Ortho-cresol isomerization catalyst and preparation method thereof and ortho-cresol isomerization method
By using nano HEU-1 molecular sieve and modified elements, the catalysts prepared by short catalyst life and low conversion rate are solved, and an efficient o-cresol isomerization reaction is achieved, which is suitable for industrial applications.
Patent Information
- Application Number
- CN202111296976.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-10-29
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2041-10-29
AI Technical Summary
In the prior art, the catalyst life of p-cresol between production by isomerization of o-cresol has a short catalyst life, a low conversion rate and a large number of by-products, resulting in difficulties in industrial application.
Nano HEU-1 molecular sieve is used as an active component, combined with modified elements, and the catalyst is prepared through the molding and calcining process, and the acidity is adjusted to improve the stability and conversion of the catalyst, and is suitable for fixed bed reactors.
It achieves long life and high conversion rate of catalysts, reduces by-product generation, and is suitable for industrial promotion.
Smart Images

Figure BDA0003329276400000141 
Figure BDA0003329276400000142 
Figure BDA0003329276400000143
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of isomerization catalysts, and in particular to an o-cresol isomerization catalyst and a preparation method thereof, and an o-cresol isomerization method. Background Art
[0002] Cresol is an important fine chemical intermediate, including three isomers: o-cresol, p-cresol and m-cresol. Among them, o-cresol is used in synthetic resins, herbicides, disinfectants, preservatives, plasticizers and fragrances; m-cresol can be used in analytical reagents and organic synthesis, and is an important raw material for antioxidants, vitamin E, synthetic resins, color film developers, etc.; p-cresol is the main raw material for the production of antioxidants, fluorescent brighteners, plasticizers, medical disinfectants, dyes, fragrances, curing agents and other products.
[0003] At present, my country has a strong demand for cresol monomers, and o-cresol is relatively easy to obtain, with a large domestic production and a relatively low price. However, the domestic supply of p-cresol and m-cresol is seriously insufficient, and large quantities of imports are needed to meet domestic market demand.
[0004] The production of m-p-cresol by isomerization of o-cresol has the advantages of high selectivity, few by-products, good atom economy and low environmental pollution, and has great application prospects. US4503269 discloses an autoclave and fixed bed reaction process for the isomerization reaction of o-cresol using HZSM-5 molecular sieve. A large amount of by-products such as phenol, xylenol and trimethylol are generated in the autoclave reaction process. The selectivity of p-cresol in the fixed bed reaction is high, the side reactions are few, the phenol yield is less than 4%, and the total yield of m-p-cresol is 50%, but the catalyst life is short.
[0005] US4691063 discloses a HZSM-5 molecular sieve formed by silica sol and modified by phosphorus for isomerization reaction of o-cresol. The phenol yield in the fourth hour of reaction is 3.8%, and the total yield of m-cresol is up to 52%. However, after 20 hours of reaction, the activity of the catalyst decreases a lot. If used in a fixed bed reactor, it needs frequent regeneration, which makes industrial application difficult.
[0006] CN103449976B reports a moving bed method for isomerizing o-cresol to produce m-cresol, and CN103341363B discloses a moving bed cresol isomerization catalyst. HZSM-5 is used as the active component, and after element and surface silicon modification, it is mixed with clay to obtain a moving bed reaction catalyst with high mechanical strength and wear resistance. The moving bed catalyst has a maximum o-cresol conversion rate of 55%, a m-cresol yield of 40%, a p-cresol yield of 14%, and a phenol yield of less than 1%. However, the moving bed process equipment is complex and requires a high degree of automation.
[0007] CN103342629A discloses a fluidized bed method for isomerizing o-cresol to produce m-cresol, and uses molecular sieve as an active component to prepare a catalyst. ZSM-5 molecular sieve catalyst has the highest activity, with an o-cresol conversion rate of 61% and a m / p-cresol selectivity of 96%. However, the fluidized bed process equipment is complex, the operation is difficult, and the production cost is high.
[0008] CN104923293B discloses a catalyst for isomerization of o-cresol and a process for catalyzing the synthesis of m-cresol using the catalyst. The method uses a silicon source and an aluminum source as raw materials to add a template agent, synthesizes an MCM-41 / ZSM-5 composite molecular sieve by a two-step crystallization method, and then undergoes ion exchange to form an H-type, and is mixed with a binder to form a catalyst. In a fixed bed reactor, the conversion rate of o-cresol is up to 54%, the selectivity of m-cresol is 98%, and the reaction time is 1000 hours, the conversion rate is 52%, and the selectivity of m-cresol is 98%. The catalyst has a long life, but its preparation process is more complicated, and there is room for further improvement in processing capacity and reaction activity. Summary of the invention
[0009] The purpose of the present invention is to solve the problems of short catalyst life, low ortho-cresol conversion rate, and many by-products in producing m-p-cresol by isomerization of ortho-cresol, and to provide an ortho-cresol isomerization catalyst and a preparation method thereof, as well as an ortho-cresol isomerization method.
[0010] In order to achieve the above-mentioned object, the first aspect of the present invention provides an o-cresol isomerization catalyst, wherein the catalyst comprises 10-90 parts by weight of nano HEU-1 molecular sieve, 10-90 parts by weight of binder and 0.1-10 parts by weight of modifying element; wherein the modifying element is selected from one or more of Group IIIB elements, Group IIA elements, Group VA elements and Group VIIA elements.
[0011] The second aspect of the present invention provides a method for preparing the o-cresol isomerization catalyst according to the first aspect of the present invention, the method comprising the following steps:
[0012] (1) forming a mixture containing nano-HEU-1 molecular sieve, alumina precursor and nitric acid to obtain formed particles, and then calcining the formed particles for the first time to obtain a calcined product;
[0013] (2) loading a modifying element on the calcined product to obtain a loaded calcined product, and then calcining the loaded calcined product for a second time to obtain the o-cresol isomerization catalyst; wherein the modifying element is selected from one or more of Group IIIB elements, Group IIA elements, Group VA elements and Group VIIA elements.
[0014] The third aspect of the present invention provides a method for isomerizing o-cresol, which comprises contacting o-cresol with the o-cresol isomerization catalyst described in the first aspect of the present invention to carry out an isomerization reaction to obtain p-cresol and m-cresol.
[0015] Through the above technical solution, the beneficial technical effects achieved by the present invention are as follows:
[0016] 1) The o-cresol isomerization catalyst provided in the present invention uses nano HEU-1 molecular sieve as an active component, and the catalyst is modified by using a modifying element, so that the pore size of the HEU-1 molecular sieve is substantially not changed while adjusting the acidity of the HEU-1 molecular sieve, so that the o-cresol isomerization catalyst can not only have a high o-cresol conversion rate and m-cresol yield, but also has a high stability of the catalyst, can be regenerated and used multiple times, and has a long catalyst life;
[0017] 2) The preparation method of the o-cresol isomerization catalyst provided in the present invention is applicable to a fixed bed, is simple to operate, and is suitable for industrial promotion. DETAILED DESCRIPTION
[0018] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0019] The first aspect of the present invention provides an o-cresol isomerization catalyst, wherein the catalyst comprises 10-90 parts by weight of nano HEU-1 molecular sieve, 10-90 parts by weight of alumina and 0.1-10 parts by weight of a modifying element; wherein the modifying element is selected from one or more of group IIIB elements, group IIA elements, group VA elements and group VIIA elements.
[0020] In the present invention, although the nano-HEU-1 molecular sieve also contains alumina, the content of alumina defined in the present invention when describing the composition of the catalyst refers to the content of alumina outside the nano-HEU-1 molecular sieve, and does not include the content of alumina in the nano-HEU-1 molecular sieve. The content of nano-HEU-1 molecular sieve and alumina in the catalyst is the feed amount in the catalyst preparation process. The content of the modifying element in the catalyst can be obtained by testing using X-ray fluorescence spectroscopy. When the modifying element is selected from group IIIB elements, group IIA elements, and group VA elements, the content of the modifying element in the catalyst can also be the feed amount in the catalyst preparation process. However, when the modifying element contains group VIIA elements, since group VIIA elements are significantly lost during the preparation process, the content of the modifying element is preferably analyzed using X-ray fluorescence spectroscopy.
[0021] In the present invention, the inventors of the present invention use nano HEU-1 molecular sieve as the active component and modify the catalyst using modifying elements, while adjusting the acidity of the HEU-1 molecular sieve, the pore size of the HEU-1 molecular sieve will not be substantially changed, so that the o-cresol isomerization catalyst can not only have a higher o-cresol conversion rate and m-cresol yield, but also the catalyst has higher stability and a longer service life.
[0022] In a preferred embodiment, the catalyst comprises 50-80 parts by weight, preferably 60-70 parts by weight of nano HEU-1 molecular sieve, 20-50 parts by weight, preferably 30-40 parts by weight of alumina and 2-7 parts by weight, preferably 2-5 parts by weight of modifying elements.
[0023] In a preferred embodiment, the crystal size of the nano HEU-1 molecular sieve is 1-200 nm, preferably 20-100 nm, and more preferably 40-60 nm.
[0024] In a preferred embodiment, the molar ratio of silicon dioxide to aluminum oxide in the nano HEU-1 molecular sieve is 20-100:1, preferably 25-75:1, and more preferably 35-45:1.
[0025] In a preferred embodiment, the IIIB group element is selected from one or more of Y, Ce, La, Pr and Nd, preferably Ce and / or La; the IIA group element is selected from one or more of Mg, Ca, Sr and Ba, preferably Mg; the VA group element is selected from P, and the VIIA group element is selected from Cl and / or F.
[0026] In a preferred embodiment, the modifying element is a Group IIIB element and a Group VA element, or a Group IIIB element and a Group VIIA element.
[0027] In a preferred embodiment, the modifying elements are group IIIB elements and group VA elements, wherein the mass ratio of the group IIIB elements to the group VA elements is 1-2:1, preferably 1.1-1.5:1.
[0028] In a preferred embodiment, the modifying elements are group IIIB elements and group VIIA elements, wherein the mass ratio of the group IIIB elements to the group VIIA elements is 1-3:1, preferably 1.4-1.8:1.
[0029] A second aspect of the present invention provides a method for preparing an o-cresol isomerization catalyst, the method comprising the following steps:
[0030] (1) forming a mixture containing nano-HEU-1 molecular sieve, alumina precursor and nitric acid to obtain formed particles, and then calcining the formed particles for the first time to obtain a calcined product;
[0031] (2) loading a modifying element on the calcined product to obtain a loaded calcined product, and then calcining the loaded calcined product for a second time to obtain the o-cresol isomerization catalyst; wherein the modifying element is selected from one or more of Group IIIB elements, Group IIA elements, Group VA elements and Group VIIA elements.
[0032] In step (1):
[0033] In a preferred embodiment, the crystal size of the nano HEU-1 molecular sieve is 1-200 nm, preferably 20-100 nm, and more preferably 40-60 nm.
[0034] In a preferred embodiment, the molar ratio of silicon dioxide to aluminum oxide in the nano-HEU-1 molecular sieve is preferably 20-100:1, preferably 25-75:1, and more preferably 35-45:1.
[0035] In a preferred embodiment, the alumina precursor is selected from one or more of aluminum sol, aluminum gel, and pseudo-boehmite, preferably pseudo-boehmite.
[0036] In a preferred embodiment, based on the mass of aluminum oxide in the aluminum oxide precursor, the mass ratio of the nano HEU-1 molecular sieve to the aluminum oxide precursor is 10-90:10-90, preferably 50-80:20-50, and more preferably 60-70:30-40.
[0037] In a preferred embodiment, the concentration of nitric acid is 0.5-10 wt %, preferably 1-3 wt %.
[0038] In a preferred embodiment, the mass of the nitric acid is 20-55%, preferably 45-50%, of the sum of the mass of the nano-HEU-1 molecular sieve and the alumina precursor.
[0039] In a preferred embodiment, the molding is selected from compression molding, rolling molding, spray molding, and extrusion molding, preferably extrusion molding.
[0040] The present invention does not specifically limit the operating conditions of the molding, and the molding can be carried out according to conventional operations in the art. The present invention also does not specifically limit the molding shape and size of the molded particles, which can be clover, four-leaf clover, cylindrical, hollow, etc. The specific shape and size can be selected according to actual needs.
[0041] In a preferred embodiment, the shaped particles are dried before being calcined for the first time.
[0042] In a preferred embodiment, the operating conditions of the first calcination include: the first calcination temperature is 380-600° C., preferably 400-560° C.; the first calcination time is 2-10 h, preferably 4-6 h.
[0043] In step (2):
[0044] In a preferred embodiment, the IIIB group element is selected from one or more of Y, Ce, La, Pr and Nd, preferably Ce and / or La; the IIA group element is selected from one or more of Mg, Ca, Sr and Ba, preferably Mg; the VA group element is selected from P, and the VIIA group element is selected from Cl and / or F.
[0045] In a preferred embodiment, the loading operation method comprises: mixing the calcined product with a solution containing a modified element precursor, stirring at 40-90° C. for 1-5 hours and then drying to obtain a loaded calcined product.
[0046] In a preferred embodiment, the modifying element precursor is selected from a soluble compound containing the modifying element. The present invention does not specifically limit the soluble compound containing the modifying element, and the modifying element precursor may be a nitrate or chloride containing a IIIB group element and a IIA group element, such as a nitrate or chloride containing Y, Ce, La, Pr, Nd, Mg, Ca, Sr, and Ba; or an ammonium salt or acid containing a VA group element and a VIIA group element, such as NH4F, NH4Cl, (NH4)2HPO4 or (NH4)H2PO4, HF, H3PO4, or HCl.
[0047] In a preferred embodiment, the solvent in the solution containing the modifying element precursor is water, and the concentration of the modifying element precursor is 2-20 wt %, preferably 4-10 wt %.
[0048] In a preferred embodiment, the feeding amount of the calcined product and the solution containing the modifying element precursor is such that in the prepared catalyst, the mass ratio of nano HEU-1 molecular sieve and the modifying element is 10-90:0.1-10, preferably 50-80:2-7, and further preferably 60-70:2-5.
[0049] In a preferred embodiment, when the modifying element is selected from Group IIIB elements, Group IIA elements or Group VA elements, the amount of the modifying element added is preferably the same as the content of the modifying element in the prepared catalyst; further preferably, the amount of the solution containing the modifying element precursor is 1.01-1.08 times the content of the modifying element in the prepared catalyst, preferably 1.01-1.04 times.
[0050] In a preferred embodiment, when the modifying element is selected from Group VIIA elements, due to the loss of Group AII elements during the preparation process, the feeding amount of the solution containing the modifying element precursor is preferably 1.5-20 times the content of the modifying element in the prepared catalyst.
[0051] In a preferred embodiment, the modifying elements are group IIIB elements and group VA elements. During loading, the group VA elements are first loaded on the calcined product to obtain a loaded product containing group VA elements, and then the group IIIB elements are loaded on the loaded product containing group VA elements to obtain a loaded calcined product; wherein the feeding amount of the modifying element precursor is such that the mass ratio of group IIIB elements to group VA elements in the loaded calcined product is 1-2:1, preferably 1.1-1.5:1.
[0052] In a preferred embodiment, the modifying elements are group IIIB elements and group VIIA elements. During loading, the group VA elements are first loaded on the calcined product to obtain a loaded product containing group VIIA elements, and then the group IIIB elements are loaded on the loaded product containing group VIIA elements to obtain a loaded calcined product; wherein the feeding amount of the modifying element precursor is such that the element mass ratio of group IIIB elements to group VIIA elements in the loaded calcined product is 1-3:1, preferably 1.4-1.8:1.
[0053] In a preferred embodiment, the operating conditions of the second calcination include: the second calcination temperature is 450-550° C., preferably 480-520° C.; the second calcination time is 2-10 h, preferably 3-6 h.
[0054] In a preferred embodiment, the present invention does not impose any special limitation on drying, and the drying may be carried out according to conventional operations, for example, the drying may be carried out at 90-120° C. for 2-6 hours.
[0055] In a preferred embodiment, the method further comprises the step (3) of subjecting the o-cresol isomerization catalyst to steam treatment.
[0056] In step (3):
[0057] In a preferred embodiment, the water vapor treatment is carried out under an oxygen-containing atmosphere at normal pressure, and the oxygen-containing atmosphere is selected from air and / or oxygen. The normal pressure is not particularly limited in the present invention and can be understood in accordance with common sense.
[0058] In a preferred embodiment, the operating conditions of the water vapor treatment include: the mass space velocity of the water vapor is 0.2-3h -1 , preferably 0.5-1.2h -1 ; The treatment temperature is 250-400°C, preferably 300-380°C; The treatment time is 4-10h, preferably 6-8h.
[0059] The third aspect of the present invention provides a method for isomerizing o-cresol, which comprises contacting o-cresol with the o-cresol isomerization catalyst described in the first aspect of the present invention to carry out an isomerization reaction to obtain p-cresol and m-cresol.
[0060] In a preferred embodiment, the operating conditions of the isomerization reaction include: reaction temperature of 300-450°C; reaction pressure of 0.1-2.5 MPa; mass space velocity of o-cresol of 1-5 h -1 ; The volume ratio of hydrogen to o-cresol is 200-600:1.
[0061] In a preferred embodiment, the reaction is carried out in a fixed bed reactor.
[0062] The present invention will be described in detail below by way of examples. The pseudo-boehmite used in the examples and comparative examples is produced by Condea of Germany and is branded as Pural SB powder. The mass content of the modifying element in the catalyst is tested by X-ray fluorescence spectroscopy.
[0063] Example 1
[0064] (1) mixing nano-HEU-1 molecular sieve (average particle size of 50 nm, silica / alumina molar ratio of 35), pseudo-boehmite and 1 wt% of dilute nitric acid, extruding the mixed mixture to obtain shaped particles, drying the shaped particles at 110° C. for 4 h, and then calcining them for the first time, and calcining them at 540° C. for 5 h to obtain a calcined product; wherein the mass ratio of nano-HEU-1 molecular sieve to pseudo-boehmite is 65:35 based on the mass of alumina in the pseudo-boehmite, and the amount of dilute nitric acid added is 50% of the sum of the mass of nano-HEU-1 molecular sieve and pseudo-boehmite;
[0065] (2) The above-mentioned calcined product was mixed with 4 wt% La(NO3)3 solution, and dried after stirring at 80°C for 1.5 hours, and then dried at 110°C for 4 hours to obtain a loaded calcined product; the loaded calcined product was calcined for a second time at 520°C for 5 hours to obtain an o-cresol isomerization catalyst; wherein, based on the mass of the nano HEU-1 molecular sieve in the calcined product and the mass of the La element in the La(NO3)3 solution, the mass ratio of the calcined product to the La(NO3)3 solution was 65:2.3;
[0066] (3) The above-mentioned o-cresol isomerization catalyst is treated with water vapor in an air atmosphere at a mass space velocity of 1 h -1 , the treatment temperature is 360°C, the treatment time is 6h, and o-cresol isomerization catalyst A-1 is obtained.
[0067] In the o-cresol isomerization catalyst A-1 prepared in Example 1, the La element content is 2.24 wt %, and the mass ratio of nano HEU-1 molecular sieve, alumina and modifying element (La) is 65:35:2.24.
[0068] Example 2
[0069] Same as Example 1, except that:
[0070] (2) The calcined product was mixed with a 5 wt % Mg(NO3)2 solution, stirred at 80°C for 1.5 h, and then dried, and then dried at 110°C for 4 h to obtain a loaded calcined product; the loaded calcined product was calcined for a second time at 520°C for 5 h to obtain an o-cresol isomerization catalyst; wherein the mass ratio of the calcined product to the Mg(NO3)2 solution was 65:2.5 based on the mass of the nano HEU-1 molecular sieve in the calcined product and the mass of the Mg element in the Mg(NO3)2 solution;
[0071] (3) The above-mentioned o-cresol isomerization catalyst was treated with water vapor in an air atmosphere, and the mass space velocity of the water vapor was 0.5h -1, the treatment temperature is 370°C, the treatment time is 8h, and o-cresol isomerization catalyst A-2 is obtained.
[0072] In the o-cresol isomerization catalyst A-2 prepared in Example 2, the Mg content is 2.42 wt %, and the mass ratio of nano HEU-1 molecular sieve, alumina and modifying element (Mg) is 65:35:2.42.
[0073] Example 3
[0074] Same as Example 1, except that:
[0075] (2) The calcined product was mixed with 8 wt % (NH4)2HPO4 solution, stirred at 90°C for 1 hour and then dried, and dried at 110°C for 4 hours to obtain a loaded calcined product; the loaded calcined product was calcined for a second time at 520°C for 5 hours to obtain an o-cresol isomerization catalyst; wherein, based on the mass of the nano HEU-1 molecular sieve in the calcined product and the mass of the P element in the (NH4)2HPO4 solution, the mass ratio of the calcined product to the (NH4)2HPO4 solution was 65:2.6;
[0076] (3) The above-mentioned o-cresol isomerization catalyst was treated with steam in an oxygen atmosphere at a mass space velocity of 1.2 h -1 , the treatment temperature is 380°C, the treatment time is 6h, and o-cresol isomerization catalyst A-3 is obtained.
[0077] In the o-cresol isomerization catalyst A-3 prepared in Example 3, the P element content is 2.56 wt %, and the mass ratio of nano-HEU-1 molecular sieve, alumina and modifying element (P) is 65:35:2.56.
[0078] Example 4
[0079] Same as Example 1, except that:
[0080] (2) The above-mentioned calcined product was mixed with 8wt% (NH4)2HPO4 solution, stirred at 90°C for 1h, dried, and dried at 110°C for 4h to obtain a loaded product containing P; the loaded product containing P was mixed with 4wt% La(NO3)3 solution, stirred at 80°C for 1.5h, dried, and dried at 110°C for 4h to obtain a loaded calcined product; the loaded calcined product was calcined for a second time at 520°C for 5h to obtain an o-cresol isomerization catalyst; wherein, based on the mass of nano HEU-1 molecular sieve in the calcined product, the mass of P element in the (NH4)2HPO4 solution, and the mass of La element in the La(NO3)3 solution, the mass ratio of the calcined product to the (NH4)2HPO4 solution was 65:2.3; the mass ratio of the calcined product to the La(NO3)3 solution was 65:1.9;
[0081] (3) The above-mentioned o-cresol isomerization catalyst is treated with steam in an oxygen atmosphere at a mass space velocity of 1 h -1 , the treatment temperature is 380°C, the treatment time is 8h, and o-cresol isomerization catalyst A-4 is obtained.
[0082] In the o-cresol isomerization catalyst A-4 prepared in Example 4, the P element content is 2.24wt%, and the La element content is 1.88wt%; the mass ratio of nano-HEU-1 molecular sieve, alumina and modifying elements (P and La) is 65:35:4.12.
[0083] Example 5
[0084] Same as Example 1, except that:
[0085] (2) The above-mentioned calcined product was mixed with 10wt% NH4F solution in a mass ratio of 1:5, and the mixture was dried after stirring at 80°C for 2h, and then dried at 110°C for 4h to obtain a loaded product containing F; the loaded product containing F was mixed with 4wt% Ce(NO3)3 solution, and the mixture was dried after stirring at 80°C for 1.5h, and then dried at 110°C for 4h to obtain a loaded calcined product, and the loaded calcined product was calcined for a second time at 520°C for 5h to obtain an o-cresol isomerization catalyst; wherein, based on the mass of nano HEU-1 molecular sieve in the calcined product and the mass of Ce element in the Ce(NO3)3 solution, the mass ratio of the calcined product to the Ce in the Ce(NO3)3 solution is 65:1.8.
[0086] (3) The above-mentioned o-cresol isomerization catalyst was treated with steam in an air atmosphere at a mass space velocity of 1.2 h -1 , the treatment temperature is 360°C, the treatment time is 8h, and o-cresol isomerization catalyst A-5 is obtained.
[0087] In the o-cresol isomerization catalyst A-5 prepared in Example 5, the F element content is 2.54wt%, and the Ce element content is 1.73wt%; the mass ratio of the nano HEU-1 molecular sieve, the oxidant and the modifying element (F and Ce) is 65:35:4.27.
[0088] Example 6
[0089] Same as Example 1, except that:
[0090] In step (1), HEU-1 molecular sieve with a silica / alumina molar ratio of 50 and an average particle size of 50 nm is used to replace the nano HEU-1 molecular sieve with a silica / alumina molar ratio of 35 and an average particle size of 50 nm;
[0091] In step (2), the mass ratio of the calcined product to the La(NO3)3 solution is 65:2.4, based on the mass of the nano HEU-1 molecular sieve in the calcined product and the mass of the La element in the La(NO3)3 solution;
[0092] Step (3) The above-mentioned o-cresol isomerization catalyst is subjected to steam treatment in an air atmosphere, and the mass space velocity of the steam is 0.8h -1 , the treatment temperature is 380°C, the treatment time is 6h, and o-cresol isomerization catalyst A-6 is obtained.
[0093] In the o-cresol isomerization catalyst A-6 prepared in Example 6, the La element content is 2.37 wt %, and the mass ratio of nano HEU-1 molecular sieve, alumina and modifying element (La) is 65:35:2.37.
[0094] Comparative Example 1
[0095] The same as Example 1, except that only step (1) is performed.
[0096] (1) Nano-HEU-1 molecular sieve (average particle size of 50 nm, silicon oxide / aluminum oxide molar ratio of 35), pseudo-boehmite and 1 wt% of dilute nitric acid are mixed, and the mixed mixture is extruded to obtain molded particles, and the molded particles are dried at 110° C. for 4 hours and then calcined for the first time, and then calcined at 540° C. for 5 hours to obtain a calcined product; wherein the mass ratio of nano-HEU-1 molecular sieve to pseudo-boehmite is 65:35 based on the mass of aluminum oxide in the pseudo-boehmite, and the amount of dilute nitric acid added is 50% of the sum of the mass of nano-HEU-1 molecular sieve and pseudo-boehmite.
[0097] The calcined product was used as o-cresol isomerization catalyst D-1. In the o-cresol isomerization catalyst D-1 prepared in Comparative Example 1, the mass ratio of nano HEU-1 molecular sieve and alumina was 65:35.
[0098] Comparative Example 2
[0099] Same as Example 1, except that:
[0100] In step (1), the nano-HEU-1 molecular sieve in Example 1 is replaced by an HZSM-5 molecular sieve having a silicon oxide / aluminum oxide molar ratio of 38 and an average particle size of 50 nm.
[0101] Omit step (3).
[0102] In the o-cresol isomerization catalyst D-2 prepared in Comparative Example 2, the La element content is 2.07 wt %, the mass ratio of the HZSM-5 molecular sieve, the oxidant and the modifying element (La) is 65:35:2.07.
[0103] Comparative Example 3
[0104] Same as Example 4, except that:
[0105] In step (1), the nano HEU-1 molecular sieve is replaced by an HZSM-5 molecular sieve having a silicon oxide / aluminum oxide molar ratio of 38 and an average particle size of 50 nm.
[0106] Omit step (3).
[0107] In the o-cresol isomerization catalyst D-3 prepared in Comparative Example 3, the P element content is 2.30wt%, and the La element content is 1.95wt%; the mass ratio of HZSM-5 molecular sieve, oxidant and modifying element (P and La) is 65:35:4.25.
[0108] Test Example 1
[0109] The o-cresol isomerization catalysts prepared in Examples 1-6 and Comparative Examples 1-3 were respectively loaded into a fixed bed microreactor for o-cresol isomerization reaction, with H2 as carrier gas, a volume ratio of hydrogen to o-cresol of 400:1, and a mass space velocity of o-cresol of 1 h -1 , the reaction temperature is 400℃, the reaction pressure is 0.1MPa, and the experimental results are shown in Table 1.
[0110] The reaction is stopped when the instantaneous o-cresol conversion rate of o-cresol in the reaction drops to 10%. The o-cresol conversion rate, m-cresol yield, p-cresol yield and phenol yield are calculated according to the o-cresol feed amount and the product generation amount during the whole reaction process.
[0111]
[0112]
[0113]
[0114]
[0115] Table 1
[0116]
[0117]
[0118] Test Example 2
[0119] The deactivated catalysts obtained after the reaction in Examples 1-6 and Comparative Examples 1-3 were regenerated by burning carbon with air containing 5% by volume of oxygen, and then the test of Test Example 1 was repeated under the same conditions. When the regeneration test was performed, if the initial o-cresol conversion rate of the regenerated catalyst was measured to be lower than 30%, the regeneration test was stopped. The regeneration times and the experimental results of the o-cresol conversion rate, m-cresol yield, p-cresol yield and phenol yield in the last regeneration test are shown in Table 2.
[0120] Table 2
[0121]
[0122] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for isomerizing o-cresol, characterized in that: The method comprises contacting o-cresol with an o-cresol isomerization catalyst to carry out an isomerization reaction to obtain p-cresol and m-cresol; Wherein, the o-cresol isomerization catalyst comprises 10-90 parts by weight of nano HEU-1 molecular sieve, 10-90 parts by weight of alumina and 0.1-10 parts by weight of modifying elements; wherein, the modifying elements are selected from one or more of group IIIB elements, group IIA elements, group VA elements and group VIIA elements; the group IIIB elements are selected from one or more of Y, Ce, La, Pr and Nd; the group IIA elements are selected from one or more of Mg, Ca, Sr and Ba; the group VA elements are selected from P, and the group VIIA elements are selected from Cl and / or F.
2. The method according to claim 1, wherein: The o-cresol isomerization catalyst comprises 50-80 parts by weight of nano HEU-1 molecular sieve, 20-50 parts by weight of aluminum oxide and 2-7 parts by weight of a modifying element.
3. The method according to claim 2, wherein: The o-cresol isomerization catalyst comprises 60-70 parts by weight of nano HEU-1 molecular sieve, 30-40 parts by weight of aluminum oxide and 2-5 parts by weight of a modifying element.
4. The method according to claim 1 or 2, wherein: The crystal size of the nano HEU-1 molecular sieve is 1-200 nm; The molar ratio of silicon dioxide to aluminum oxide in the nano HEU-1 molecular sieve is 20-100:
1.
5. The method according to claim 4, wherein: The crystal size of the nano HEU-1 molecular sieve is 20-100 nm; The molar ratio of silicon dioxide to aluminum oxide in the nano HEU-1 molecular sieve is 25-75:
1.
6. The method according to claim 5, wherein: The crystal size of the nano HEU-1 molecular sieve is 40-60 nm; The molar ratio of silicon dioxide to aluminum oxide in the nano HEU-1 molecular sieve is 35-45:
1.
7. The method according to claim 1, wherein: The IIIB group element is Ce and / or La; the IIA group element is Mg.
8. The method according to claim 1, wherein: The operating conditions of the isomerization reaction include: reaction temperature of 300-450°C; reaction pressure of 0.1-2.5MPa; mass space velocity of o-cresol of 1-5h -1 ; The volume ratio of hydrogen to o-cresol is 200-600:
1.
9. A method for preparing the o-cresol isomerization catalyst used in the method according to claims 1-8, wherein: The method comprises the following steps: (1) forming a mixture containing nano-HEU-1 molecular sieve, alumina precursor and nitric acid to obtain formed particles, and then calcining the formed particles for the first time to obtain a calcined product; (2) loading a modifying element on the calcined product to obtain a loaded calcined product, and then calcining the loaded calcined product for a second time to obtain the o-cresol isomerization catalyst; wherein the modifying element is selected from one or more of group IIIB elements, group IIA elements, group VA elements and group VIIA elements; Step (3), subjecting the o-cresol isomerization catalyst to steam treatment.
10. The preparation method according to claim 9, wherein: In step (1), the oxidant precursor is selected from one or more of aluminum sol, aluminum gel, and pseudo-boehmite; and / or, the mass ratio of the nano HEU-1 molecular sieve to the binder precursor is 10-90:10-90, based on the mass of the corresponding aluminum oxide in the aluminum oxide precursor; and / or, the concentration of the nitric acid is 0.5-10wt%; And / or, the mass of the nitric acid is 20-55% of the sum of the mass of the nano-HEU-1 molecular sieve and the binder precursor.
11. The preparation method according to claim 10, wherein: In step (1), the oxidant precursor is pseudo-boehmite; and / or, based on the mass of the corresponding aluminum oxide in the aluminum oxide precursor, the mass ratio of the nano HEU-1 molecular sieve to the binder precursor is 50-80:20-50; and / or, the concentration of the nitric acid is 1-3wt%; And / or, the mass of the nitric acid is 45-50% of the sum of the mass of the nano-HEU-1 molecular sieve and the binder precursor.
12. The preparation method according to claim 11, wherein Based on the mass of the corresponding aluminum oxide in the aluminum oxide precursor, the mass ratio of the nano HEU-1 molecular sieve to the binder precursor is 60-70:30-40.
13. The preparation method according to claim 9, wherein: In step (2), the loading operation method includes: mixing the calcined product with a solution containing a modified element precursor, stirring at 40-90° C. for 1-5 hours, and then drying to obtain a loaded calcined product.
14. The preparation method according to claim 13, wherein: The modifying element precursor is selected from soluble compounds containing the modifying element.
15. The preparation method according to claim 13, wherein: The feeding amounts of the calcined product and the solution containing the modifying element precursor are such that the mass ratio of the nano HEU-1 molecular sieve to the modifying element in the prepared catalyst is 10-90:0.1-10.
16. The preparation method according to claim 15, wherein: The mass ratio of nano HEU-1 molecular sieve to the modified element is 50-80:2-7.
17. The preparation method according to claim 16, wherein: The mass ratio of nano HEU-1 molecular sieve to the modified element is 60-70:2-5.
18. The preparation method according to claim 9, wherein: In step (1), the operating conditions of the first calcination include: the first calcination temperature is 380-600°C, and the first calcination time is 2-10h; In step (2), the operating conditions of the second calcination include: the second calcination temperature is 450-550° C., and the second calcination time is 2-10 hours.
19. The preparation method according to claim 18, wherein: In step (1), the operating conditions of the first calcination include: the first calcination temperature is 400-560°C, and the first calcination time is 4-6h; In step (2), the operating conditions of the second calcination include: the second calcination temperature is 480-520° C., and the second calcination time is 3-6 hours.
20. The preparation method according to claim 9, wherein: In step (3), the operating conditions of the water vapor treatment include: the mass space velocity of the water vapor is 0.2-3h -1 The treatment temperature is 250-400℃ and the treatment time is 4-10h.
21. The preparation method according to claim 20, wherein: In step (3), the operating conditions of the water vapor treatment include: the mass space velocity of the water vapor is 0.5-1.2h -1 , the treatment temperature is 300-380℃, and the treatment time is 6-8h.