrothermal reactor, and placed in an oven at 80°C for 6 hours to complete the hydrothermal reaction. After the reaction is completed, the reaction product is filtered and washed with deionized water, and the operation is repeated until the last washing liquid is neutral, and then placed in an oven at 105°C for drying. The obtained powder is a polymorphic phosphorus adsorbent.
[0069] Example 4
[0070] The only difference between this embodiment and embodiment 2 is that the metal salt solution in step 3 is 1 mol / L calcium chloride; the rest is the same as embodiment 2.
[0071] Example 5
[0072] The only difference between this embodiment and embodiment 2 is that the metal salt solution in step 3 is 1 mol / L magnesium chloride; the rest is the same as embodiment 2.
[0073] Example 6
[0074] The difference between this embodiment and embodiment 2 is that the metal salt solution in step 3 is 1 mol / L ferric chloride; the rest is the same as embodiment 2.
[0075] Example 7
[0076] The only difference between this embodiment and embodiment 2 is that the metal salt solution in step 3 is 1 mol / L manganese chloride; the rest is the same as embodiment 2.
[0077] Example 8
[0078] The only difference between this embodiment and embodiment 2 is that the metal salt solution in step 3 is a mixed solution of ferric chloride, magnesium chloride and manganese chloride, and the concentrations of ferric chloride, magnesium chloride and manganese chloride are all 1 mol / L; the rest is the same as embodiment 2.
[0079] The phosphorus removal effect of the polymorphic phosphorus adsorbents prepared in Examples 1 to 8 was tested, and the test method was as follows:
[0080] Take a wastewater sample containing multiple forms of phosphorus pollution, the wastewater sample contains 1 mg / L of orthophosphate, 1 mg / L of dimethoate, 1 mg / L of glyphosate, and 30 mg / L of silicate, adjust the pH of the wastewater to 6.5-9.0, then add 5 g / L of the phosphorus removal adsorbent prepared in Comparative Example 1, stir the reaction for 30 minutes, let it stand and filter to measure the residual concentration of various phosphorus pollutants in the supernatant, the phosphorus removal effect is shown in Table 1:
[0081] Table 1 Test results of phosphorus removal effect of multi-form phosphorus adsorbent
[0082] Example Orthophosphate Dimethoate Glyphosate Silicate Example 1 0.30mg / L 0.15mg / L 0.25mg / L 21.60mg / L Example 2 0.35mg / L 0.17mg / L 0.28mg / L 22.16mg / L Example 3 0.25mg / L 0.12mg / L 0.22mg / L 20.25mg / L Example 4 0.55mg / L 0.67mg / L 0.70mg / L 21.37mg / L Example 5 0.50mg / L 0.55mg / L 0.65mg / L 21.52mg / L Example 6 0.55mg / L 0.45mg / L 0.47mg / L 21.35mg / L Example 7 0.85mg / L 0.80mg / L 0.90mg / L 22.80mg / L Example 8 0.60mg / L 0.67mg / L 0.65mg / L 23.50mg / L
[0083] As can be seen from Table 1, the polymorphic phosphorus adsorbent provided in the embodiments of the present application has a good adsorption effect on polymorphic phosphorus such as orthophosphate, dimethoate, and glyphosate in wastewater. Among them, when the metal salt solution is a mixed solution of calcium chloride, magnesium chloride, and manganese chloride, the polymorphic phosphorus adsorbent obtained has the most outstanding adsorption effect on phosphorus.
[0084] The embodiments of the present invention have been described above, and the above description is exemplary, not exhaustive, and is not limited to the disclosed embodiments. Many modifications and changes will be apparent to those of ordinary skill in the art without departing from the scope and spirit of the described embodiments. The selection of terms used herein is intended to best explain the principles of the embodiments, practical applications, or improvements to the technology in the market, or to enable other persons of ordinary skill in the art to understand the embodiments disclosed herein.
Claims
1. A method for preparing a polymorphic phosphorus adsorbent, characterized in that: include: Step a), placing the biochar material in an acid solution for stirring and activation; The activated biochar material is sequentially washed and dried to obtain activated biochar; Step b), ball milling the activated biochar material to obtain powdered biochar with a diameter less than 0.1 mm; Step c), adding the powdered biochar into a metal salt solution for impregnation treatment to obtain an impregnation treatment solution; the metal salt solution includes divalent or trivalent metal ions; Step d), adding an organic nitrogen quaternary ammonium salt to the impregnation treatment solution for hydrothermal reaction; washing and drying the reaction product to obtain a polymorphic phosphorus adsorbent.
2. The preparation method according to claim 1, characterized in that: In the step a), the acid solution is a 1-4 mol / L nitric acid solution, and the mixing ratio of the biochar material to the nitric acid solution is 10 ml-50 ml: 1 g.
3. The preparation method according to claim 1, characterized in that: In step c), the metal ions of the metal salt solution include: Ca 2+ ,Mg 2+ , Mn 2+ and Fe 3+ One or more of the following; the concentration of metal ions in the metal salt solution is 1-2 mol / L, and the solvent is water.
4. The preparation method according to claim 1, characterized in that: In the step c), the metal salt solution is a mixed solution of calcium chloride, magnesium chloride and manganese chloride.
5. The preparation method according to claim 3, characterized in that: In the step c), the mixing ratio of the metal salt solution to the biochar is 10 ml to 30 ml: 1 g.
6. The preparation method according to claim 1, characterized in that: In the step c), the immersion treatment is carried out under stirring conditions, the stirring speed is 150 to 350 r / min, and the immersion time is 20 to 30 hours.
7. The preparation method according to claim 1, characterized in that: In the step d), the organic nitrogen quaternary ammonium salt is a short-chain organic nitrogen quaternary ammonium salt of C3 to C6; the mass ratio of the added amount of the organic nitrogen quaternary ammonium salt to the biochar material is 2 to 5:
1.
8. The preparation method according to claim 1, characterized in that: The organic nitrogen quaternary ammonium salt is 3-chloropropyltrimethylammonium chloride, tetramethylammonium chloride or tetraethylammonium chloride.
9. The preparation method according to claim 1, characterized in that: In the step d), the temperature of the hydrothermal reaction is 70-80° C., and the reaction time is 4-8 hours.
10. A polymorphic phosphorus adsorbent, characterized in that: It is prepared according to the method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Method for preparaing dephosphorized and ferrum-carried activated carbon adsorbent
CN102614854A
Strong alkaline type anion activated carbon adsorbent as well as preparation method and application thereof
CN103877935A
Preparation method for modified biological carbon which efficiently adsorbs soil inorganic phosphorus and dissolves organic phosphorus at same time and application
CN107459025A
Preparation method of biochar modified material for removing phosphorus in eutrophic water body
CN109534432A
Water pollutant adsorbing material and preparation method thereof
CN110605095A
Cited By
Quaternary ammonium salt / magnetic biochar composite material, preparation method and application
CN119306301A
Environment-friendly treatment process for glyphosate production mother liquor
CN119841496A
An environmentally friendly treatment process for glyphosate production mother liquor
CN119841496B