A modified ZSM-23 molecular sieve and its preparation method and application

The dealuminized silicon and water vapor treatment method of the template agent ZSM-23 molecular sieve without removing the template agent ZSM-23 has solved the problems of low acid modification efficiency and channel blockage, and achieved a catalytic effect with high selectivity and high conversion.

CN116062771BActive Publication Date: 2024-12-06CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202111269813.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2021-10-29
Publication Date
2024-12-06
Estimated Expiration
2041-10-29

AI Technical Summary

Technical Problem

The prior art has problems of low efficiency, uneven adhesion dispersion and blockage of pores in the acidic modification process of the outer surface of the modified ZSM-23 molecular sieve, which affects the catalytic performance.

Method used

The ZSM-23 molecular sieve with the unremoved template agent is mixed with the dealuminized silicon reagent, and the template agent in the acidic center and pores of the outer surface are removed at a certain point to form a suitable modification of the SiO2/Al2O3 molar ratio. , retaining the openness of the pores.

Benefits of technology

The selectivity of isomer hydrocarbons is significantly improved, while maintaining high normal alkane conversion, reducing non-selective cracking reactions, and enhancing the performance of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116062771B_ABST
    Figure CN116062771B_ABST
Patent Text Reader

Abstract

The present invention provides a modified ZSM-23 molecular sieve and a preparation method and application thereof. The outer surface SiO 2 / Al 2 O 3 The molar ratio is 500-1500, the bulk SiO 2 / Al 2 O 3 The molar ratio is 60-200, the total IR acid content of pyridine is 0.02-0.35 mmol / g, and the total IR acid content of di-tert-butylpyridine is 0.001-0.015 mmol / g. The catalyst prepared by the modified ZSM-23 molecular sieve is used for the isomerization reaction of normal alkanes, which can significantly improve the selectivity of isoalkanes while ensuring a high conversion rate of normal alkanes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of molecular sieves and preparation thereof, and in particular to a modified ZSM-23 molecular sieve and a preparation method thereof. Background Art

[0002] In 1978, Plank et al. of Mobile Company used pyrrolidine as template and hydrothermal synthesis to synthesize a medium-pore high-silicon zeolite molecular sieve named ZSM-23, with MTT topological structure. ZSM-23 molecular sieve has a one-dimensional ten-membered ring straight pore structure with a pore size of 0.45×0.52nm. Its unique pore structure and acid properties make it show high catalytic activity and selectivity in the isomerization reaction of normal alkanes.

[0003] The isomerization reaction of normal alkanes catalyzed by molecular sieves follows the pore-mouth mechanism and the lock-key mechanism. However, since there are some acidic centers on the outer surface of the molecular sieve that do not have shape-selective isomerization catalytic properties, they are prone to cause side reactions such as cracking. Therefore, modifying the outer surface of the molecular sieve to reduce the acidity of the outer surface while retaining the acidity in the pores is of great significance for improving the selectivity of the isomerization reaction.

[0004] CN102794193A discloses a method for modifying the outer surface of a microporous molecular sieve. The method comprises mixing silica sol with a microporous molecular sieve, physically adsorbing the molecular sieve and silica sol by liquid phase deposition, attaching colloidal ions of silica sol to the outer surface of the molecular sieve, and then filtering, drying, and calcining to prepare a molecular sieve with reduced acidity on the outer surface. However, due to the low interaction between the surface of the molecular sieve and the attached material, this silanization method requires repeated multiple cycles of impregnation to achieve the purpose of eliminating the acidity of the outer surface, resulting in a large amount of waste of silicone esters and greatly reducing the efficiency of the modification process.

[0005] CN109529923A discloses a method for preparing an oxide-modified microporous molecular sieve shape-selective catalyst. The method is to add a microporous molecular sieve from which the template agent has not been removed into a metal nitrate solution, stir evenly, and then filter, dry, and roast to obtain a metal oxide-modified microporous molecular sieve shape-selective catalyst. However, although this method of nitride or metal oxide modification can better cover the acidity of the outer surface of the molecular sieve, the dispersion degree of the attached matter is uneven during the modification process, which easily leads to blockage of the molecular sieve pores and affects the catalytic performance of the molecular sieve. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention provides a modified ZSM-23 molecular sieve and a preparation method and application thereof. The catalyst prepared by the modified ZSM-23 molecular sieve is used in the isomerization reaction of normal alkanes, which can significantly improve the selectivity of isoalkanes while ensuring a high conversion rate of normal alkanes.

[0007] The first aspect of the present invention provides a modified ZSM-23 molecular sieve, wherein the outer surface SiO2 / Al2O3 molar ratio of the modified ZSM-23 molecular sieve is 500-1500, the bulk SiO2 / Al2O3 molar ratio is 60-200, the total infrared acid content of pyridine is 0.02-0.35 mmol / g, and the total infrared acid content of di-tert-butylpyridine is 0.001-0.015 mmol / g.

[0008] Furthermore, preferably, the outer surface SiO2 / Al2O3 molar ratio of the modified ZSM-23 molecular sieve is 600-1000, and the bulk SiO2 / Al2O3 molar ratio is 80-150.

[0009] Further, preferably, the total IR acid content of pyridine in the modified ZSM-23 molecular sieve is 0.10 to 0.25 mmol / g, and the total IR acid content of di-tert-butylpyridine is 0.005 to 0.012 mmol / g.

[0010] The second aspect of the present invention provides a method for preparing a modified ZSM-23 molecular sieve, comprising the following steps:

[0011] (1) preparing a ZSM-23 molecular sieve without removing the template;

[0012] (2) mixing the ZSM-23 molecular sieve obtained in step (1) with a dealumination and siliconization agent to carry out dealumination and siliconization;

[0013] (3) treating the material obtained in step (2) with water vapor;

[0014] (4) treating the material obtained in step (3) with a buffer solution to obtain a modified ZSM-23 molecular sieve.

[0015] Furthermore, in step (1), the ZSM-23 molecular sieve without removing the template can be prepared by hydrothermal synthesis. For example, silicon source, aluminum source, template, alkali source and water are added in the following molar ratios: SiO2: (0.003-0.02) Al2O3: (0.4-2.0) R (template): (0.01-10) Na2O: (10-200) H2O, the mixed materials are crystallized at 150-180°C for 2-5 days, the product is washed to a pH value of 7-8, and then filtered and dried at 80-120°C to obtain the ZSM-23 molecular sieve without removing the template.

[0016] Furthermore, in the preparation process of the ZSM-23 molecular sieve, the silicon source is selected from one or more of silica sol, white carbon black, tetraethyl orthosilicate, etc., the aluminum source is selected from one or more of aluminum sulfate 18hydrate, pseudo-boehmite, sodium aluminate, etc., the template agent is selected from one or more of isopropylamine, dimethylamine, pyrrolidine, the alkali source is selected from one or more of sodium hydroxide, potassium hydroxide, etc., and the water is deionized water.

[0017] Furthermore, in step (2), the dealumination and siliconization reagent is at least one of ammonium hexafluorosilicate solution, ethyl orthosilicate solution, and the like.

[0018] Furthermore, in step (2), the molar concentration of the dealumination and siliconization reagent is 0.5 to 1.5 mol / L. The mass ratio of the ZSM-23 molecular sieve obtained in step (1) to the dealumination and siliconization reagent is 1:2 to 1:8.

[0019] Furthermore, in step (2), the specific operation process of dealumination and siliconization is as follows: the ZSM-23 molecular sieve obtained in step (1) is mixed with water, then heated to 60-100°C, and stirred continuously, and the dealumination and siliconization reagent is added dropwise, and stirring is continued for 60-120 minutes after the addition is completed, and the filter cake is filtered while hot, and the filter cake is washed with water, filtered again and dried. The liquid-to-solid volume ratio of water to the ZSM-23 molecular sieve obtained in step (1) is 2:1-8:1.

[0020] Furthermore, in step (3), the conditions for the water vapor treatment are: temperature of 400-700° C., preferably 500-600° C., pressure of 0.01-0.3 MPa, preferably 0.1-0.2 MPa, time of 0.5-6 h, preferably 1-4 h.

[0021] Furthermore, in step (4), the buffer solution is one or more of oxalic acid-ammonium oxalate solution and acetic acid-ammonium acetate solution. The pH value of the buffer solution is 4.5 to 6.5, preferably 5.0 to 6.0. In the buffer solution, the molar concentration of organic acid radicals is 0.1 to 1.0 mol / L. The liquid-to-solid volume ratio of the buffer solution to the material obtained in step (3) is 3:1 to 10:1.

[0022] Furthermore, in step (4), the specific treatment process is: mixing and stirring the material obtained in step (3) with a buffer solution, the treatment temperature is 40 to 80° C., and the treatment time is 0.5 to 3 hours.

[0023] Furthermore, in step (4), solid-liquid separation (such as suction filtration) is performed; and the above operation is repeated 2 to 4 times, and the final material is dried to obtain the modified ZSM-23 molecular sieve.

[0024] The third aspect of the present invention provides an application of the modified ZSM-23 molecular sieve in a catalyst for the shape-selective isomerization of normal alkanes.

[0025] Furthermore, the normal alkane isomerization catalyst comprises the modified ZSM-23 molecular sieve and a Group VIII noble metal component, wherein the Group VIII noble metal component has a content of 0.01% to 10%, preferably 0.1% to 3%, based on the weight of the metal.

[0026] Furthermore, the Group VIII noble metal is platinum and / or palladium.

[0027] Furthermore, the normal alkane includes at least one of n-dodecane, n-tetradecane, n-hexadecane, n-octadecane and the like.

[0028] Compared with the prior art, the present invention has the following advantages:

[0029] 1. The modified ZSM-23 molecular sieve of the present invention has a low total infrared acid content of di-tert-butylpyridine, eliminates the acid sites on the outer surface and has an open and unobstructed pore structure. The catalyst prepared by the modified ZSM-23 molecular sieve of the present invention significantly improves the selectivity of isoalkanes while ensuring a high conversion rate of normal alkanes.

[0030] 2. The preparation method of the modified ZSM-23 molecular sieve of the present invention is as follows: first, the molecular sieve obtained by hydrothermal synthesis is not treated with a de-template agent, and the organic template agent molecules in the pores act as pore protectors. The acidic centers on the outer surface of the molecular sieve are removed by a dealuminizing and siliconizing method, thereby reducing the non-selective cracking reaction of normal alkanes on the outer surface of the molecular sieve. The aluminum on the outer surface of the molecular sieve is replaced by non-acidic silicon atoms under the action of the dealuminizing and siliconizing agent. Due to the presence of the template agent molecules, the acidic centers in the pores are protected. Subsequently, a constant pressure and high temperature steam treatment method is used to reduce the total acid content of the molecular sieve, and the template agent molecules in the pores are also removed. Finally, a buffer solution is used to remove the non-framework aluminum generated during the hydrothermal treatment, so that the pores of the molecular sieve are more open and unobstructed, which is easy for the diffusion of intermediate products in the shape-selective isomerization reaction of normal alkanes. The catalyst prepared by the modified ZSM-23 of the present invention significantly improves the selectivity of isoalkanes while ensuring a high conversion rate of normal alkanes. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 This is the XRD pattern of the modified molecular sieve obtained in Example 1. DETAILED DESCRIPTION

[0032] The functions and effects of the technical solution of the present invention are further illustrated below in conjunction with embodiments and comparative examples, but the following embodiments do not constitute a limitation on the protection scope of the present invention.

[0033] In the present invention, % involved in the embodiments and comparative examples are all mass fractions unless otherwise specified.

[0034] In the present invention, the outer surface SiO2 / Al2O3 molar ratio is measured by X-ray photoelectron spectroscopy (XPS), and the element composition and state of the catalyst surface are measured on a Multilab2000 electron spectrometer of Thermofisher Company of the United States, the excitation source is Mg Kα, and the cathode voltage and current are 13kV and 20mA respectively. The electron binding energy is calibrated by C1s (284.6eV).

[0035] In the present invention, the bulk SiO2 / Al2O3 molar ratio is obtained by X-ray fluorescence spectroscopy (XRF) analysis using a ZSX100e X-ray fluorescence spectrometer, with a Kα spectral line, Li F1 crystal, Rh target, SC scintillation detector, 20s timing, and a vacuum optical path atmosphere.

[0036] In the present invention, the pyridine infrared determination method is as follows: the powdered ZSM-23 molecular sieve is pressed into tablets, vacuumed, and then degassed at 450° C. for 2 hours. When the temperature drops to room temperature, the pyridine molecule is used as a probe molecule to measure the infrared spectrum of chemical desorption and calculate the adsorption amount.

[0037] In the present invention, the total infrared acid amount of di-tert-butylpyridine refers to the kinetic diameter of The 2,6-di-tert-butylpyridine molecule can contact the proton acid. The infrared determination method of 2,6-di-tert-butylpyridine is as follows: the powdered ZSM-23 molecular sieve is pressed into a tablet, evacuated, and degassed at 450°C for 2 hours. When the temperature drops to room temperature, the 2,6-di-tert-butylpyridine molecule is used as a probe molecule to measure its infrared spectrum of chemical desorption and calculate the adsorption amount.

[0038] Example 1

[0039] 8g of sodium hydroxide was weighed and dissolved in 810mL of water. During the stirring process, 6.66g of aluminum sulfate 18hydrate, 150g of silica sol (mass fraction of 40%), and 35.4g of isopropylamine (iPA) were added in sequence to form a mixed gel with a material molar ratio of SiO2: 0.01Al2O3: 0.6iPA: 0.1Na2O: 50H2O. The mixed initial gel was placed in a closed reactor and crystallized at 160°C for 3 days. The obtained mixture product was washed to a pH value of 7, and then filtered and dried at 120°C to obtain ZSM-23 powder without removing the template agent. 30g of the above ZSM-23 powder was taken, 180mL of water was added and mixed evenly, stirred and heated to 60°C, and 90mL of 0.5mol / L ammonium hexafluorosilicate solution was added dropwise at a uniform rate using a peristaltic pump. The temperature was maintained at 60°C and stirred continuously for 90min. Filter while hot, add 240mL of water to the filter cake, heat to 60℃ and keep for 20min, filter while hot, dry the filter cake at 120℃ for 24h, then place the dried product in a hydrothermal treatment furnace, treat at 500℃, 0.1MPa pressure for 2h, place the obtained material in 300mL of oxalic acid-ammonium oxalate solution with a pH value of 6.0, in which the molar concentration of oxalate is 0.3mol / L, stir and heat to 60℃, keep for 30min and filter while hot, repeat this process 3 times, dry the filter cake at 120℃ for 24h, and the modified molecular sieve is named ZSM-23-1. The XRD pattern of the modified molecular sieve is shown in Figure 1 .

[0040] Example 2

[0041] 8g of sodium hydroxide was weighed and dissolved in 810mL of water. During the stirring process, 6.66g of aluminum sulfate 18hydrate, 150g of silica sol (mass fraction of 40%) and 35.4g of isopropylamine were added in sequence to form a mixed gel with a material molar ratio of SiO2: 0.01Al2O3: 0.6iPA: 0.1Na2O: 50H2O. The mixed initial gel was placed in a closed reactor and crystallized at 160°C for 3 days. The obtained mixture product was washed to a pH value of 7, and then filtered and dried at 120°C to obtain ZSM-23 powder without removing the template agent. 30g of the above ZSM-23 powder was taken, 180mL of water was added and mixed evenly, stirred and heated to 60°C, and 90mL of 0.8mol / L ammonium hexafluorosilicate solution was added dropwise at a uniform rate using a peristaltic pump. The temperature was maintained at 60°C and stirred continuously for 90min. Filter while hot, add 240 mL of water to the filter cake, heat to 60 ° C and keep for 20 min, filter while hot, dry the filter cake at 120 ° C for 24 h, then place the dried product in a hydrothermal treatment furnace, treat at 530 ° C and 0.1 MPa pressure for 2 h, place the obtained material in 300 mL of acetic acid-ammonium acetate solution with a pH value of 6.0, in which the molar concentration of acetate is 0.4 mol / L, stir and heat to 60 ° C, keep for 30 min, then filter while hot, repeat this process 3 times, and dry the filter cake at 120 ° C for 24 h. The modified molecular sieve is named ZSM-23-2.

[0042] Example 3

[0043] 8g of sodium hydroxide was weighed and dissolved in 810mL of water. During the stirring process, 6.66g of aluminum sulfate 18hydrate, 150g of silica sol (mass fraction of 40%), and 35.4g of isopropylamine were added in sequence to form a mixed gel with a material molar ratio of SiO2: 0.01Al2O3: 0.6iPA: 0.1Na2O: 50H2O. The mixed initial gel was placed in a closed reactor and crystallized at 160°C for 3 days. The obtained mixture product was washed to a pH value of 7, and then filtered and dried at 120°C to obtain ZSM-23 powder without removing the template agent. 30g of the above ZSM-23 powder was taken, 180mL of water was added and mixed evenly, stirred and heated to 60°C, and 90mL of 0.8mol / L ethyl orthosilicate solution was added dropwise at a uniform rate using a peristaltic pump. The temperature was maintained at 60°C and stirred continuously for 90min. Filter while hot, add 240 mL of water to the filter cake, heat to 60 ° C and keep for 20 minutes, filter while hot, dry the filter cake at 120 ° C for 24 hours, then place the dried product in a hydrothermal treatment furnace, treat at 550 ° C and 0.1 MPa pressure for 2 hours, place the obtained material in 300 mL of acetic acid-ammonium acetate solution with a pH value of 5.5, in which the molar concentration of acetate is 0.4 mol / L, stir and heat to 60 ° C, keep for 30 minutes, then filter while hot, repeat this process 3 times, and dry the filter cake at 120 ° C for 24 hours. The modified molecular sieve is named ZSM-23-3.

[0044] Example 4

[0045] 8g of sodium hydroxide was weighed and dissolved in 810mL of water. During the stirring process, 6.66g of aluminum sulfate 18hydrate, 150g of silica sol (mass fraction of 40%) and 35.4g of isopropylamine were added in sequence to form a mixed gel with a material molar ratio of SiO2: 0.01Al2O3: 0.6iPA: 0.1Na2O: 50H2O. The mixed initial gel was placed in a closed reactor and crystallized at 160°C for 3 days. The obtained mixture product was washed to a pH value of 7, and then filtered and dried at 120°C to obtain ZSM-23 powder without removing the template agent. 30g of the above ZSM-23 powder was taken, 180mL of water was added and mixed evenly, stirred and heated to 60°C, and 90mL of 0.8mol / L ammonium hexafluorosilicate solution was added dropwise at a uniform rate using a peristaltic pump. The temperature was maintained at 60°C and stirred continuously for 90min. Filter while hot, add 240 mL of water to the filter cake, heat to 60 ° C and keep for 20 min, filter while hot, dry the filter cake at 120 ° C for 24 h, then place the dried product in a hydrothermal treatment furnace, treat at 500 ° C and 0.15 MPa pressure for 2 h, place the obtained material in 300 mL of oxalic acid-ammonium oxalate solution with a pH value of 5.5, wherein the molar concentration of oxalate is 0.3 mol / L, stir and heat to 60 ° C, keep for 30 min, then filter while hot, repeat this process 3 times, and dry the filter cake at 120 ° C for 24 h. The modified molecular sieve obtained is named ZSM-23-4.

[0046] Example 5

[0047] 8g of sodium hydroxide was weighed and dissolved in 810mL of water. During the stirring process, 6.66g of aluminum sulfate 18hydrate, 150g of silica sol (mass fraction of 40%), and 35.4g of isopropylamine were added in sequence to form a mixed gel with a material molar ratio of SiO2: 0.01Al2O3: 0.6iPA: 0.1Na2O: 50H2O. The mixed initial gel was placed in a closed reactor and crystallized at 160°C for 3 days. The obtained mixture product was washed to a pH value of 7, and then filtered and dried at 120°C to obtain ZSM-23 powder without removing the template agent. 30g of the above ZSM-23 powder was taken, 180mL of water was added and mixed evenly, stirred and heated to 60°C, and 90mL of 1.0mol / L ethyl orthosilicate solution was added dropwise at a uniform rate using a peristaltic pump. The temperature was maintained at 60°C and stirred continuously for 90min. Filter while hot, add 240 mL of water to the filter cake, heat to 60 ° C and keep for 20 min, filter while hot, dry the filter cake at 120 ° C for 24 h, then place the dried product in a hydrothermal treatment furnace, treat at 530 ° C and 0.15 MPa pressure for 2 h, place the obtained material in 300 mL of oxalic acid-ammonium oxalate solution with a pH value of 5.5, wherein the molar concentration of oxalate is 0.6 mol / L, stir and heat to 60 ° C, keep for 30 min, then filter while hot, repeat this process 3 times, and dry the obtained filter cake at 120 ° C for 24 h. The modified molecular sieve is named ZSM-23-5.

[0048] Example 6

[0049] 8g of sodium hydroxide was weighed and dissolved in 810mL of water. During the stirring process, 6.66g of aluminum sulfate 18hydrate, 150g of silica sol (mass fraction of 40%), and 35.4g of isopropylamine were added in sequence to form a mixed gel with a material molar ratio of SiO2: 0.01Al2O3: 0.6iPA: 0.1Na2O: 50H2O. The mixed initial gel was placed in a closed reactor and crystallized at 160°C for 3 days. The obtained mixture product was washed to a pH value of 7, and then filtered and dried at 120°C to obtain ZSM-23 powder without removing the template agent. 30g of the above ZSM-23 powder was taken, 180mL of water was added and mixed evenly, stirred and heated to 60°C, and 90mL of 1.0mol / L ammonium hexafluorosilicate solution was added dropwise at a uniform rate using a peristaltic pump. The temperature was maintained at 60°C and stirred continuously for 90min. Filter while hot, add 240 mL of water to the filter cake, heat to 60 ° C and keep for 20 min, filter while hot, dry the filter cake at 120 ° C for 24 h, then place the dried product in a hydrothermal treatment furnace, treat at 550 ° C and 0.15 MPa pressure for 2 h, place the obtained material in 300 mL of oxalic acid-ammonium oxalate solution with a pH value of 5.0, wherein the molar concentration of oxalate is 0.3 mol / L, stir and heat to 60 ° C, keep for 30 min, then filter while hot, repeat this process 3 times, and dry the filter cake at 120 ° C for 24 h. The modified molecular sieve obtained is named ZSM-23-6.

[0050] Example 7

[0051] 8g of sodium hydroxide was weighed and dissolved in 810mL of water. During the stirring process, 6.66g of aluminum sulfate 18hydrate, 150g of silica sol (mass fraction of 40%), and 35.4g of isopropylamine were added in sequence to form a mixed gel with a material molar ratio of SiO2: 0.01Al2O3: 0.6iPA: 0.1Na2O: 50H2O. The mixed initial gel was placed in a closed reactor and crystallized at 160°C for 3 days. The obtained mixture product was washed to a pH value of 7, and then filtered and dried at 120°C to obtain ZSM-23 powder without removing the template agent. 30g of the above ZSM-23 powder was taken, 180mL of water was added and mixed evenly, stirred and heated to 60°C, and 90mL of 1.2mol / L ethyl orthosilicate solution was added dropwise at a uniform rate using a peristaltic pump. The temperature was maintained at 60°C and stirred continuously for 90min. Filter while hot, add 240 mL of water to the filter cake, heat to 60 ° C and keep for 20 min, filter while hot, dry the filter cake at 120 ° C for 24 h, then place the dried product in a hydrothermal treatment furnace, treat at 570 ° C and 0.15 MPa pressure for 2 h, place the obtained material in 300 mL of oxalic acid-ammonium oxalate solution with a pH value of 4.5, wherein the molar concentration of oxalate is 0.4 mol / L, stir and heat to 60 ° C, keep for 30 min, then filter while hot, repeat this process 3 times, and dry the filter cake at 120 ° C for 24 h. The modified molecular sieve obtained is named ZSM-23-7.

[0052] Example 8

[0053] 8g of sodium hydroxide was weighed and dissolved in 810mL of water. During the stirring process, 6.66g of aluminum sulfate 18hydrate, 150g of silica sol (mass fraction of 40%), and 35.4g of isopropylamine were added in sequence to form a mixed gel with a material molar ratio of SiO2: 0.01Al2O3: 0.6iPA: 0.1Na2O: 50H2O. The mixed initial gel was placed in a closed reactor and crystallized at 160°C for 3 days. The obtained mixture product was washed to a pH value of 7, and then filtered and dried at 120°C to obtain ZSM-23 powder without removing the template agent. 30g of the above ZSM-23 powder was taken, 180mL of water was added and mixed evenly, stirred and heated to 60°C, and 90mL of 1.5mol / L ammonium hexafluorosilicate solution was added dropwise at a uniform rate using a peristaltic pump, and the temperature was maintained at 60°C and stirred continuously for 90min. Filter while hot, add 240 mL of water to the filter cake, heat to 60 ° C and keep for 20 min, filter while hot, dry the filter cake at 120 ° C for 24 h, then place the dried product in a hydrothermal treatment furnace, treat at 570 ° C and 0.2 MPa pressure for 2 h, place the obtained material in 300 mL of acetic acid-ammonium acetate solution with a pH value of 4.5, in which the molar concentration of acetate is 0.4 mol / L, stir and heat to 60 ° C, keep for 30 min, then filter while hot, repeat this process 3 times, and dry the filter cake at 120 ° C for 24 h. The modified molecular sieve is named ZSM-23-8.

[0054] Comparative Example 1

[0055] 8g of sodium hydroxide was weighed and dissolved in 810mL of water. During the stirring process, 6.66g of aluminum sulfate 18hydrate, 150g of silica sol (mass fraction of 40%), and 35.4g of isopropylamine were added in sequence to form a mixed gel with a material molar ratio of SiO2: 0.01Al2O3: 0.6iPA: 0.1Na2O: 50H2O. The mixed initial gel was placed in a closed reactor for crystallization at 160°C for 3 days. The obtained mixture product was washed to a pH value of 7, and then filtered, dried at 120°C, and then calcined at 550°C for 6h to obtain a ZSM-23 powder with the template removed. 30g of the above ZSM-23 powder was taken, 180mL of water was added, mixed evenly, stirred and heated to 60°C, and 90mL of 0.5mol / L ammonium hexafluorosilicate solution was added dropwise at a uniform rate using a peristaltic pump. The temperature was maintained at 60°C and stirred continuously for 90min. Filter while hot, add 240 mL of water to the filter cake, heat to 60 ° C and keep for 20 min, filter while hot, dry the filter cake at 120 ° C for 24 h, then place the dried product in a hydrothermal treatment furnace, treat at 500 ° C and 0.1 MPa pressure for 2 h, place the obtained material in 300 mL of oxalic acid-ammonium oxalate solution with a pH value of 6.0, wherein the molar concentration of oxalate is 0.3 mol / L, stir and heat to 60 ° C, keep for 30 min, then filter while hot, repeat this process 3 times, and dry the filter cake at 120 ° C for 24 h. The modified molecular sieve obtained is named ZSM-23-B.

[0056] Comparative Example 2

[0057] 8g of sodium hydroxide was weighed and dissolved in 810mL of water. During the stirring process, 6.66g of aluminum sulfate 18hydrate, 150g of silica sol (mass fraction of 40%), and 35.4g of isopropylamine were added in sequence to form a mixed gel with a material molar ratio of SiO2: 0.01Al2O3: 0.6iPA: 0.1Na2O: 50H2O. The mixed initial gel was placed in a closed reactor and crystallized at 160°C for 3 days. The obtained mixture product was washed to a pH value of 7, and then filtered and dried at 120°C to obtain ZSM-23 powder without removing the template agent. 30g of the above ZSM-23 powder was taken, 180mL of water was added and mixed evenly, stirred and heated to 60°C, and 90mL of 1.0mol / L ammonium hexafluorosilicate solution was added dropwise at a uniform rate using a peristaltic pump. The temperature was maintained at 60°C and stirred continuously for 90min. Filter while hot, add 240mL of water to the filter cake, heat to 60°C and keep for 20min, filter while hot, and dry the filter cake at 120°C for 24h. Then, place the obtained material in a hydrothermal treatment furnace and treat it at 550°C and 0.15MPa pressure for 2h. The obtained modified molecular sieve is named ZSM-23-C.

[0058] Comparative Example 3

[0059] 8 g of sodium hydroxide was weighed and dissolved in 810 mL of water. During stirring, 6.66 g of aluminum sulfate 18hydrate, 150 g of silica sol (mass fraction of 40%) and 35.4 g of isopropylamine were added in sequence to form a mixed gel with a material molar ratio of SiO2: 0.01Al2O3: 0.6iPA: 0.1Na2O: 50H2O. The mixed initial gel was placed in a closed reactor and crystallized at 160°C for 3 days. The obtained mixture product was washed to a pH value of 7, and then filtered and dried at 120°C to obtain a ZSM-23 powder without removing the template. Take 30g of the above ZSM-23 powder and place it in a hydrothermal treatment furnace, treat it at 550℃ and 0.15MPa pressure for 2h, and place the obtained material in 300mL of 0.3mol / L hydrochloric acid solution, stir and heat to 60℃, keep it for 30min, then filter it while hot, wash the filter cake twice, and dry the obtained material at 120℃ for 24h. The modified molecular sieve is named ZSM-23-D.

[0060] Table 1 Characterization results of modified molecular sieves obtained in Examples and Comparative Examples

[0061]

[0062] Example 9

[0063] Catalysts C1-C8 were prepared using the modified molecular sieves obtained in Examples 1-8, respectively. The specific steps were as follows: 10 g of modified ZSM-23 molecular sieve was taken, pressed into tablets of 20-40 mesh, impregnated with 10 mL of 0.005 g / mL H2PtCl6 solution, placed at room temperature for 6 hours, dried at 120°C for 4 hours, and then reduced at 500°C in a hydrogen atmosphere for 4 hours to obtain catalysts containing 0.5 wt% Pt, respectively named C1-C8. 10 mL of the above-prepared catalysts were respectively taken and loaded into a stainless steel tube reactor, heated to the reaction temperature under a hydrogen atmosphere, reacted with the raw material oil n-dodecane, and the products were analyzed by gas chromatography. Reaction conditions: reaction temperature was 280°C, reaction pressure was normal pressure, liquid hourly volume space velocity was 1.0 h -1 , the hydrogen-to-oil volume ratio was 15:1, and the isomerization reaction results are shown in Table 2.

[0064] Comparative Example 4

[0065] Catalysts C9-C11 were prepared using the modified molecular sieves obtained in Comparative Examples 1-3, respectively. The specific steps are as follows: 10 g of modified ZSM-23 molecular sieve was taken, pressed into tablets of 20-40 mesh, impregnated with 10 mL of 0.005 g / mL H2PtCl6 solution, placed at room temperature for 6 hours, dried at 120°C for 4 hours, and then reduced at 500°C in a hydrogen atmosphere for 4 hours to obtain catalysts containing 0.5 wt% Pt, respectively named C9-C11. 10 mL of the above-prepared catalysts were respectively taken and loaded into a stainless steel tube reactor, heated to the reaction temperature under a hydrogen atmosphere, and reacted with the raw material oil n-dodecane, and the products were analyzed by gas chromatography. Reaction conditions: reaction temperature was 280°C, reaction pressure was normal pressure, and the volume space velocity of n-dodecane liquid was 1.0 h -1 , the hydrogen-to-oil volume ratio was 15:1, and the isomerization reaction results are shown in Table 2.

[0066] It can be seen from the evaluation results that the selectivity and yield of isomerized hydrocarbons of the catalyst prepared by the present invention are better than those of the reference catalyst under the same process conditions.

[0067] Table 2 Application results of catalysts obtained in Examples and Comparative Examples

[0068] Catalyst No. n-Dodecane conversion, % Isohydrocarbon selectivity, % Yield of isomerized hydrocarbons, % C1 94.2 65.2 61.4 C2 93.8 68.4 64.2 C3 93.3 72.6 67.7 C4 92.8 78.7 73.0 C5 92.5 86.6 80.1 C6 92.2 87.3 80.5 C7 90.1 81.5 73.4 C8 88.4 76.4 67.5 C9 85.5 59.5 50.9 C10 91.3 61.8 56.4 C11 83.2 50.2 41.8

Claims

1. A method for preparing a modified ZSM-23 molecular sieve, comprising the following steps: (1) preparing a ZSM-23 molecular sieve without removing the template; (2) mixing the ZSM-23 molecular sieve obtained in step (1) with a dealumination and siliconization agent to carry out dealumination and siliconization; (3) treating the material obtained in step (2) with water vapor; (4) treating the material obtained in step (3) with a buffer solution to obtain a modified ZSM-23 molecular sieve; in, In step (2), the dealuminous siliconizing agent is at least one of an ammonium hexafluorosilicate solution and an ethyl orthosilicate solution; the molar concentration of the dealuminous siliconizing agent is 0.5 to 1.5 mol / L; wherein the mass ratio of the ZSM-23 molecular sieve obtained in step (1) to the dealuminous siliconizing agent is 1:2 to 1:8; In step (3), the conditions of the water vapor treatment are: temperature of 400-700° C., pressure of 0.01-0.3 MPa, and time of 0.5-6 h; In step (4), the buffer solution is one or more of oxalic acid-ammonium oxalate solution and acetic acid-ammonium acetate solution; the pH value of the buffer solution is 4.5-6.5; and the liquid-to-solid volume ratio of the buffer solution to the material obtained in step (3) is 3:1-10:

1.

2. The method according to claim 1, Features: In step (2), the operation process of dealumination and siliconization is as follows: the ZSM-23 molecular sieve obtained in step (1) is mixed evenly with water, and then the temperature is raised to 60-100° C., and stirring is continued, and the dealumination and siliconization reagent is added dropwise. After the addition is completed, stirring is continued for 60-120 minutes, and the mixture is filtered while hot, and the filter cake is washed with water, and then filtered again and dried.

3. The method according to claim 1, Features: In step (3), the conditions for the water vapor treatment are: temperature of 500-600° C., pressure of 0.1-0.2 MPa, and time of 1-4 h.

4. The method according to claim 1, Features: The pH value of the buffer solution is 5.0-6.0; in the buffer solution, the molar concentration of the organic acid radical is 0.1-1.0 mol / L.

5. The method according to claim 1, Features: In step (4), the treatment process is: mixing and stirring the material obtained in step (3) with a buffer solution, the treatment temperature is 40 to 80° C., and the treatment time is 0.5 to 3 hours.

6. A modified ZSM-23 molecular sieve prepared according to the method described in any one of claims 1 to 5.

7. The modified ZSM-23 molecular sieve according to claim 6, Features: The outer surface SiO 2 / Al 2 O 3 The molar ratio is 500-1500, the bulk SiO 2 / Al 2 O 3 The molar ratio is 60-200, the total IR acid content of pyridine is 0.02-0.35 mmol / g, and the total IR acid content of di-tert-butylpyridine is 0.001-0.015 mmol / g.

8. The modified ZSM-23 molecular sieve according to claim 6, Features: The outer surface SiO 2 / Al 2 O 3 The molar ratio is 600-1000, the bulk SiO 2 / Al 2 O 3 The molar ratio is 80-150.

9. The modified ZSM-23 molecular sieve according to claim 6, Features: The total infrared acid content of pyridine in the modified ZSM-23 molecular sieve is 0.10-0.25 mmol / g, and the total infrared acid content of di-tert-butylpyridine is 0.005-0.012 mmol / g.

10. Use of the modified ZSM-23 molecular sieve prepared by the method according to any one of claims 1 to 5 in a catalyst for the shape-selective isomerization of normal alkanes.