A low-temperature, high-efficiency, green method for preparing porous carbon

By using ternary metal carbonate activator for low-temperature ball milling and liquid activation treatment, the problem of low reaction rate of high-temperature activator is solved, the high specific surface area and hierarchical pore structure of porous carbon are achieved, the process is simplified and the energy consumption is reduced. Consumption.

CN116062728BInactive Publication Date: 2024-10-18TIANJIN NORMAL UNIVERSITY
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202111280339.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-30
Publication Date
2024-10-18
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing porous carbon preparation methods, the high-temperature activator solid-phase reaction results in low activation rate and high energy consumption, and a single activator limits the pore size distribution of porous carbon, making it difficult to achieve hierarchical pore characteristics of micropores, mesopores, and macropores. .

Method used

A ternary metal carbonate activator (a mixture of K2CO3, CaCO3 and Na2CO3) is used for ball milling to form a liquid activator at low temperature, which promotes liquid-solid reaction, increases the activation rate, and prepares porous materials through hydrochloric acid soaking and drying steps. carbon.

Benefits of technology

The specific surface area and pore volume of porous carbon are significantly increased at lower temperatures, achieving structural distribution of micropores, mesopores, and macropores, simplifying the process, reducing energy consumption, and avoiding the impact of strong alkaline activators on equipment. corrosion and environmental pollution.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116062728B_ABST
    Figure CN116062728B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing porous carbon at low temperature, high efficiency and greenness. The method comprises the following steps: mixing resin and carbonate activator, ball milling until the mixture is uniform, obtaining a mixed powder, wherein the carbonate activator is a mixture of K2CO3, CaCO3 and Na2CO3, heating the mixed powder to 665-900°C in an inert gas environment and keeping the temperature for 0.5-5h, cooling to room temperature, obtaining a product; soaking the product in hydrochloric acid until the pH is less than 5, filtering, washing to neutrality, drying, and obtaining porous carbon. The invention uses resin as raw material and ternary metal carbonate as carbonate activator to construct porous carbon materials with excellent structural characteristics and chemical states. The porous carbon obtained by the preparation method of the invention has a microporous, mesoporous and macroporous pore structure, a large specific surface area, a large mesoporous volume, a simple preparation process, and cheap and easy-to-obtain raw materials and activators, and is green and friendly to equipment and the environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of porous carbon, and in particular relates to a low-temperature, high-efficiency and green method for preparing porous carbon. Background Art

[0002] Porous carbon (PC) materials are one of the most popular candidates as main framework or activation materials in most energy conversion and storage applications due to their excellent physical and chemical properties and light weight, such as lithium-ion batteries, lithium-sulfur batteries and supercapacitors. The texture characteristics and interface properties of composite materials are the main determinants of their performance, which may vary depending on the mechanism and functional requirements of different electrochemical systems.

[0003] The existing porous carbon preparation methods mostly use template method and chemical / physical activation method. The template method is usually to perform template synthesis by adding templates such as magnesium oxide, calcium oxide, and silicon dioxide to form porous structures such as hollow spheres, nanocages, and York shells. However, the presynthesis process of each template with size and morphology control is mostly complex, energy-intensive, and difficult to scale, which will hinder its widespread application. The chemical / physical activation method generally uses potassium hydroxide, zinc chloride, phosphoric acid, potassium carbonate, sodium carbonate, water vapor, etc. as activators, among which potassium hydroxide is the most commonly used chemical activator and has been industrialized. However, potassium hydroxide activation mainly generates porous carbon with a microporous (pore size <2nm) structure. Potassium hydroxide, as a strong alkaline substance, not only corrodes production equipment, but also has adverse effects on the environment. Based on this, people explore the use of a single carbonate as an activator to prepare porous carbon: For example, the invention patent CN111917651A uses potassium carbonate as an activator, and uses low-order carbon sources such as leaves, lignin, and cellulose as raw materials to prepare porous carbon by high-temperature activation under a nitrogen atmosphere. Although the porous carbon obtained by this method has the advantages of simple preparation process and easy availability of raw materials, the prepared porous carbon has a single pore size, low specific surface area and pore volume, and the activation process requires a high temperature and high energy consumption. In addition, sodium carbonate is also used as a chemical activator for the preparation of porous carbon. For example, the invention patent CN104118861A uses sodium carbonate as an activator and starch cross-linked with epichlorohydrin as a carbon source to obtain porous carbon with a high specific surface area under a nitrogen atmosphere, but the pore size distribution is still dominated by micropores, and there are problems such as high activation temperature, low activation rate, and high energy consumption.

[0004] As is known to all, during the chemical activation of carbon materials, the carbon-containing raw materials will remove water, carbon dioxide and other components at high temperature and become a single carbon material. During this process, the activator reacts chemically with the carbon, so that the carbon material has a porous structure and has certain specific surface area, pore volume and other characteristics. The reactivity of the activator and the carbon material has become one of the important factors affecting the performance of porous carbon. Since the single activator generally has a high melting point (the melting points of commonly used activators are shown in Table 1), the activator is in a solid state during the high temperature (generally ≤850°C) activation process to prepare porous carbon. Therefore, the activation reaction that occurs is a solid-phase (activator)-solid-phase (carbon material) reaction between the solid-phase activator and the solid-phase carbon material, and the low reaction rate of the solid-solid reaction limits the pore-forming effect of the activator. Therefore, in order to obtain higher reaction activity, the general method is to increase the reaction temperature, which causes the problem of high energy consumption. In addition, a single activator generally produces a carbon material with a certain pore size distribution range, which limits the multi-level pore characteristics of porous carbon.

[0005] Table 1

[0006] Activator <![CDATA[K2CO3]]> <![CDATA[CaCO3]]> <![CDATA[NaCO3]]> <![CDATA[(Na 0.82 K 0.18 )2Ca(CO3)2]]> Melting point(℃) 891 1339 851 665

[0007] Therefore, it has become a top priority to use mild activators to achieve higher activation efficiency at lower temperatures and prepare porous carbon with microporous, mesoporous, and macroporous structures to meet the needs of different devices for porous carbon. Summary of the invention

[0008] In view of the deficiencies in the prior art, the present invention provides a low-temperature, high-efficiency and green method for preparing porous carbon.

[0009] The purpose of the present invention is achieved through the following technical solutions.

[0010] A low-temperature, high-efficiency, green method for preparing porous carbon comprises the following steps:

[0011] 1) mixing a resin and a carbonate activator, and ball-milling the mixture until the mixture is uniform to obtain a mixed powder, wherein the carbonate activator is a mixture of K2CO3, CaCO3 and Na2CO3, and the ratio of K2CO3, CaCO3 and Na2CO3 is (28-36): (40-48): (19-28) by weight, and the ratio of the resin to the carbonate activator is 1: (0.5-5) by weight;

[0012] In the step 1), the rotation speed of the ball mill is 250-600 r / min, and the ball milling time is 0.5-5 h.

[0013] 2) heating the mixed powder obtained in step 1) to 665-900° C. in an inert gas environment and maintaining the temperature for 0.5-5 h, then cooling to room temperature to obtain a product;

[0014] In the step 2), the heating rate is 1-10°C / min.

[0015] In the step 2), the heating temperature is 665-850°C.

[0016] 3) The product obtained in step 2) is soaked in hydrochloric acid until the pH is less than 5, filtered, washed to neutrality, and dried to obtain porous carbon.

[0017] In the step 3), the soaking time is 0.5 to 10 hours.

[0018] In the step 3), the concentration of the hydrochloric acid is 0.2-1 mol / L.

[0019] In the step 3), the drying temperature is 80-120°C.

[0020] The porous carbon obtained by the above preparation method.

[0021] In the above technical solution, the specific surface area of ​​the porous carbon is 1700-2800m 2 / g, total pore volume is 1.2~2cm 3 / g, the mesopore volume is 0.3~0.55cm 3 / g.

[0022] The above preparation method uses resin as raw material and ternary metal carbonate as carbonate activator, and invents a ternary eutectic activation strategy for constructing porous carbon materials with excellent structural characteristics and chemical states. The porous carbon described in the present invention has a pore structure of micropores (pore size <2nm), mesopores (2-50nm), and macropores (>50nm), a large specific surface area, a large mesopore volume, a simple preparation process, and cheap and easy-to-obtain raw materials and activators, and is green and friendly to equipment and the environment.

[0023] The present invention has the following advantages:

[0024] (1) The above preparation method uses a specific ratio of potassium, calcium and sodium carbonates (i.e., KC / CC / NC) to form a liquid ternary metal carbonate activator (Na) with a lower melting point (665°C) under heating. 0.82 K 0.18 )2Ca(CO3)2 can convert the solid phase (single activator)-solid phase (carbon material) reaction in the process of activating carbon materials with a single activator into a liquid phase (ternary metal carbonate)-solid phase (carbon material) reaction at a relatively low temperature, which greatly improves the activation rate, accelerates the activation process, and greatly improves the specific surface area and pore volume of porous carbon.

[0025] (2) Since the components of the carbonate activator in the above preparation method are all neutral carbonates, the reaction environment is mild and environmentally friendly, and the corrosion of the production equipment by the strong alkaline activator is avoided.

[0026] (3) The above-mentioned preparation method realizes the preparation of porous carbon under relatively low temperature and neutral environment, which can avoid the loss of elements such as N, S, and P in carbon-containing raw materials under high temperature, so that the prepared porous carbon contains more heteroatoms, which is conducive to the regulation of porous carbon elements, thereby expanding its application field. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 It is a schematic diagram of the implementation principle of the preparation method of the present invention;

[0028] Figure 2 This is a performance comparison diagram of the porous carbon of Example 1 of the present invention and the porous carbon prepared by using a single carbonate as an activating agent reported in the literature (as shown in Table 2);

[0029] Figure 3 This is a SEM image of the porous carbon obtained in Example 1 of the present invention;

[0030] Figure 4 This is a SEM image of the porous carbon obtained in Example 2 of the present invention;

[0031] Figure 5 This is the EDS spectrum of the porous carbon obtained in Example 2 of the present invention;

[0032] Figure 6 Isothermal adsorption curves of the porous carbon obtained in Example 2 of the present invention and the porous carbon obtained in Comparative Examples 1, 2, and 3;

[0033] Figure 7 The pore size distribution diagram of the porous carbon obtained in Example 2 of the present invention and the porous carbon obtained in Comparative Examples 1, 2, and 3;

[0034] Figure 8 This is the XRD pattern of the porous carbon obtained in Example 2 of the present invention;

[0035] Fig. 9 This is a SEM image of the porous carbon obtained in Example 3 of the present invention;

[0036] Fig.10 This is the Raman image of the porous carbon obtained in Example 3 of the present invention. DETAILED DESCRIPTION

[0037] The reaction principle diagram of the preparation method of the present invention is as follows Figure 1As shown, the resin and the ternary carbonate activator are first mixed evenly. In the subsequent high-temperature activation process, the ternary carbonate activator will form a carbonate with a low melting point, which can be converted into a liquid at a relatively low temperature of 665°C. Therefore, during the high-temperature activation process, the liquid carbonate activator reacts with the solid carbon material in a liquid-solid reaction, making its activation rate much higher than the solid-solid reaction of a single carbonate, thereby greatly improving the activation efficiency and efficiently preparing porous carbon at a relatively low temperature.

[0038] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0039] Example 1

[0040] A low-temperature, high-efficiency, green method for preparing porous carbon comprises the following steps:

[0041] 1) Mixing the resin and the carbonate activator, ball milling at a speed of 500 r / min for 3 h until the mixture is uniform, to obtain a mixed powder, wherein the carbonate activator is a mixture of K2CO3, CaCO3 and Na2CO3, the ratio of K2CO3, CaCO3 and Na2CO3 is 32:44.5:23.5 by mass, and the ratio of the resin to the carbonate activator is 1:1 by mass;

[0042] 2) heating the mixed powder obtained in step 1) to 800° C. at a heating rate of 2° C. / min in a nitrogen environment and keeping the temperature at this temperature for 2 h, then cooling the mixture to room temperature (20-25° C.) to obtain a product;

[0043] 3) The product obtained in step 2) was soaked in 1 mol / L hydrochloric acid for 10 h until the pH was less than 5, filtered, washed with deionized water until neutral, and dried at 120° C. for 12 h to obtain porous carbon.

[0044] like Figure 3 The SEM of the porous carbon prepared in this example is shown. The SEM analysis results show that the porous carbon obtained in Example 1 has a three-dimensional porous structure with interconnected micropores, mesopores and macropores. After testing, the specific surface area of ​​the porous carbon obtained in Example 1 is 2286 m 2 / g, with a total pore volume of 1.61 cm 3 / g, of which the mesopore volume is 0.53cm 3 / g.

[0045] Example 2

[0046] A low-temperature, high-efficiency, green method for preparing porous carbon comprises the following steps:

[0047] 1) Mixing the resin and the carbonate activator, ball milling at a speed of 500 r / min for 3 h until the mixture is uniform, to obtain a mixed powder, wherein the carbonate activator is a mixture of K2CO3, CaCO3 and Na2CO3, the ratio of K2CO3, CaCO3 and Na2CO3 is 32:44.5:23.5 by mass, and the ratio of the resin to the carbonate activator is 1:1 by mass;

[0048] 2) heating the mixed powder obtained in step 1) to 800° C. at a heating rate of 2° C. / min in a nitrogen environment and keeping the temperature at this temperature for 0.5 h, and then cooling the mixture to room temperature (20-25° C.) to obtain a product;

[0049] 3) The product obtained in step 2) was soaked in 1 mol / L hydrochloric acid for 10 h until the pH was less than 5, filtered, washed with deionized water until neutral, and dried at 120° C. for 12 h to obtain porous carbon.

[0050] The porous carbon SEM ( Figure 4 ) The analysis results show that the porous carbon obtained in Example 2 has an obvious nanosheet structure. EDS ( Figure 5 ) The test results show that the C, N, and O elements in the porous carbon obtained in Example 2 are evenly distributed. The BET test results ( Figure 6 , 7 ) shows that the specific surface area of ​​the porous carbon obtained in Example 2 is 1906 m 2 / g, with a total pore volume of 1.22 cm 3 / g, of which the mesopore volume is 0.36cm 3 / g, which is superior to the porous carbon prepared by single carbonate activator in terms of specific surface area and total pore volume. Figure 7 It can be seen that the pore size distribution of the porous carbon prepared by using the ternary carbonate activator in Example 2 includes not only micropores (≤2nm) but also a large number of mesopores distributed in the range of 2 to 6nm; while the porous carbon prepared by using a single carbonate activator (such as the following comparative examples 1 to 3) has a main pore size distribution of micropores (≤2nm). Therefore, the use of the carbonate activator of the present invention can broaden the pore size distribution of the porous carbon, which is conducive to the preparation of a multi-level pore structure. XRD test results ( Figure 8 ) shows that the degree of graphitization of the porous carbon obtained in Example 2 is high enough.

[0051] Example 3

[0052] A low-temperature, high-efficiency, green method for preparing porous carbon comprises the following steps:

[0053] 1) Mixing the resin and the carbonate activator, ball milling at a speed of 500 r / min for 3 h until the mixture is uniform, to obtain a mixed powder, wherein the carbonate activator is a mixture of K2CO3, CaCO3 and Na2CO3, the ratio of K2CO3, CaCO3 and Na2CO3 is 32:44.5:23.5 by mass, and the ratio of the resin to the carbonate activator is 1:1 by mass;

[0054] 2) heating the mixed powder obtained in step 1) to 800° C. at a heating rate of 2° C. / min in a nitrogen environment and keeping the temperature at this temperature for 5 hours, then cooling the temperature to room temperature (20-25° C.) to obtain a product;

[0055] 3) The product obtained in step 2) was soaked in 1 mol / L hydrochloric acid for 10 h until the pH was less than 5, filtered, washed with deionized water until neutral, and dried at 120° C. for 12 h to obtain porous carbon.

[0056] The porous carbon SEM ( Fig. 9 ) analysis results show that the porous carbon obtained in Example 3 has a graphite sheet structure, Raman ( Fig.10 ) The test analysis shows that the porous carbon obtained in Example 3 has a multilayer graphene structure. The BET test results of this example show that the specific surface area of ​​the porous carbon obtained in Example 3 is 2732m 2 / g, with a total pore volume of 1.75 cm 3 / g, of which the mesopore volume is 0.51cm 3 / g.

[0057] Example 4

[0058] A low-temperature, high-efficiency, green method for preparing porous carbon comprises the following steps:

[0059] 1) mixing the resin and the carbonate activator, and ball milling them at a speed of 500 r / min for 3 h until the mixture is uniform, to obtain a mixed powder, wherein the carbonate activator is a mixture of K2CO3, CaCO3 and Na2CO3, and the ratio of K2CO3, CaCO3 and Na2CO3 is 30:48:22 by weight, and the ratio of the resin to the carbonate activator is 1:1 by weight;

[0060] 2) heating the mixed powder obtained in step 1) to 900° C. at a heating rate of 2° C. / min in a nitrogen environment and keeping the temperature at this temperature for 0.5 h, and then cooling the mixture to room temperature (20-25° C.) to obtain a product;

[0061] 3) The product obtained in step 2) was soaked in 1 mol / L hydrochloric acid for 10 h until the pH was less than 5, filtered, washed with deionized water until neutral, and dried at 120° C. for 12 h to obtain porous carbon.

[0062] The BET test results of this example show that the specific surface area of ​​the porous carbon obtained in Example 4 is 2675 m 2 / g, with a total pore volume of 1.63 cm 3 / g, of which the mesopore volume is 0.45cm 3 / g.

[0063] Example 5

[0064] A low-temperature, high-efficiency, green method for preparing porous carbon comprises the following steps:

[0065] 1) Mixing the resin and the carbonate activator, ball milling at a speed of 500 r / min for 3 h until the mixture is uniform, to obtain a mixed powder, wherein the carbonate activator is a mixture of K2CO3, CaCO3 and Na2CO3, the ratio of K2CO3, CaCO3 and Na2CO3 is 32:44.5:23.5 by mass, and the ratio of the resin to the carbonate activator is 1:1 by mass;

[0066] 2) heating the mixed powder obtained in step 1) to 665° C. at a heating rate of 2° C. / min in a nitrogen environment and keeping the temperature at this temperature for 2 h, then cooling the temperature to room temperature (20-25° C.) to obtain a product;

[0067] 3) The product obtained in step 2) was soaked in 1 mol / L hydrochloric acid for 10 h until the pH was less than 5, filtered, washed with deionized water until neutral, and dried at 120° C. for 12 h to obtain porous carbon.

[0068] The BET test results of this example show that the specific surface area of ​​the porous carbon obtained in Example 5 is 1938 m 2 / g, with a total pore volume of 1.51 cm 3 / g, of which the mesopore volume is 0.44cm 3 / g.

[0069] Example 6

[0070] A low-temperature, high-efficiency, green method for preparing porous carbon comprises the following steps:

[0071] 1) Mixing the resin and the carbonate activator, ball milling at a speed of 500 r / min for 3 h until the mixture is uniform, to obtain a mixed powder, wherein the carbonate activator is a mixture of K2CO3, CaCO3 and Na2CO3, the ratio of K2CO3, CaCO3 and Na2CO3 is 28:44:28 by mass, and the ratio of the resin to the carbonate activator is 1:0.5 by mass;

[0072] 2) heating the mixed powder obtained in step 1) to 700° C. at a heating rate of 2° C. / min in a nitrogen environment and keeping the temperature at this temperature for 2 h, then cooling the mixture to room temperature (20-25° C.) to obtain a product;

[0073] 3) The product obtained in step 2) was soaked in 1 mol / L hydrochloric acid for 10 h until the pH was less than 5, filtered, washed with deionized water until neutral, and dried at 120° C. for 12 h to obtain porous carbon.

[0074] The BET test results of this example show that the specific surface area of ​​the porous carbon obtained in Example 7 is 1705 m 2 / g, with a total pore volume of 1.43 cm 3 / g, of which the mesopore volume is 0.42cm 3 / g.

[0075] Example 7

[0076] A low-temperature, high-efficiency, green method for preparing porous carbon comprises the following steps:

[0077] 1) Mixing the resin and the carbonate activator, ball milling at a speed of 500 r / min for 3 h until the mixture is uniform, to obtain a mixed powder, wherein the carbonate activator is a mixture of K2CO3, CaCO3 and Na2CO3, the ratio of K2CO3, CaCO3 and Na2CO3 is 32:46:22 by mass, and the ratio of the resin to the carbonate activator is 1:4 by mass;

[0078] 2) heating the mixed powder obtained in step 1) to 700° C. at a heating rate of 2° C. / min in a nitrogen environment and keeping the temperature at this temperature for 2 h, then cooling the mixture to room temperature (20-25° C.) to obtain a product;

[0079] 3) The product obtained in step 2) was soaked in 1 mol / L hydrochloric acid for 10 h until the pH was less than 5, filtered, washed with deionized water until neutral, and dried at 120° C. for 12 h to obtain porous carbon.

[0080] The BET test results of this example show that the specific surface area of ​​the porous carbon obtained in Example 7 is 2412 m 2 / g, with a total pore volume of 1.92 cm 3 / g, of which the mesopore volume is 0.54cm 3 / g.

[0081] The results of the porous carbon obtained in Examples 1-7 are shown in Table 2:

[0082] Table 2

[0083]

[0084] From the BET test results in Table 2, it can be seen that the porous carbon obtained by using carbonate activator has the advantage of rich mesopores. By regulating the heat treatment temperature, the structure of porous carbon such as pore size and specific surface area can be further optimized. By regulating the insulation time, the pore volume and specific surface area of ​​porous carbon can also be optimized to a certain extent.

[0085] Comparative Example 1

[0086] A method for preparing porous carbon comprises the following steps:

[0087] 1) 10 g of resin and 10 g of K2CO3 as an activator were mixed by ball milling at 500 r / min for 3 h, wherein the ratio of resin to K2CO3 was 1:1 by mass;

[0088] 2) heating the mixture obtained in step 1) to 800° C. at a heating rate of 2° C. / min in a nitrogen atmosphere and keeping the temperature at this temperature for 2 h, then cooling to room temperature to obtain a product;

[0089] 3) Soak the product obtained in step 2) in 1 mol / L hydrochloric acid for 10 h until the pH is less than 5, filter, wash until neutral, and dry at 120°C.

[0090] The BET test results show that the specific surface area of ​​the porous carbon obtained in Comparative Example 1 is 925 m 2 / g, with a total pore volume of 0.58 cm 3 / g, of which the mesopore volume is 0.03cm 3 / g.

[0091] Comparative Example 2

[0092] This comparative example is basically the same as comparative example 1, except that K2CO3 in comparative example 1 is replaced by CaCO3. The BET test results show that the specific surface area of ​​the porous carbon obtained in comparative example 2 is 165 m 2 / g, with a total pore volume of 0.17 cm 3 / g, of which the mesopore volume is 0.01cm 3 / g.

[0093] Comparative Example 3

[0094] This comparative example is basically the same as comparative example 1, except that K2CO3 in comparative example 1 is replaced by Na2CO3. The BET test results show that the specific surface area of ​​the porous carbon obtained in comparative example 3 is 558 m 2 / g, with a total pore volume of 0.48 cm 3 / g, of which the mesopore volume is 0.04cm 3 / g.

[0095] Comparative Example 4

[0096] This comparative example is basically the same as comparative example 1, except that K2CO3 in comparative example 1 is replaced by a mixture of K2CO3 and Na2CO3, wherein the ratio of K2CO3 to Na2CO3 is 1:1 by mass. The BET test results show that the specific surface area of ​​the porous carbon obtained in comparative example 4 is 1268 m 2 / g, the total pore volume is 0.86m 3 / g, of which the mesopore volume is 0.23cm 3 / g.

[0097] Comparative Example 5

[0098] This comparative example is basically the same as comparative example 1, except that K2CO3 in comparative example 1 is replaced by a mixture of CaCO3 and Na2CO3, wherein the ratio of CaCO3 to Na2CO3 is 1:1 by mass. The BET test results show that the specific surface area of ​​the porous carbon obtained in comparative example 5 is 908 m 2 / g, with a total pore volume of 0.62 cm 3 / g, of which the mesopore volume is 0.09cm 3 / g.

[0099] The test results of the porous carbon obtained in Comparative Examples 1-5 are shown in Table 3:

[0100] Table 3

[0101]

[0102] From the comparison of the BET test results in Table 3 with those in Table 2, it can be seen that the porous carbon prepared using a ternary metal carbonate activator is superior to the porous carbon prepared using a single carbonate activator or a two-phase carbonate activator in terms of specific surface area and pore volume, and has the advantage of rich mesopore volume.

[0103] The porous carbon obtained in Example 1 was compared with the data in references S1 to S13. The comparison results are as follows: Figure 2 As shown, the specific surface area of ​​the porous carbon obtained in Example 1 is 2286 m 2 / g, and the total pore volume is 1.61cm 3 / g, the specific surface area and total pore volume are better than those of the porous carbon prepared in the literature listed in Table 4.

[0104] Table 4

[0105]

[0106]

[0107] The documents represented by the above document codes are as follows:

[0108] S1.Liang,Y.;Dong,H.;Aurbach,D.;Yao,Y.,Nature Energy 2020,5,646-656.DOI 10.1038 / s41560-020-0655-0.

[0109] S2.Ji,H.;Wu,J.;Cai,Z.;Liu,J.;Kwon,D.-H.;Kim,H.;Urban,A.;Papp,JK;Foley,E.;Tian ,Y.;Balasubramanian,M.;Kim,H.;Clement,RJ;McCloskey,BD;Yang,W.;Ceder,G.,Nature Energy 2020,5(3),213-221.DOI 10.1038 / s41560-020-0573-1.

[0110] S3.Liu,J.;Bao,Z.;Cui,Y.;Dufek,EJ;Goodenough,JB;Khalifah,P.;Li,Q.;Liaw,BY;Liu,P.;Manthiram,A.;Meng,YS. amanian,VR;Toney,MF;Viswanathan,VV;Whittingham,MS;Xiao,J.;Xu,W.;Yang,J.;Yang,X.-Q.;Zhang,J.-G.,Nat.Energy 2019,4(3),180-186.DOI 10.1038 / s41560-019-0338-x.

[0111] S4.Mao,W.;Yue,W.;Xu,Z.;Wang,J.;Zhang,J.;Li,D.;Zhang,B.;Yang,S.;Dai,K.;Liu,G.;Ai,G.,ACS Appl.Mater. 2020,12(35),39282-39292.DOI10.1021 / acsami.0c11282.

[0112] S5.Zhu,Y.;Simon,P.;Ye,J.,National Science Review 2020,7(1),191-201.DOI 10.1093 / nsr / nwz140.

[0113] S6.Geng,H.;Peng,Y.;Qu,L.;Zhang,H.;Wu,M.,Adv.Energy Mater.2020,10(10),1903030.DOI 10.1002 / aenm.201903030.

[0114] S7. Hong, Y.; Mao, W.; Hu, Q.; Chang, S.; Li, D.; Zhang, J.; Liu, G.; Ai, G., J. PowerSources 2019, 428, 44-52. DOI https: / / doi.org / 10.1016 / j.jpowsour.2019.04.093.

[0115] S8. Luo, J.-D.; Zhang, H.; Qi,

[0116] S9. Ai, G.; Hu, Q.; Zhang, L.; Dai, K.; Wang, J.; Xu, Z.; Huang, Y.; Zhang, B.; Li, D.; Zhang, T.; Liu, G.; Mao, W., ACS Appl. Mater. Interfaces 2019, 11(37), 33987-33999. DOI10.1021 / acsami.9b11561.

[0117] S10. Mao, W.; Yue, W.; Xu, Z.; Chang, S.; Hu, Q.; Pei, F.; Huang, X.; Zhang, J.; Li, D.; Liu, G.; Ai, G., ACS Nano 2020, 14(4), 4741-4754. DOI 10.1021 / acsnano.0c00620.

[0118] S11. Yu, Z.; Liu, M.; Guo, D.; Wang, J.; Chen, X.; Li, J.; Jin, H.; Yang, Z.; Chen, Xa; 10.1002 / anie.201914972.

[0119] S12.Yin,J.;Zhang,W.;Alhebshi,NA;Salah,N.;Alshareef,HN,SmallMethods 2020,4(3),1900853.DOI 10.1002 / smtd.201900853.

[0120] S13. He, Y.; Zhuang, X.; Lei, C.; Lei, L.; Hou, Y.; Mai, Y.; Feng, X., Nano Today 2019, 24, 103-119. DOI 10.1016 / j.nantod.2018.12.004.

[0121] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.

Claims

1. A low-temperature, high-efficiency, green method for preparing porous carbon, characterized in that: The following steps are involved: 1) mixing a resin and a carbonate activator, and ball-milling the mixture until the mixture is uniformly mixed to obtain a mixed powder, wherein the carbonate activator is a mixture of K2CO3, CaCO3 and Na2CO3, and the ratio of K2CO3, CaCO3 and Na2CO3 is (28-36): (40-48): (19-28) by weight, and the ratio of the resin to the carbonate activator is 1: (0.5-5) by weight; 2) heating the mixed powder obtained in step 1) to 665-900° C. in an inert gas environment and maintaining the temperature for 0.5-5 h, then cooling to room temperature to obtain a product; 3) soaking the product obtained in step 2) in hydrochloric acid until the pH is less than 5, filtering, washing to neutrality, and drying to obtain porous carbon; In the step 1), the rotation speed of the ball mill is 250-600 r / min, and the ball milling time is 0.5-5 h.

2. The preparation method according to claim 1, characterized in that: In the step 2), the heating rate is 1-10°C / min.

3. The preparation method according to claim 1 or 2, characterized in that: In the step 2), the heating temperature is 665-850°C.

4. The preparation method according to claim 1, characterized in that: In the step 3), the soaking time is 0.5 to 10 hours.

5. The preparation method according to claim 1, characterized in that: In the step 3), the concentration of the hydrochloric acid is 0.2-1 mol / L.

6. The preparation method according to claim 1, characterized in that: In the step 3), the drying temperature is 80-120°C.

7. Porous carbon obtained by the preparation method according to any one of claims 1 to 6.

8. The porous carbon according to claim 7, characterized in that The porous carbon has a specific surface area of ​​1700 to 2800 m2 / g, a total pore volume of 1.2 to 2 cm3 / g, and a mesopore volume of 0.3 to 0.55 cm3 / g.

Citation Information

Patent Citations

  • Preparation method of multilevel porous carbon with ultrahigh specific surface area

    CN104118861A

  • Multicast forwarding method and system for cross chip

    CN111917651A

  • Preparation method of biomass-based porous carbon and product

    CN109879281A

  • Method for preparing graphitized hierarchical porous carbon

    CN110436459A

  • Method for preparing electrical double-layer capacitor active carbon by using template method

    CN110683541A