Adsorption heat exchanger

By using nitric acid-resistant adhesives and crosslinking agents to meet the loading requirements under specific conditions, the problem of adsorption layer degradation in adsorption heat exchangers was solved, and the stability and performance of the adsorption layer were maintained for a long time.

CN116056779BActive Publication Date: 2026-11-10DAIKIN INDUSTRIES LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202180053621.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-30
Filing Date
2021-09-30
Publication Date
2026-11-10
Estimated Expiration
2041-09-30

AI Technical Summary

Technical Problem

In adsorption heat exchangers, the adsorption layer is prone to deterioration in a short period of time, leading to a decline in performance.

Method used

By selecting adhesives and crosslinking agents with nitric acid resistance, the adsorbent is ensured to remain stable under high temperature and humidity conditions, meeting the loading requirements under specific conditions. Fluoropolymers, acrylic resins, or epoxy resins are used as adhesives, combined with crosslinking agents such as carbodiimide-based or isocyanate-based hydrocarbons to inhibit adsorbent shedding.

Benefits of technology

It effectively inhibits the deterioration of the adsorption layer, maintains the performance stability of the adsorption heat exchanger, and extends its service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116056779B_ABST
    Figure CN116056779B_ABST
Patent Text Reader

Abstract

An adsorption heat exchanger (20) includes a substrate sheet (26) and an adsorbent (41) supported on the substrate sheet (26) by an adhesive (42). The adsorption heat exchanger satisfies at least one of a first condition and a second condition. The first condition is that after immersing the substrate sheet (26) with the adsorbent (41) in a 10% nitric acid aqueous solution at an ambient temperature of 70°C for 40 hours, the loading of the adhesive (42) and the adsorbent (41) is 32% to 100% of that before immersion. The second condition is that after 5000 cycles of alternating exposure to a dry state at an ambient temperature of 70°C and a humidity of 20% and to a humid state with water sprayed onto the adsorption heat exchanger (26), the loading of the adhesive (42) and the adsorbent (41) is 90% to 100% of that before exposure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This disclosure relates to an adsorption heat exchanger. Background Technology

[0002] Adsorption heat exchangers with an adsorption layer formed on their surface are known to date. For example, as described in Patent Document 1, such an adsorption heat exchanger is installed in a humidity control device for regulating air humidity. Specifically, in this humidity control device, an adsorption heat exchanger is installed in the refrigerant circuit of a refrigeration cycle. In the adsorption heat exchanger functioning as an evaporator, moisture contained in the air passing through the adsorption heat exchanger is adsorbed by the adsorption layer. In the adsorption heat exchanger functioning as a condenser, moisture released from the adsorption layer is introduced into the air passing through the adsorption heat exchanger.

[0003] An adsorption heat exchanger includes a substrate sheet and an adsorbent supported on the substrate sheet by an adhesive. For example, a urethane resin is used as the adhesive.

[0004] Existing technical documents

[0005] Patent documents

[0006] Patent Document 1: Japanese Patent Publication No. 2009-019863 Summary of the Invention

[0007] -The technical problem the invention aims to solve-

[0008] In adsorption heat exchangers, there are instances where adsorption performance decreases, particularly when the adsorption layer deteriorates in a short period of time, leading to a decline in performance.

[0009] The purpose of this disclosure is to suppress the degradation of the adsorption layer in an adsorption heat exchanger.

[0010] - Technical solutions for solving technical problems -

[0011] The first aspect of this disclosure pertains to an adsorption heat exchanger 20, which includes a substrate sheet 26 and an adsorbent 41 supported on the substrate sheet 26 by an adhesive 42. The adsorption heat exchanger satisfies at least one of a first condition and a second condition. The first condition is that after immersing the substrate sheet 26 with the adsorbent 41 in a 10% nitric acid aqueous solution at an ambient temperature of 70°C for 40 hours, the loading of the adhesive 42 and the adsorbent 41 is 32% to 100% of that before immersion. The second condition is that after 5000 cycles of alternating exposure to a dry state at an ambient temperature of 70°C and a humidity of 20%, and to a humid state with water sprayed onto the adsorption heat exchanger 20, the loading of the adhesive 42 and the adsorbent 41 is 90% to 100% of that before exposure.

[0012] In the first aspect, by configuring the adsorption heat exchanger 20 to satisfy at least one of the first and second conditions, its degradation over time can be suppressed within a desired range when the adsorption heat exchanger 20 is actually used.

[0013] The second aspect of this disclosure is that, based on the adsorption heat exchanger of the first aspect, the first condition is satisfied.

[0014] In the second aspect, by satisfying the first condition, the degradation of the adsorption heat exchanger 20 over time can be suppressed within the desired range when it is actually used.

[0015] The third aspect of this disclosure is that, based on the adsorption heat exchanger of the first aspect, the second condition is satisfied.

[0016] In the third aspect, by satisfying the second condition, the degradation of the adsorption heat exchanger 20 over time can be suppressed within the desired range when it is actually used.

[0017] The fourth aspect of this disclosure is that, based on the adsorption heat exchanger of the first aspect, both the first and second conditions are satisfied.

[0018] In the fourth aspect, by satisfying both the first and second conditions, the degradation of the adsorption heat exchanger 20 over time can be more reliably suppressed within the desired range when it is actually used.

[0019] The fifth aspect of this disclosure is that, based on the adsorption heat exchanger of any one of the first to fourth aspects, the combined thickness of the adhesive 42 and the adsorbent 41 is in the range of 20 μm or more and 100 μm or less.

[0020] The sixth aspect of this disclosure is that, based on the adsorption heat exchanger of any one of the first to fifth aspects, the adhesive contains at least one of fluororesin, acrylic resin, epoxy resin and urethane resin, and the crosslinking agent is a hydrocarbon having at least one of carbodiimide group, isocyanate group and ester group.

[0021] In the sixth aspect, the aforementioned materials are used as their respective specific materials, thereby enabling the realization of an adsorption heat exchanger. Attached Figure Description

[0022] Figure 1 This is a piping system diagram showing the structure of the refrigerant circuit of the humidity control device. Figure 1 (A) shows the action in the first action. Figure 1 (B) shows the action in the second action.

[0023] Figure 2This is a simplified 3D diagram of an adsorption heat exchanger.

[0024] Figure 3 This is a side view of the heat exchanger unit that makes up the adsorption heat exchanger.

[0025] Figure 4 It is shown Figure 3 A sectional view of section AA in the image.

[0026] Figure 5 This is a schematic diagram showing the adhesive and absorbent disposed on the substrate sheet.

[0027] Figure 6 It is shown in Figure 5 An example of a coating applied to a substrate sheet.

[0028] Figure 7 This is a diagram illustrating the test method for the water permeability of the adhesive.

[0029] Figure 8 This is a graph showing the relationship between the water permeability of each adhesive and the performance of the adsorption heat exchanger.

[0030] Figure 9 This is a diagram showing test pieces used to test the tensile strength, etc., of adhesives.

[0031] Figure 10 This is a graph showing the relationship between the elongation of the resin used in the adhesive and the applied tensile force. Detailed Implementation

[0032] The embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0033] <Structure of Humidity Control Device>

[0034] First, the humidity control device equipped with the adsorption heat exchanger 20 of this embodiment will be described. This humidity control device is configured to perform dehumidification operation and humidification operation, supplying dehumidified air to the room during the dehumidification operation and supplying humidified air to the room during the humidification operation.

[0035] like Figure 1 As shown, the humidity control device includes a refrigerant circuit 10. This refrigerant circuit 10 is a closed loop comprising a first adsorption component 11, a second adsorption component 12, a compressor 13, a four-way reversing valve 14, and an electric expansion valve 15, and is filled with refrigerant. A vapor compression refrigeration cycle is performed in the refrigerant circuit 10 by circulating the filled refrigerant. Furthermore, both the first adsorption component 11 and the second adsorption component 12 are constructed using an adsorption heat exchanger 20 according to the present invention. Details regarding the adsorption heat exchanger 20 will be described later.

[0036] In the refrigerant circuit 10 described above, the discharge side of the compressor 13 is connected to the first port of the four-way reversing valve 14, and the suction side of the compressor 13 is connected to the second port of the four-way reversing valve 14. One end of the first adsorption component 11 is connected to the third port of the four-way reversing valve 14. The other end of the first adsorption component 11 is connected to one end of the second adsorption component 12 via the electric expansion valve 15. The other end of the second adsorption component 12 is connected to the fourth port of the four-way reversing valve 14.

[0037] The aforementioned four-way directional valve 14 can be in the first state ( Figure 1 (A) shows the state) and the second state ( Figure 1 The system switches between states shown in (B), where in the first state, the first valve port is connected to the third valve port and the second valve port is connected to the fourth valve port, and in the second state, the first valve port is connected to the fourth valve port and the second valve port is connected to the third valve port.

[0038] <Structure of an Adsorption Heat Exchanger>

[0039] As described above, the first adsorption component 11 and the second adsorption component 12 are each composed of an adsorption heat exchanger 20. (Refer to...) Figure 2 , Figure 3 , Figure 4 The adsorption heat exchanger 20 will be described.

[0040] The adsorption heat exchanger 20 includes two sub-units 21 and 22 (see reference). Figure 2 Each subunit 21, 22 includes a heat exchanger body 25 and an adsorption layer 30. The heat exchanger body 25 is a so-called transverse finned tube heat exchanger, and the adsorption layer 30 is formed to cover the surface of the heat exchanger body 25 (see reference). Figure 4 In the adsorption heat exchanger 20, two sub-units 21 and 22 are arranged overlapping each other. The sub-unit located upstream of the airflow through the adsorption heat exchanger 20 constitutes the first sub-unit 21, and the sub-unit located downstream of the airflow through the adsorption heat exchanger 20 constitutes the second sub-unit 22.

[0041] The heat exchanger body 25 includes a cylindrical heat transfer tube 27 as a heat transfer tube component and a plurality of fins 26. Each fin 26 is a rectangular plate-shaped component, for example, made of aluminum. The fins 26 are arranged vertically in an opposing posture and are spaced apart from each other in a row. The straight tube portion 28 and the U-shaped tube portion 29 of the heat transfer tube 27 are alternately formed, so that the heat transfer tube 27 is formed in a left-right serpentine shape. The heat transfer tube 27 is configured such that its straight tube portion 28 passes through each of the arranged fins 26. The straight tube portion 28 of the heat transfer tube 27 is engaged with the fins 26, and the outer peripheral surface of the straight tube portion 28 is tightly engaged with the fins 26.

[0042] -Operational Actions-

[0043] The aforementioned humidification device is capable of both dehumidification and humidification operations. During both dehumidification and humidification operations, the humidification device alternately and repeatedly performs the first and second actions at predetermined time intervals (e.g., 3-minute intervals).

[0044] When operating in dehumidification mode, the aforementioned humidification device draws in outdoor air OA as the first air and indoor air RA as the second air. Conversely, when operating in humidification mode, the aforementioned humidification device draws in indoor air RA as the first air and outdoor air OA as the second air.

[0045] <First Action>

[0046] First, the first operation will be explained. In the first operation, second air is introduced into the first adsorption unit 11, and second air is introduced into the second adsorption unit 12. In the refrigerant circuit 10 during the first operation, the four-way reversing valve 14 is set to the first state. If the compressor 13 is operated, the refrigerant circulates in the refrigerant circuit 10, thereby performing a refrigeration cycle. At this time, in the refrigerant circuit 10, the first adsorption unit 11 functions as a condenser, and the second adsorption unit 12 functions as an evaporator.

[0047] Specifically, the refrigerant ejected from the compressor 13 condenses and releases heat in the first adsorption element 11. The condensed refrigerant in the first adsorption element 11 is depressurized as it passes through the electric expansion valve 15, and then absorbs heat and evaporates in the second adsorption element 12. The evaporated refrigerant in the second adsorption element 12 is drawn into the compressor 13 and compressed, and then ejected from the compressor 13 again.

[0048] In the first adsorption component 11, which is composed of an adsorption heat exchanger 20, the adsorption layer 30 on the surface of the fins 26 is heated by the refrigerant in the heat transfer tube 27 and dehumidifies. The water vapor released from the adsorption layer 30 is then introduced into the second air. Similarly, in the second adsorption component 12, which is also composed of an adsorption heat exchanger 20, the adsorption layer 30 on the surface of the fins 26 absorbs moisture from the first air, and the heat generated is absorbed by the refrigerant in the heat transfer tube 27.

[0049] In addition, during dehumidification operation, the first air dehumidified by the second adsorption component 12 is supplied to the room, and the water vapor released from the first adsorption component 11 is discharged to the outside along with the second air. On the other hand, during humidification operation, the second air humidified by the first adsorption component 11 is supplied to the room, and the first air, whose water vapor has been removed by the second adsorption component 12, is discharged to the outside.

[0050] <Second Action>

[0051] Next, the second operation will be described. In the second operation, first air is supplied to the first adsorption unit 11, and second air is supplied to the second adsorption unit 12. In the refrigerant circuit 10 during the second operation, the four-way reversing valve 14 is set to the second state. If the compressor 13 is operated, the refrigerant circulates in the refrigerant circuit 10, thereby performing a refrigeration cycle. At this time, in the refrigerant circuit 10, the second adsorption unit 12 operates as a condenser, and the first adsorption unit 11 operates as an evaporator.

[0052] Specifically, the refrigerant ejected from the compressor 13 condenses and releases heat in the second adsorption unit 12. The refrigerant condensed in the second adsorption unit 12 is depressurized as it passes through the electric expansion valve 15, and then absorbs heat and evaporates in the first adsorption unit 11. The refrigerant evaporated in the first adsorption unit 11 is drawn into the compressor 13 and compressed, and then ejected from the compressor 13 again.

[0053] In the second adsorption component 12, which is composed of an adsorption heat exchanger 20, the adsorption layer 30 on the surface of the fins 26 is heated and dehumidified by the refrigerant in the heat transfer tube 27, and the water vapor released from the adsorption layer 30 is introduced into the second air. Similarly, in the first adsorption component 11, which is composed of an adsorption heat exchanger 20, the adsorption layer 30 on the surface of the fins 26 absorbs moisture from the first air, and the heat generated is absorbed by the refrigerant in the heat transfer tube 27.

[0054] In addition, during dehumidification operation, the first air dehumidified by the first adsorption component 11 is supplied to the room, and the water vapor released from the second adsorption component 12 is discharged to the outside along with the second air. On the other hand, during humidification operation, the second air humidified by the second adsorption component 12 is supplied to the room, and the first air whose water vapor has been removed by the first adsorption component 11 is discharged to the outside.

[0055] <About the Adsorption Layer>

[0056] like Figure 4 As shown, the adsorption layer 30 is formed to cover both sides of the fin 26. The thickness of this adsorption layer 30 is, for example, approximately 0.25 mm. It should be noted that the adsorption layer 30 is formed not only on the surface of the fin 26, but also on the surface of the portion of the heat transfer tube 27 not covered by the fin 26 (such as the U-shaped tube portion 29). The thickness of the adsorption layer 30 formed on the portion other than the fin 26 may also be different from the thickness of the adsorption layer 30 on the surface of the fin 26.

[0057] The adsorption layer 30 contains an adsorbent, which is, for example, formed from a hygroscopic organic polymer material. In this adsorbent, multiple polymer backbones having hydrophilic polar groups (hydrophilic groups) in their molecules are cross-linked, and the cross-linked polymer backbones form a three-dimensional structure. Alternatively, silica and metal-organic frameworks (MOFs) can also be used as adsorbents.

[0058] Figure 5 This is a schematic cross-sectional view showing the fin 26 and its surface adsorption layer 30 under magnification. The fin 26 is formed, for example, using an aluminum substrate sheet. The adsorption layer 30 includes an adsorbent 41 and an adhesive 42 for supporting the adsorbent. It should be noted that, as... Figure 6 As shown, the fins 26 can also be formed using a substrate sheet including a coating 43, which is formed of resin. Epoxy resin can be listed as an example of the resin used for the coating 43. The combined thickness of the adhesive 42 and the adsorbent 41 is preferably 20 μm or more and 120 μm or less.

[0059] Here, with the use of the adsorption heat exchanger 20, the adsorption layer 30 deteriorates, resulting in occasional detachment of the adsorbent 41 from the fins 26. If the adsorbent 41 detaches, the performance of the adsorption heat exchanger 20 decreases. The inventors of this application have identified that one cause of this deterioration of the adsorption layer 30 is NOx (nitrogen oxides) and SOx (sulfur oxides) in the atmosphere. Based on this understanding, using an adhesive 42 that is resistant to nitric acid and sulfuric acid, particularly nitric acid, is an effective means to suppress the deterioration of the adsorption layer 30.

[0060] In other words, in the adsorption heat exchanger 20, which includes a substrate sheet (fin 26) and an adsorbent 41 supported on the substrate sheet by an adhesive 42, the adhesive 42 is preferably resistant to nitric acid.

[0061] As a more specific evaluation method, the percentage of mass reduction of the adhesive 42 after being impregnated in 10% nitric acid at 70°C for 40 hours is preferably 35% or less, more preferably 20% or less, and even more preferably 10% or less. Using such an adhesive can more effectively suppress the detachment of the adsorbent 41 during the use of the adsorption heat exchanger 20.

[0062] Furthermore, in order for the adsorption heat exchanger 20 to function, the adhesive 42 preferably has a certain degree of water permeability. Specifically, when a membrane with a thickness of 100 μm is formed using the adhesive 42 as the material, the daily water permeability of the membrane is preferably 85 g / m³. 2 The above, more preferably 120g / m 2 above.

[0063] In addition, if the adsorbent 41 absorbs moisture and swells (increases in volume), the adsorbent 41 can be prevented from falling off if a high elongation adhesive 42 is used accordingly.

[0064] The swelling rate, expressed as X%, is the ratio of the volume of the adsorbent 41 when swollen (in a state of maximal moisture absorption) to the volume of the adsorbent 41 when dry. Furthermore, the elongation rate of the adhesive 42 is the ratio of the length at which the sample breaks due to stretching both ends of the strip sample to its initial length, expressed as a percentage (%). Preferably, the elongation rate of the adhesive 42 is at least 100% (X / 100) × 100%. Using an adhesive 42 with such an elongation rate reduces the likelihood of breakage even when the adsorbent 41 swells, and is therefore preferred.

[0065] In addition, the tensile strength of adhesive 42 is preferably 12 N / mm. 2 Below, 8 N / mm is preferred. 2 The following is a further preferred value: 6N / mm 2 The following applies. If such an adhesive 42 is used, the adhesive 42 easily stretches as the adsorbent 41 swells, thus inhibiting the adsorbent 41 from falling off.

[0066] In addition, in the adsorption heat exchanger 20, which includes a substrate sheet (fin 26) and an adsorbent 41 supported on the substrate sheet by an adhesive 42, it is preferable to satisfy a first condition, which is that after the substrate sheet 26 with adsorbent 41 is immersed in a 10% nitric acid aqueous solution for 40 hours at an ambient temperature of 70°C, the loading of adhesive 42 and adsorbent 41 is 32 to 100% of that before immersion.

[0067] If the adsorption layer 30 (adsorbent 41 and binder 42) detaches from the fins 26, the performance of the adsorption heat exchanger 20 will decrease. However, if a sufficient amount of adsorption layer 30 is maintained even after detachment, the desired performance can be maintained. Specifically, even if the adsorption layer 30 detaches due to nitric acid impregnation, the adsorption heat exchanger 20 can maintain the desired performance as long as the loading after impregnation is 50-100% of the loading before impregnation. It should be noted that the loading of the adsorption layer 30 is expressed in terms of mass. That is, the mass of the adsorption layer 30 can be determined based on the mass of the heat exchanger body 25 and the mass of the adsorption heat exchanger 20 before and after nitric acid impregnation.

[0068] Furthermore, the adsorption layer 30 may deteriorate due to repeated use of the adsorption heat exchanger 20. Therefore, in an adsorption heat exchanger comprising an adsorbent supported on a substrate sheet by an adhesive, it is preferable to satisfy a second condition: after repeating the above operation 5000 times in a dry state with alternating exposure to an ambient temperature of 70°C and humidity of 20% and a wet state after spraying water onto the adsorption heat exchanger 20, the loading of the adhesive and adsorbent is 90-100%.

[0069] It should be noted that it is preferable to satisfy both the first and second conditions.

[0070] Alternatively, in an adsorption heat exchanger 20 that includes a substrate sheet (fin 26) and an adsorbent 41 supported on the substrate sheet by an adhesive 42, the adhesive 42 and a crosslinking agent can also be used to support the adsorbent 41. By using a crosslinking agent in addition to the adhesive 42, it is possible to suppress the shedding of the adsorbent 41.

[0071] The substrate sheet (fin 26) may also be made of aluminum, for example. Alternatively, it may be made of aluminum with a surface coated using a resin such as epoxy resin, which is preferred. The adsorbent 41 may also contain at least one of sodium polyacrylate, silica, and metal-organic framework (MOF) materials, with sodium polyacrylate being more preferred. The adhesive 42 may also contain at least one of fluororesin, acrylic resin, epoxy resin, and urethane resin, with acrylic resin being more preferred. The crosslinking agent may also be a hydrocarbon having at least one of carbodiimide, isocyanate, and ester groups, with a carboxyl group being more preferred. Various mixtures of the adsorbent 41, adhesive 42, and crosslinking agent can be used.

[0072] In addition, relative to 100 parts by mass of adsorbent 41, the adhesive 42 is preferably used in amounts of 16 parts by mass and 70 parts by mass and the crosslinking agent is preferably used in amounts of 20 parts by mass and 50 parts by mass.

[0073] Compared to 100 parts by weight of adsorbent 41, the adhesive 42 is more preferably used in 20 parts by weight or more, and even more preferably in 23 parts by weight or more. In addition, the adhesive 42 is more preferably used in 50 parts by weight or less, and even more preferably in 30 parts by weight or less.

[0074] Furthermore, the crosslinking agent is preferably used in an amount corresponding to the amount of adhesive 42 used and the acid value or hydroxyl value of adhesive 42. Specifically, the relative acid value or relative hydroxyl value described below is preferably 20% or more and 50% or less.

[0075] First, the acid value (AV) refers to the number of milligrams of potassium hydroxide required to neutralize 1g of resin. Second, the hydroxyl value (OHV) refers to the number of milligrams of potassium hydroxide equivalent to the hydroxyl groups in 1g of sample. Furthermore, the molecular weight of 1 mol of crosslinking agent molecules relative to the functional group (-NCN-) is the NCN equivalent, and the number of grams of the crosslinking agent functional group (NCO) portion contained in 1g of crosslinking agent is the effective NCO weight percentage. It should be noted that the molecular weight of potassium hydroxide is 56.1 g / mol, and the molecular weight of NCO is 42 g / mol.

[0076] In the case of COOH crosslinking, the required amount of crosslinking agent can be calculated using the following formula:

[0077] Crosslinking agent requirement = relative acid value x (amount of adhesive x AV / 56.1) x NCN equivalent / 1000mol

[0078] Furthermore, in the case of OH crosslinking, the required amount of crosslinking agent is calculated according to the following formula:

[0079] Crosslinking agent requirement = relative hydroxyl value x (amount of adhesive x OHV / 56.1) x 42 / (NCO% / 100) / 1000mol

[0080] In these formulas, the desired amount of crosslinking agent is determined by making the relative acid value or relative hydroxyl value 20-50%.

[0081] In other words, the amount of crosslinking agent used preferably contains an amount of acid groups or hydroxyl groups corresponding to 20-50% of the acid groups or hydroxyl groups of the adhesive 42.

[0082] Furthermore, it is preferable to use an additive in addition to the binder 42 and the crosslinking agent to support the adsorbent 41. As the additive, hydrocarbons having carboxyl groups, hydrocarbons having hydroxyl groups, etc., can be used, or they can be mixed together. In particular, hydrocarbons having carboxyl groups are preferred.

[0083] Relative to 100 parts by mass of adsorbent 41, it is preferable to use an additive of 1 part by mass and 5 parts by mass or less. Furthermore, relative to 100 parts by mass of adsorbent 41, it is more preferable to use an additive of 2 parts by mass or more, and even more preferable to use an additive of 3 parts by mass or less.

[0084] (Example)

[0085] --Evaluation of Adhesives--

[0086] Table 1 shows the evaluation of the chemical resistance of the adhesive. Acrylic resin, fluoropolymer resin, and urethane resin were used as the adhesive. Additionally, a crosslinking agent with an acid value of 25% (relative acid value) relative to the adhesive was used. The crosslinking agent was a crosslinking agent with carbodiimide groups.

[0087] Using the aforementioned adhesive and crosslinking agent, sodium polyacrylate was loaded as an adsorbent onto an aluminum substrate to produce a test piece. The test piece was then immersed in a 10% nitric acid aqueous solution and sulfuric acid at 70°C for 40 hours to confirm the loading status.

[0088] As shown in Table 1, acrylic resins and fluoropolymers did not deteriorate (adsorbent detachment). In contrast, urethane resins deteriorated under the influence of nitric acid.

[0089] It should be noted that tetrafluoroethylene-based fluororesins are preferred, but copolymers are also acceptable. The aforementioned fluororesins are copolymers of tetrafluoroethylene and hydrocarbon monomers.

[0090] In addition, regarding the case of immersion in nitric acid, the change in loading is shown.

[0091] In the case of urethane resin, the amount before impregnation was 0.7103 g, which was reduced to 0.0104 g after nitric acid impregnation (under the above conditions), leaving only 1.46%.

[0092] In contrast, with acrylic resin, the loading decreased from 0.7069 g to 0.23046 g, resulting in a loading of 32.59% after the test. With fluoropolymer, the loading decreased from 0.77779 g to 0.7393 g, resulting in a loading of 95.04% after the test.

[0093] Thus, for fluoropolymers, the reduction in loading caused by nitric acid is small, resulting in less degradation when used in adsorption heat exchangers. In the case of acrylic resins, although the reduction in loading caused by nitric acid is greater than that of fluoropolymers, it is significantly better than that of urethane resins, and degradation can be suppressed when they are actually used in adsorption heat exchangers.

[0094] The adhesive is preferably resistant to both nitric acid and sulfuric acid. However, many resins that are resistant to nitric acid are also resistant to sulfuric acid. Therefore, to save costs and time, it is sufficient to conduct a nitric acid resistance test only.

[0095] [Table 1]

[0096]

[0097] The above is an evaluation of the state in which the adsorbent is loaded onto the substrate sheet using an adhesive. In addition, the resin of the adhesive itself was also evaluated.

[0098] Specifically, for the aforementioned acrylic resin, fluororesin, and urethane resin, after measuring the weight of the samples, they were immersed in a 10% nitric acid aqueous solution at 70°C. Then, the removed samples were washed with water, dried at 100°C for one hour, and their weight was measured again.

[0099] The results are shown in Table 2. Due to nitric acid impregnation, the weight of acrylic resin decreased by 16%, and the weight of fluororesin decreased by 5%. In these cases, the performance degradation of the adsorption heat exchanger 20 over time was kept within acceptable limits. In contrast, in the case of urethane resin, due to nitric acid impregnation, the weight decreased by 38%, and in this case, the performance degradation of the adsorption heat exchanger 20 over time exceeded the acceptable range.

[0100] In addition, FT-IR (Fourier Transform Infrared Spectrometry) and TG (Thermogravimetric Analysis) were used to confirm the changes that occurred in each sample under the action of chemicals. For acrylic and fluoropolymer resins, the changes in FT-IR and TG before and after the chemical resistance test were minimal or negligible. In contrast, for urethane resins, significant changes occurred due to the chemical resistance test. In FT-IR, a shift and increase in peak values ​​were observed, indicating changes in molecular structure. A clear curve change was also observed in TG.

[0101] Based on the above results, acrylic resin or fluororesin is preferred as the adhesive.

[0102] [Table 2]

[0103] acrylic resin Fluororubber urethane resin Weight before impregnation (g) 0.114 0.146 0.121 Weight after soaking (g) 0.095 0.138 0.075 Weight reduction rate (%) 16 5 38 determination OK OK NG

[0104] ——Evaluation of crosslinking agents——

[0105] Table 3 shows the evaluation of crosslinking agents. Fluoropolymers were used as adhesives, and crosslinking agents containing isocyanate groups or carbodiimide groups were used as crosslinking agents. Cases where no crosslinking agent was used are also shown. A crosslinking agent with an acid value or hydroxyl value of 25% (relative acid value, relative hydroxyl value) relative to the adhesive was used.

[0106] Similar to the evaluation of the adhesives mentioned above, the adsorbent was loaded onto a substrate sheet and immersed in 10% nitric acid and sulfuric acid at 70°C. The loading status was confirmed after 40 hours.

[0107] As shown in Table 3, degradation occurred without the use of a crosslinking agent. In contrast, no degradation occurred when any crosslinking agent was used.

[0108] [Table 3]

[0109]

[0110] —One Thousand Wet Cycling Tests—

[0111] An adsorption heat exchanger 20, which uses an adhesive to support the adsorption layer 30 on the heat exchanger body 25, was subjected to repeated alternating exposure to dry and wet conditions (dry-wet cycle test), and the adsorbent shedding was evaluated.

[0112] The dry state specifically refers to the state in which the adsorption heat exchanger 20 is placed in a test chamber maintained at 70°C and 20% humidity, and ventilated at an average wind speed of 2.0 m / s. The humid state, on the other hand, refers to the state in which water is sprayed to allow the adsorption layer 30 to fully absorb moisture. A dry-wet cycle test is conducted as follows: the exposure time to the dry state is 9 minutes and 55 seconds, and the exposure time to the humid state is 5 seconds, with the alternating exposure treatment repeated 5000 times.

[0113] More specifically, for example, a duct is installed in a constant temperature bath set to 70°C, and test samples (30×100mm) with multiple heat exchangers are arranged at the duct inlet. Air is introduced into the duct using an air supply device, so that the air contacts the test samples at an average wind speed of 2.0 m / s. Additionally, a water spray nozzle is positioned facing the duct inlet to spray water onto the test samples. Approximately 400 ml of distilled water is used for each spray (wetting state). The water spray is adjusted to ensure that approximately 1 / 4 to 1 / 8 of the test sample on the upwind side is wetted.

[0114] In addition, by measuring the mass of the heat exchanger body 25 before loading the adsorption layer 30, and by measuring the mass of the adsorption heat exchanger 20 before and after the dry-wet cycle test, the changes in the loading (mass) of the binder 42 and adsorbent 41 before and after the test can be determined.

[0115] If the load after the wet-dry cycle test is 90-100% of the load before the test, then sufficient performance can be maintained in actual use of the adsorption heat exchanger 20.

[0116] Table 4 shows the results of the wet and dry cycle tests of Examples 1 and 2, and Comparative Examples 1 and 2 described below.

[0117] (Example 1)

[0118] As the adhesive, a 1:1 (mass ratio) mixture of fluoropolymer and acrylic resin was used. Additionally, a crosslinking agent having carbodiimide groups was used. The crosslinking agent had an acid value or hydroxyl value of 25.5% (relative acid value, relative hydroxyl value) relative to the adhesive. Using the aforementioned adhesive and crosslinking agent, the adsorbent was loaded onto a substrate sheet made of aluminum to produce the test specimen of Example 1.

[0119] (Example 2)

[0120] Acrylic resin was used as the adhesive. Furthermore, the type and amount of crosslinking agent were the same as in Example 1. The adsorbent was loaded onto a substrate sheet made of aluminum using the aforementioned adhesive and crosslinking agent to produce the test specimen of Example 2.

[0121] (Comparative Example 1)

[0122] A urethane resin was used as the adhesive, but no crosslinking agent was used. The adsorbent was loaded onto a substrate sheet made of aluminum using this adhesive, thereby producing the test specimen for Comparative Example 1.

[0123] (Comparative Example 2)

[0124] Acrylic resin was used as the adhesive, but no crosslinking agent was used. The adsorbent was loaded onto a substrate sheet made of aluminum using this adhesive, thereby producing the test specimen for Comparative Example 2.

[0125] The test results of the two examples and two comparative examples are shown in Table 4. In Comparative Examples 1 and 2, the adsorbent did not detach if the number of cycles slightly exceeded 1000. However, in Comparative Example 1, detachment occurred if the number of cycles exceeded 3000, and in Comparative Example 2, detachment occurred below 5000 cycles.

[0126] Compared to these comparative examples, in the case of Example 1, the adsorbent did not detach even after more than 7,000 cycles, but finally detached after more than 10,000 cycles.

[0127] In Example 2, the adsorbent did not detach even after 8530 cycles.

[0128] As described above, when using acrylic resin, fluororesin, and a crosslinking agent, the adsorbent did not detach even after 5000 cycles in a dry-wet cycle test. With this structure, the performance degradation over time of the adsorption heat exchanger is suppressed within acceptable limits.

[0129] [Table 4]

[0130]

[0131] Furthermore, Table 5 shows the loading capacity after wet-dry cycling tests using fluoropolymer, acrylic resin, and urethane resin as adhesives, respectively. Using various adhesives, samples were prepared in the same manner as described above, with the adsorbent loaded onto an aluminum substrate sheet, and the results at the time point of 5452 wet-dry cycles are shown.

[0132] As shown in Table 5, when using fluoropolymer or acrylic resin, the residue rate of the adhesive and adsorbent was 100.00% after 5452 cycles, with no detachment. In contrast, when using urethane resin, the residue rate was 89.97% at the 5452-cycle mark, with more than 10% detaching.

[0133] Thus, by using fluoropolymers or acrylic resins, even after a wet-dry cycle test (5000 cycles), the loading of the adhesive and adsorbent can be maintained at more than 90% of the level before the test, which can suppress the deterioration of the adsorption heat exchanger and is therefore preferred.

[0134] [Table 5]

[0135] acrylic resin Fluororubber urethane resin Residual rate (%) 100.00 100.00 89.97 determination OK OK NG

[0136] —Evaluation of the water permeability of adhesives—

[0137] The type of adhesive affects the performance of the adsorption heat exchanger. Therefore, it is preferable that the resin used as the adhesive, in addition to having excellent chemical resistance, can at least achieve performance close to that of conventional adsorption heat exchangers. In this regard, the inventors know that the water permeability of the adhesive is related to the performance of the adsorption heat exchanger 20. Therefore, the water permeability of each adhesive was evaluated.

[0138] Figure 7 This demonstrates a test method for the water permeability of the adhesive. The adhesive resin film 54 is a film obtained by forming the resin used as the adhesive to a thickness of 100 μm. The opening of a water-impermeable container 51 is covered with the adhesive resin film 54, and the container is sealed. A sufficient amount of desiccant 52 is placed inside the container 51 to achieve a humidity of 0%. The container 51 is then placed in a thermostatic bath 50. The temperature of the thermostatic bath 50 is maintained at 25°C, and the humidity is maintained at 90%.

[0139] In this way, due to the humidity difference with the adhesive resin film 54 as the boundary, moisture moves from the thermostatic bath 50 side (outside of container 51) through the adhesive resin film 54 into container 51 (indicated by arrow 53). Therefore, by measuring the change in the mass of container 51 (including the mass of adhesive resin film 54 and desiccant 52) ​​over time, the amount of moisture that has permeated through the adhesive resin film 54 can be measured.

[0140] Figure 8 The water permeability of four adhesive resin films (54, 100 μm thick) are shown: urethane resin, fluoropolymer resin, a 1:1 mixture of fluoropolymer resin and acrylic resin, and acrylic resin. Units are g / m³. 2 ·day, which is equivalent to 1m 2 The daily water permeability (g) of the membrane area. Multiple measurements were performed, with each result indicated by a black circle (●) and the average value indicated by a white square (◇).

[0141] In addition, the case where the binder is a urethane resin is 100%, and the performance of the adsorption heat exchanger using various resins as binders is expressed by relative values.

[0142] When fluoropolymer is used solely as an adhesive, the water permeability is 60.42 g / m³. 2 • On that day, compared to the case where urethane resin was used as a binder, the performance of the adsorption heat exchanger was 84.8%. In contrast, the water permeability was 86.52 g / m³ when a 1:1 mixture of fluoropolymer and acrylic resin was used as a binder, and when acrylic resin was used alone as a binder. 2 · Tianhe 136.45g / m 2 • The performance of the adsorption heat exchanger was 89.7% and 90.2% respectively, compared to the case where urethane resin was used as a binder.

[0143] From the viewpoint of suppressing the performance degradation of adsorption heat exchangers compared to using urethane resins, a water permeability of 85 g / m³ is preferred. 2 • More than 1 day. However, considering other factors, the use of fluoropolymers may be considered.

[0144] --Tensile strength and elongation of the adhesive--

[0145] Depending on the type, adsorbents swell (increase in volume) after absorbing moisture. For example, sodium polyacrylate swells upon absorbing water. In this case, if the adhesive can stretch along with the adsorbent as it swells, it can prevent deterioration phenomena such as adhesive breakage and adsorbent detachment.

[0146] Specifically, the swelling rate is defined as the ratio of the volume of the adsorbent 41 when it is swollen (in a state where it has absorbed water to the maximum extent) to its volume when it is dry, and is expressed as a percentage % (200% when the volume doubles during swelling, 100% when the volume remains unchanged during swelling, etc.).

[0147] Furthermore, the elongation of adhesive 42 is the ratio of the length L at which the specimen breaks due to the tension at both ends to the initial length L0, expressed as a percentage (%). That is, the elongation is (L / L0) × 100%.

[0148] When the swelling rate of the adsorbent is X (%), if the elongation rate of the adhesive is greater than the cube root of (X / 100) × 100%, the adhesive can elongate sufficiently as the adsorbent swells, thereby preventing breakage.

[0149] Figure 9 The method for testing elongation is shown below. A test piece 60 with a width of 1 cm, a length of 7 cm, and a film thickness of 10–300 μm is prepared using a resin as an adhesive. For this test piece, a 1 cm holding area 61 is clamped at each end using clamps and stretched to both sides until the test piece 60 breaks. Since the initial distance between the clamps is the length of the extension area 62 (5 cm), the elongation can be determined by measuring the distance between the clamps at the point of breakage.

[0150] When the swelling ratio of the adsorbent is X, its elongation in size is the cube root of X. Therefore, if the elongation of the adhesive resin film 54 is greater than the cube root of X, the breakage of the adhesive due to the swelling of the adsorbent can be suppressed.

[0151] In addition, the tensile strength of adhesive 42 is preferably 12 N / mm. 2 Below, 8 N / mm is preferred. 2 The following is a further preferred value: 6N / mm 2 The following applies. If such an adhesive 42 is used, the adhesive 42 easily stretches as the adsorbent 41 swells, thus inhibiting the adsorbent 41 from falling off.

[0152] Regarding this, Figure 10 The diagram illustrates the relationship between the elongation (L-L0) and the applied force (force per unit cross-sectional area) of urethane resins, fluoropolymers, and mixtures of fluoropolymers and acrylic resins. For mixtures, three mass mixing ratios of fluoropolymer to acrylic resin are shown: 3:7, 5:5, and 7:3. As the elongation increases, the applied force increases, and the force at break decreases to zero.

[0153] The elongation at the fracture point all exceeded 50.0 mm. Compared with the initial length of 50.0 mm, the length at fracture exceeded 100.0 mm, so the elongation rate was more than 200%.

[0154] Here, the swelling ratio of sodium polyacrylate is approximately 200%. Therefore, if the elongation of the adhesive is 200 / 100 cube root × 100%, or approximately 126% or more, breakage can be avoided. Figure 10 The examples shown all satisfy this condition.

[0155] Furthermore, in the case of adsorbent swelling, the resin used as a binder is preferably a resin that is easily elongated. That is, when using a binder that elongates under relatively small forces, it is easier for the resin to elongate due to adsorbent swelling, and therefore this is preferred. Specifically, a tensile strength of 12 N / mm is preferred. 2 The following is preferred: 8 N / mm. 2 The following is a further preferred value: 6N / mm 2 the following.

[0156] Therefore, from this perspective, it is preferable to use a mixture of fluoropolymer and acrylic resin.

[0157] The embodiments have been described above, but it should be understood that various changes can be made to the embodiments and specific details without departing from the spirit and scope of the claims. The above embodiments and variations can also be appropriately combined or substituted as long as the function of the object of this disclosure is not affected.

[0158] -Industry Applicability-

[0159] In summary, this disclosure is useful for adsorption heat exchangers.

[0160] - Symbol Explanation -

[0161] 20 Adsorption heat exchanger

[0162] 25 Heat exchanger body

[0163] 26. Fins (substrate sheets)

[0164] 30 Adsorption layer

[0165] 41 Adsorbent

[0166] 42 Adhesives

[0167] 43 Coating

[0168] 50 constant temperature bath

[0169] 51 Containers

[0170] 52 Desiccant

[0171] 53 arrows

[0172] 54 Adhesive resin film

[0173] 60 test pieces

[0174] 61. Maintain the area

[0175] 62 Extended Area

Claims

1. An adsorption heat exchanger (20) comprising a substrate sheet (26) and an adsorbent (41) supported on the substrate sheet (26) by an adhesive (42), characterized in that: The adsorbent (41) absorbs and releases moisture from the air. The adhesive (42) contains at least one of fluoropolymer, acrylic resin and epoxy resin. The adsorbent (41) contains at least one of the following: an organic polymer material having multiple cross-linked polymer backbones forming a three-dimensional structure, silica, and a metal-organic framework material. The adsorption heat exchanger satisfies the first condition. The first condition is that, at an ambient temperature of 70°C, after immersing the substrate sheet (26) with the adsorbent (41) in a 10% nitric acid aqueous solution for 40 hours, the loading of the adhesive (42) and the adsorbent (41) is 32-95.04% of that before immersion.

2. The adsorption heat exchanger according to claim 1, characterized in that: The combined thickness of the adhesive (42) and the adsorbent (41) is in the range of more than 20 μm and less than 120 μm.

3. The adsorption heat exchanger according to claim 1 or 2, characterized in that: The adhesive contains at least one of a fluoropolymer and an acrylic resin. The adhesive (42) and crosslinking agent are used to support the adsorbent (41). The crosslinking agent is a hydrocarbon compound having at least one of a carbodiimide group and an isocyanate group.

Citation Information

Patent Citations

  • Humidity adjusting device

    JP2009019863A

  • Acid-resistant heatproof elastic bonding agent and preparation method thereof

    CN105820790A

  • Heat transfer fin, and heat exchanger

    JP2012077987A