Composite semipermeable membrane, spiral membrane element, water treatment system and water treatment method

By using composite semipermeable membrane and spiral membrane elements with moderate elastic modulus in the ZLD system, combined with the design of low-pressure, medium-pressure and high-pressure reverse osmosis membrane modules, the problem of reducing salt retention caused by frequent opening/closing is solved, and the problem of extended The life of the membrane is reduced and energy consumption is reduced.

CN116078179BActive Publication Date: 2024-11-08NITTO DENKO CORP
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
CN202211370782.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-11-05
Filing Date
2022-11-03
Publication Date
2024-11-08
Estimated Expiration
2042-11-03

AI Technical Summary

Technical Problem

In ZLD systems, frequent turn-on/close operations lead to a shortened life of the composite semipermeable membrane, a reduced salt retention rate, and an increased operating pressure to compensate for the decrease in osmotic flux, the pump power consumption increases.

Method used

A composite semipermeable membrane with a surface elastic modulus of membranes above 250MPa and below 500MPa is adopted, and wastewater concentration is performed by spiral membrane elements in the water treatment system using low-pressure, medium-pressure and high-pressure reverse osmosis membrane modules, medium-pressure reverse osmosis membrane modules. Using a helical membrane element, the knitting density of the permeable flow path material is adjusted to improve durability.

Benefits of technology

It extends the life of the composite semipermeable membrane, reduces the reduction of salt retention, reduces the demand for operating pressure, improves the durability of water pressure opening/closing, and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116078179B_ABST
    Figure CN116078179B_ABST
Patent Text Reader

Abstract

The present invention relates to a composite semipermeable membrane, a spiral membrane element, a water treatment system and a water treatment method. The composite semipermeable membrane (12) of the present invention has a porous support membrane (12a) and a surface layer (12b) supported by the porous support membrane (12a). The elastic modulus of the membrane surface calculated by measuring the force curve using AFM in water is greater than 250 MPa and less than 500 MPa. The spiral membrane element (20) of the present invention has the composite semipermeable membrane (12) of the present invention. The water treatment system (100) of the present invention has the spiral membrane element (20) of the present invention.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a composite semipermeable membrane, a spiral membrane element, a water treatment system and a water treatment method. Background Art

[0002] In recent years, the ZLD system (zero liquid discharge system) has attracted attention. "ZLD" refers to a technical concept for reducing liquid waste discharged into the natural world such as rivers and oceans to zero. In the ZLD system, wastewater is concentrated by membrane separation technology, and then water is evaporated from the concentrated wastewater to generate solid waste. The energy consumption when generating solid waste in the final stage is very large. According to the membrane separation technology, energy consumption can be suppressed by significantly reducing the amount of wastewater in the final stage.

[0003] A typical ZLD system has a plurality of reverse osmosis membrane units connected in series, as described in Patent Document 1. Wastewater is gradually concentrated by the plurality of reverse osmosis membrane units.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Publication No. 2020-44457 Summary of the invention

[0007] Problems to be solved by the invention

[0008] In a water treatment system, when the salt retention rate is lower than a specified level, it is recommended to replace the membrane. The longer the life of the membrane, the lower the cost of water treatment, so it is preferred. The life of the membrane is affected by various factors such as the purpose of the water treatment system, the composition of the raw water, the temperature of the raw water, and the operating pressure. Here, the inventors found that in a specific water treatment system such as the ZLD system, there is a situation where the life of the membrane is lower than expected. And it was found that the reason is that the system is frequently operated and stopped repeatedly.

[0009] For example, in a well-known seawater desalination system, seawater is supplied to the seawater desalination system at a constant flow rate, and fresh water is generated at a constant flow rate. On the other hand, in a specific water treatment system such as a ZLD system, the flow rate of wastewater (raw water) is sometimes not constant. As one reason why the flow rate of wastewater is not constant, it can be cited that the flow rate of wastewater depends on the operation of the factory. Although a buffer tank is provided for stabilizing the flow rate of wastewater, the ZLD system automatically stops when the water level of the buffer tank is lower than a specified water level.

[0010] When the operation and stop of the system are frequently switched, the composite semipermeable membrane is subjected to water pressure or relieved of water pressure. As a result, the composite semipermeable membrane is damaged and its interception performance is rapidly reduced. For example, if a permeation side flow path material with a high knitting density is used, damage to the composite semipermeable membrane can be suppressed. However, when a permeation side flow path material with a high knitting density is used, the permeation flux is reduced. When the operating pressure is increased to compensate for the reduction in the permeation flux, the power consumption of the pump increases.

[0011] The present invention aims to provide a composite semipermeable membrane suitable for a system that is frequently opened and closed repeatedly, such as a ZLD system. In addition, the present invention provides a spiral membrane element using the composite semipermeable membrane, a water treatment system using the spiral membrane element, and a water treatment method using the spiral membrane element.

[0012] Means used to solve problems

[0013] The present invention provides a composite semipermeable membrane, wherein the composite semipermeable membrane comprises a porous support membrane and a surface layer supported by the porous support membrane, and

[0014] The elastic modulus of the membrane surface calculated by force curve measurement using an AFM in water is 250 MPa or more and 500 MPa or less.

[0015] In another aspect, the present invention provides a spiral membrane element, wherein the spiral membrane element has the composite semipermeable membrane of the present invention.

[0016] In another aspect, the present invention provides a water treatment system, wherein the water treatment system comprises the spiral membrane element of the present invention.

[0017] In another aspect, the present invention provides a water treatment method, wherein the water treatment method comprises the following steps:

[0018] A process for concentrating wastewater using a low-pressure reverse osmosis membrane module;

[0019] A step of further concentrating the wastewater concentrated by the low-pressure reverse osmosis membrane module by using a medium-pressure reverse osmosis membrane module; and

[0020] The process of further concentrating the wastewater concentrated by the medium-pressure reverse osmosis membrane module by using a high-pressure reverse osmosis membrane module,

[0021] The medium-pressure reverse osmosis membrane module comprises the spiral membrane element of the present invention.

[0022] The supply pressure of the low-pressure reverse osmosis membrane module is lower than the supply pressure of the medium-pressure reverse osmosis membrane module.

[0023] The supply pressure of the medium-pressure reverse osmosis membrane module is lower than the supply pressure of the high-pressure reverse osmosis membrane module, and

[0024] The supply pressure of the medium-pressure reverse osmosis membrane module is greater than or equal to 2.0 MPa and less than or equal to 4.0 MPa.

[0025] Effects of the Invention

[0026] According to the present invention, it is possible to provide a composite semipermeable membrane suitable for a system such as a ZLD system that frequently repeats opening and closing. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a developed perspective view of the spiral membrane element according to the first embodiment.

[0028] Figure 2 For Figure 1 A cross-sectional view of a composite semipermeable membrane used in a spiral membrane element is shown.

[0029] Figure 3 A cross-sectional view illustrating the mechanism by which the composite semipermeable membrane is damaged.

[0030] Figure 4 This is a structural diagram of the water treatment system according to the second embodiment.

[0031] Figure 5 A diagram illustrating a method for measuring a force curve using AFM in water.

[0032] Fig. 6A This is an optical microscope image of the composite semipermeable membrane of sample 1 after staining.

[0033] Figure 6B This is an optical microscope image of the composite semipermeable membrane of sample 3 after staining.

[0034] Figure 6C This is an optical microscope image of the composite semipermeable membrane of Sample 7 after staining. DETAILED DESCRIPTION

[0035] Hereinafter, embodiments of the present invention will be described with reference to the drawings. The present invention is not limited to the following embodiments.

[0036] (Implementation Method 1)

[0037] Figure 1 The spiral membrane element 20 of the first embodiment of the present invention is shown. The spiral membrane element 20 has a water collecting pipe 21 and a stack 22. The stack 22 is arranged around the water collecting pipe 21. A raw water flow path and a permeate flow path are formed inside the stack 22. The water collecting pipe 21 passes through the center of the stack 22.

[0038] Raw water is supplied to the inside of the spiral membrane element 20 from one end face of the stack 22, and flows through the raw water flow path in parallel with the length direction of the water collecting pipe 21. In the spiral membrane element 20, the raw water is filtered to generate concentrated water and permeate water. The permeate water is guided to the outside through the water collecting pipe 21. The concentrated water is discharged to the outside of the spiral membrane element 20 from the other end face of the stack 22.

[0039] As the raw water to be treated (filtered) by the spiral membrane element 20, wastewater discharged from factories and the like can be cited. As wastewater, coking wastewater, coal chemical wastewater, produced water, etc. can be cited. Coking wastewater, coal chemical wastewater, and produced water sometimes contain aromatic compounds at a concentration of about several ppm to about several hundred ppm. Aromatic compounds are known as components that cause chemical degradation of composite semipermeable membranes. Therefore, it is not easy to treat wastewater containing aromatic compounds. However, the composite semipermeable membrane of this embodiment can be used for a long time even with wastewater containing aromatic compounds. However, raw water is not limited to wastewater.

[0040] The stack 22 is composed of a composite semipermeable membrane 12, a raw water side flow material 13, and a permeate side flow material 14. The end surface of the composite semipermeable membrane 12 constitutes the end surface of the stack 22. Specifically, the stack 22 is composed of a plurality of composite semipermeable membranes 12, a plurality of raw water side flow materials 13, and a plurality of permeate side flow materials 14.

[0041] The raw water side flow path material 13 may be a member having a mesh structure made of a resin material such as polyester, polyethylene, polypropylene, etc. The permeate side flow path material 14 may be a knitted fabric made of a resin material such as polyester, polyethylene, polypropylene, etc. The permeate side flow path material 14 is typically a warp knitted fabric.

[0042] A plurality of composite semipermeable membranes 12 are overlapped, sealed at three sides in a bag-like structure, and wound on a water collecting pipe 21. A raw water side flow path material 13 is arranged between the composite semipermeable membranes 12 and the composite semipermeable membranes 12 in a manner located outside the bag-like structure. The raw water side flow path material 13 ensures a space as a raw water flow path between the composite semipermeable membranes 12 and the composite semipermeable membranes 12. A permeate side flow path material 14 is arranged between the composite semipermeable membranes 12 and the composite semipermeable membranes 12 in a manner located inside the bag-like structure. The permeate side flow path material 14 ensures a space as a permeate water flow path between the composite semipermeable membranes 12 and the composite semipermeable membranes 12. The membrane sheet 11 is composed of a pair of composite semipermeable membranes 12 and the permeate side flow path material 14. The open end of the membrane sheet 11 is connected to the water collecting pipe 21 in a manner that the permeate water flow path is connected to the water collecting pipe 21.

[0043] The water collecting pipe 21 collects the permeated water that permeates each composite semipermeable membrane 12 and guides it to the outside of the spiral membrane element 20. A plurality of through holes 21h are provided at predetermined intervals along the length direction of the water collecting pipe 21. The permeated water flows into the water collecting pipe 21 through these through holes 21h.

[0044] Figure 2 For Figure 1 A cross-sectional view of a composite semipermeable membrane 12 used in the spiral membrane element 20 shown. The composite semipermeable membrane 12 comprises a porous support membrane 12a, a surface layer 12b and a coating layer 12c. The porous support membrane 12a, the surface layer 12b and the coating layer 12c are stacked in sequence. The surface layer 12b and the coating layer 12c are supported by the porous support membrane 12a. The surface layer 12b is arranged on the porous support membrane 12a. The coating layer 12c is arranged on the surface layer 12b. The coating layer 12c covers the surface layer 12b. In detail, the coating layer 12c is in direct contact with the surface layer 12b.

[0045] Figure 3 A cross-sectional view illustrating the mechanism by which the composite semipermeable membrane is damaged. When raw water is introduced into the spiral membrane element and water pressure F is applied to the composite semipermeable membrane 121, a portion of the composite semipermeable membrane 121 sinks into the groove 14m of the permeable side flow path material 14. The remaining portion of the composite semipermeable membrane 121 is pressed against the permeable side flow path material 14, and a load indicated by a dotted arrow is locally applied. The groove 14m is, for example, a portion between a longitudinal row of coils. When the introduction of raw water stops, the composite semipermeable membrane 121 is relieved of the water pressure F. The load indicated by the dotted arrow is hardly applied. When the introduction of raw water is resumed, water pressure F is applied to the composite semipermeable membrane 121 again. When the application and release of water pressure F are repeated, defects are generated on the composite semipermeable membrane 121, centered on the portion repeatedly pressed against the permeable side flow path material 14. Defects of the composite semipermeable membrane 121 are easily generated on a thin surface layer. As a result, the salt rejection rate of the composite semipermeable membrane 121 decreases rapidly.

[0046] It is also believed that when the composite semipermeable membrane 121 has sufficient rigidity to resist the water pressure F, the composite semipermeable membrane 121 is not easily damaged by the on / off of the water pressure F. However, contrary to expectations, having appropriate flexibility is effective in suppressing damage caused by the on / off of the water pressure F.

[0047] That is, the elastic modulus of the membrane surface 12p of the composite semipermeable membrane 12 of the present embodiment is more than 250MPa and less than 500MPa. The elastic modulus of the membrane surface 12p is calculated by measuring the force curve of the AFM (atomic force microscope) in water. When the elastic modulus of the membrane surface 12p is within such a range, even if the opening / closing of the water pressure is repeatedly performed, the composite semipermeable membrane 12 is not easily damaged. As a result, the life of the spiral membrane element 20 is extended.

[0048] The method of measuring the force curve using AFM in water is as described in the first embodiment.

[0049] In the composite semipermeable membrane 12, the coating layer 12c contains a polymer. With the coating layer 12c, the elastic modulus of the membrane surface 12p can be easily adjusted.

[0050] The type of polymer contained in the coating layer 12c is different from the type of polymer contained in the surface layer 12b. The surface layer 12b is made of polyamide, for example. The polymer contained in the coating layer 12c includes, for example, a polymer selected from polyvinyl alcohol, betaine polymer and polyol. At least one polymer selected from the group consisting of oxazoline. These polymers are hydrophilic (having a hydrophilic group). With these polymers, the elastic modulus of the membrane surface 12p can be easily adjusted.

[0051] There is no particular restriction on the thickness of the coating 12c. The thickness of the coating 12c is, for example, 10 nm to 1000 nm. The thickness of the coating 12c is obtained by the following method. That is, the thickness of the coating 12c is measured at any number of points (e.g., 10 points) on the cross section of the composite semipermeable membrane 12. The average value of the obtained measured values ​​can be regarded as the thickness of the coating 12c. The thickness is measured using SEM or TEM.

[0052] The presence of the coating layer 12c can be confirmed using a scanning electron microscope or a transmission electron microscope. The composition analysis of the polymer contained in the coating layer 12c can be performed by Fourier transform infrared spectroscopy (FT-IR), X-ray photoelectron spectroscopy (XPS) or time-of-flight secondary ion mass spectrometry (TOF-SIMS).

[0053] There are various factors that determine the elastic modulus of the membrane surface 12p. Specifically, the material of the surface layer 12b, the thickness of the surface layer 12b, the surface roughness (Ra) of the surface layer 12b, the material of the coating 12c, the thickness of the coating 12c, the temperature when the surface layer 12b is formed, etc. can be cited. The elastic modulus of the membrane surface 12p is improved by heat treating the surface layer 12b after the surface layer 12b is formed. The heat treatment is performed, for example, by exposing the membrane to warm water at about 50°C. In addition, when the material of the coating 12c is soft or the material of the coating 12c has high hydrophilicity, the elastic modulus of the membrane surface 12p tends to decrease. When the thickness of the coating 12c increases, the elastic modulus of the membrane surface 12p tends to decrease. However, when the thickness of the coating 12c is excessively increased, the permeation flux (m 3 / m 2 / day) decreased.

[0054] In the spiral membrane element 20, the permeate side flow path material 14, which is a warp knitted fabric, has a knitting density of 31 to 60 wales and 34 to 52 horizontal rows. The composite semipermeable membrane 12 is in contact with the permeate side flow path material 14. In the present embodiment, the knitting density of the permeate side flow path material 14 is adjusted to match the composite semipermeable membrane 12. The effect of adjusting the elastic modulus of the membrane surface of the composite semipermeable membrane 12 and the effect of adjusting the knitting density of the permeate side flow path material 14 are combined with each other, thereby further improving the durability of opening / closing to water pressure while ensuring the desired permeation flux.

[0055] It should be noted that wale refers to the longitudinal stitch of a knitted fabric. Course refers to the transverse stitch of a knitted fabric. The density (knitting density) of a knitted fabric is represented by the number of wales per inch (wale density) and the number of courses per inch (course density). The knitting density can be represented by (wale density)×(course density).

[0056] The degree of damage of the composite semipermeable membrane 12 can be known by the reduction of the salt retention rate after the opening / closing test. The salt retention rate is defined by the NaCl retention rate, for example. Specifically, a NaCl aqueous solution of a specified concentration is supplied to the spiral membrane element 20 under a specified supply pressure, and the NaCl retention rate is measured. Next, the supply of the NaCl aqueous solution is stopped. Then, the supply of the NaCl aqueous solution is restarted. This cycle is repeated n times (for example, 7000 times). The supply pressure is, for example, greater than 2.0 MPa and less than 4.0 MPa. The degree of damage of the composite semipermeable membrane 12 can be known based on the difference between the first NaCl retention rate and the nth NaCl retention rate.

[0057] The NaCl retention rate can be measured according to Japanese Industrial Standard JIS K 3805 (1990). Specifically, the NaCl aqueous solution is passed through a composite semipermeable membrane 12 of a specified size under a specified supply pressure. After the 30-minute preparation phase (first time) is completed, the conductivity of the permeated water and the supply water is measured using a conductivity measuring device, and the NaCl retention rate can be calculated based on the following formula according to its result and the calibration curve (concentration-conductivity). Concentration determination can be performed by ion chromatography instead of conductivity determination.

[0058] NaCl rejection rate (%) = (1-(NaCl concentration of permeated water / NaCl concentration of feed water)) × 100 The composite semipermeable membrane 12 is typically a reverse osmosis membrane (RO membrane). However, the composite semipermeable membrane 12 may also be a nanofiltration membrane (NF membrane).

[0059] In this specification, "NF membrane" refers to a composite semipermeable membrane having a NaCl rejection rate of 5% or more and less than 93% when filtering a NaCl aqueous solution with a concentration of 2000 mg / liter under the conditions of a supply pressure of 1.55 MPa and 25°C. "RO membrane" refers to a composite semipermeable membrane having a NaCl rejection rate of 93% or more when filtering a NaCl aqueous solution with a concentration of 2000 mg / liter under the conditions of a supply pressure of 1.55 MPa and 25°C.

[0060] The composite semipermeable membrane 12 can be produced by the following method.

[0061] First, a porous support membrane 12a is prepared as a support. The porous support membrane 12a is not particularly limited as long as it is a membrane on which a surface layer 12b can be formed. As the porous support membrane 12a, an ultrafiltration membrane having a microporous layer with an average pore size of 0.01 μm to 0.4 μm formed on a non-woven fabric can be used. As the material for forming the microporous layer, for example, polyarylethersulfones such as polysulfone and polyethersulfone; polyimide; polyvinylidene fluoride; polyetherimide, etc. can be listed. From the viewpoint of chemical stability, mechanical stability and thermal stability, polysulfone or polyarylethersulfone can be used. In addition, a self-supporting porous support membrane made of a thermosetting resin such as an epoxy resin having the above-mentioned average pore size can also be used. There is no particular limitation on the thickness of the porous support membrane 12a, for example, it is in the range of 10 μm to 200 μm, and it can also be in the range of 20 μm to 75 μm.

[0062] In this specification, "average pore size" refers to a value calculated by the following method. First, the surface or cross section of a film or layer is observed using an electron microscope (e.g., a scanning electron microscope), and the diameters of a plurality of holes (e.g., any 10 holes) observed are actually measured. The average value of the actual measured values ​​of the hole diameters is defined as the "average pore size". "The diameter of a hole" refers to the major diameter of a hole, and more specifically, refers to the diameter of the smallest circle that can surround a hole.

[0063] Next, a first solution containing a raw material of the surface layer 12b is brought into contact with the porous support film 12a. The first solution is typically an aqueous solution containing a polyfunctional amine as a raw material of the surface layer 12b (hereinafter referred to as "amine aqueous solution"). By bringing the amine aqueous solution into contact with the porous support film 12a, a layer containing amine is formed on the surface of the porous support film 12a. In addition to water, the amine aqueous solution may also contain a polar solvent other than water, such as alcohol. A polar solvent other than water, such as alcohol, may be used instead of water.

[0064] The polyfunctional amine is an amine having a plurality of reactive amino groups. Examples of the polyfunctional amine include aromatic polyfunctional amines, aliphatic polyfunctional amines, and alicyclic polyfunctional amines.

[0065] Examples of the aromatic polyfunctional amine include metaphenylenediamine, paraphenylenediamine, o-phenylenediamine, 1,3,5-triaminobenzene, 1,2,4-triaminobenzene, 3,5-diaminobenzoic acid, 2,4-diaminotoluene, 2,6-diaminotoluene, N,N′-dimethyl-metaphenylenediamine, 2,4-diaminoanisole, amphenol, and xylylenediamine.

[0066] Examples of the aliphatic polyfunctional amine include ethylenediamine, propylenediamine, tris(2-aminoethyl)amine, and N-phenylethylenediamine.

[0067] Examples of the alicyclic polyfunctional amine include 1,3-diaminocyclohexane, 1,2-diaminocyclohexane, 1,4-diaminocyclohexane, piperazine, and piperazine derivatives.

[0068] Only one type selected from these polyfunctional amines may be used, or two or more types may be used in combination.

[0069] In order to facilitate the formation of the amine-containing layer and improve the performance of the surface layer 12 b , a polymer such as polyvinyl alcohol, polyvinyl pyrrolidone, polyacrylic acid, or a polyol such as sorbitol or glycerol may be added to the amine aqueous solution.

[0070] The concentration of the amine component in the aqueous amine solution may be in the range of 0.1 mass % to 15 mass %, or in the range of 1 mass % to 10 mass %. By appropriately adjusting the concentration of the amine component, defects such as pinholes in the surface layer 12b can be suppressed. In addition, a surface layer 12b having excellent salt retention performance can be formed. In addition, if the concentration of the amine component is appropriately adjusted, the thickness of the surface layer 12b can also be appropriately adjusted, thereby obtaining a composite semipermeable membrane 12 capable of achieving sufficient permeation flux.

[0071] There is no particular limitation on the method of bringing the amine aqueous solution into contact with the porous support membrane 12a. A method of immersing the porous support membrane 12a in an amine aqueous solution, a method of coating the amine aqueous solution on the porous support membrane 12a, and a method of spraying the amine aqueous solution on the porous support membrane 12a can be appropriately adopted. In addition, after implementing the process of bringing the amine aqueous solution into contact with the porous support membrane 12a, a process of removing excess amine aqueous solution from the porous support membrane 12a can be implemented. For example, by extending the layer containing amine using a rubber roller, excess amine aqueous solution can be removed from the porous support membrane 12a. By removing the excess amine aqueous solution, a surface layer 12b of appropriate thickness can be formed.

[0072] Next, the second solution is brought into contact with the layer containing amines. The second solution is a solution containing other raw materials of the surface layer 12b. In detail, the second solution is a solution containing a polyfunctional acyl halide as other raw materials of the surface layer 12b (hereinafter referred to as "acyl halide solution"). When the acyl halide solution is brought into contact with the layer containing amines, a polymerization reaction of amines and acyl halides is carried out at the interface between the layer containing amines and the acyl halide solution layer. Thus, the surface layer 12b is formed.

[0073] The polyfunctional acid halide is an acid halide having a plurality of reactive carbonyl groups. Examples of the polyfunctional acid halide include aromatic polyfunctional acid halides, aliphatic polyfunctional acid halides, and alicyclic polyfunctional acid halides.

[0074] Examples of the aromatic polyfunctional acid halide include trimesoyl chloride, terephthaloyl chloride, isophthaloyl chloride, biphenyl diphthaloyl chloride, naphthalene diphthaloyl chloride, benzenetrisulfonyl chloride, benzene disulfonyl chloride, and chlorosulfonyl terephthaloyl chloride.

[0075] Examples of the aliphatic polyfunctional acid halide include malonyl chloride, succinoyl chloride, glutaryl chloride, trimalonyl chloride, succinoyl chloride, glutaryl chloride, glutaryl halide, and adipoyl halide.

[0076] Examples of the alicyclic polyfunctional acid halide include cyclopropanetricarboxylic acid chloride, cyclobutanetetracarboxylic acid chloride, cyclopentanetricarboxylic acid chloride, cyclopentanetetracarboxylic acid chloride, cyclohexanetricarboxylic acid chloride, tetrahydrofurantetracarboxylic acid chloride, cyclopentanedicarboxylic acid chloride, cyclobutanedicarboxylic acid chloride, cyclohexanedicarboxylic acid chloride, and tetrahydrofurandicarboxylic acid chloride.

[0077] Only one selected from these polyfunctional acyl halides can be used, or two or more can be used in combination. In order to obtain a surface layer 12b with excellent salt interception performance, aromatic polyfunctional acyl halides can be used. In addition, a cross-linked structure can be formed by using a polyfunctional acyl halide of more than 3 yuan in at least a part of the polyfunctional acyl halide component.

[0078] As the solvent of the acid halide solution, an organic solvent, in particular a non-polar organic solvent, can be used. The organic solvent is not particularly limited as long as it has low solubility in water, does not deteriorate the porous support membrane 12a, and can dissolve the multifunctional acid halide component. Examples of organic solvents include saturated hydrocarbons such as cyclohexane, heptane, octane, and nonane; halogenated hydrocarbons such as 1,1,2-trichlorotrifluoroethane, etc. Saturated hydrocarbons with a boiling point of less than 300°C or less than 200°C can be used.

[0079] The concentration of the acyl halide component in the acyl halide solution may be in the range of 0.01 mass % to 5 mass %, or in the range of 0.05 mass % to 3 mass %. By appropriately adjusting the concentration of the acyl halide component, the unreacted amine component and the acyl halide component can be reduced. In addition, the generation of defects such as pinholes in the surface layer 12b can be suppressed, thereby providing a composite semipermeable membrane 12 having excellent salt retention performance. In addition, if the concentration of the acyl halide component is appropriately adjusted, the thickness of the surface layer 12b can also be appropriately adjusted, thereby providing a composite semipermeable membrane 12 capable of achieving sufficient permeation flux.

[0080] There is no particular limitation on the method of bringing the acyl halide solution into contact with the amine-containing layer. The amine-containing layer and the porous support membrane 12a may be immersed in the acyl halide solution, or the acyl halide solution may be coated on the surface of the amine-containing layer. The contact time between the amine-containing layer and the acyl halide solution is, for example, 10 seconds to 5 minutes or 30 seconds to 1 minute. After bringing the amine-containing layer into contact with the acyl halide solution, a process of removing excess acyl halide solution from the amine-containing layer may be performed.

[0081] Next, the surface layer 12b is heated together with the porous support film 12a to be dried. By heating the surface layer 12b, the mechanical strength, heat resistance, etc. of the surface layer 12b can be improved. The heating temperature is, for example, 70°C to 200°C or 80°C to 130°C. The heating time is, for example, 30 seconds to 10 minutes or 40 seconds to 7 minutes. After the drying process is carried out at room temperature, a further drying process can be carried out using a dryer at an atmospheric temperature higher than room temperature.

[0082] It should be noted that various additives may be added to the aqueous amine solution and / or the acyl halide solution in order to facilitate the formation of the surface layer 12b or to improve the performance of the composite semipermeable membrane 12 to be obtained. Examples of additives include surfactants such as sodium dodecylbenzenesulfonate, sodium dodecyl sulfate, and sodium lauryl sulfate; alkaline compounds such as sodium hydroxide, trisodium phosphate, and triethylamine that are effective in removing hydrogen halide generated by polymerization; acylation catalysts, solubility parameters of 8 to 14 (cal / cm 3 ) 1 / 2 of compounds, etc.

[0083] By carrying out the above steps, a membrane having a porous support membrane 12a and a surface layer 12b can be obtained. The thickness of the surface layer 12b is not particularly limited, and is, for example, 0.05 μm to 2 μm, or 0.1 μm to 1 μm.

[0084] In addition, in this specification, a method of directly forming the surface layer 12b on the surface of the porous support film 12a by interfacial polymerization is described. However, the surface layer 12b can be formed on a support other than the porous support film 12a, and the obtained surface layer 12b can be transferred to the porous support film 12a and integrated. In other words, the surface layer 12b can be transferred from another support to the porous support film 12a.

[0085] Next, a coating layer 12c is formed. The coating layer 12c can be formed by bringing the aqueous solution containing the polymer described above into contact with the surface layer 12b to form a layer containing the polymer, and then drying the layer containing the polymer. There is no particular limitation on the method of bringing the aqueous solution into contact with the surface layer 12b. The surface layer 12b can be immersed in the aqueous solution together with the porous support membrane 12a, or the aqueous solution can be applied to the surface of the surface layer 12b. The contact time between the surface layer 12b and the aqueous solution is, for example, 10 seconds to 5 minutes. After bringing the surface layer 12b into contact with the aqueous solution, a process of removing excess aqueous solution from the surface layer 12b can be implemented. In addition to water, the aqueous solution can also contain polar solvents other than water, such as alcohol. Polar solvents other than water, such as alcohol, can be used instead of water.

[0086] Next, the polymer-containing layer is heated to dry it. By heating the polymer-containing layer, the mechanical strength, heat resistance, etc. of the coating layer 12c can be improved. The heating temperature is, for example, 80°C to 150°C. The heating time is, for example, 10 seconds to 300 seconds. The drying process can be carried out at room temperature, and then a further drying process can be carried out using a dryer at an atmospheric temperature higher than room temperature.

[0087] By carrying out the above steps, the composite semipermeable membrane 12 having the porous support membrane 12 a , the surface layer 12 b , and the coating layer 12 c can be obtained.

[0088] (Implementation Method 2)

[0089] Figure 4 1 is a structural diagram of a water treatment system according to Embodiment 2. The water treatment system 100 has a plurality of reverse osmosis membrane modules. The plurality of reverse osmosis membrane modules include a low-pressure reverse osmosis membrane module 110, a medium-pressure reverse osmosis membrane module 120, and a high-pressure reverse osmosis membrane module 130. The low-pressure reverse osmosis membrane module 110, the medium-pressure reverse osmosis membrane module 120, and the high-pressure reverse osmosis membrane module 130 are connected to each other in a manner of filtering wastewater in sequence.

[0090] At least one reverse osmosis membrane module selected from the group consisting of the low-pressure reverse osmosis membrane module 110, the medium-pressure reverse osmosis membrane module 120, and the high-pressure reverse osmosis membrane module 130 includes the spiral membrane element 20 described in Embodiment 1. The spiral membrane element 20 has excellent durability against opening / closing of water pressure. Therefore, in the water treatment system 100, even if opening / closing is repeated, the salt retention performance of the module including the spiral membrane element 20 can be maintained for a long time.

[0091] In detail, the medium-pressure reverse osmosis membrane module 120 includes the spiral membrane element 20 described in Embodiment 1. Since the supply pressure in the low-pressure reverse osmosis membrane module 110 is low, even if the water pressure is repeatedly turned on / off, it is not easy to damage the composite semipermeable membrane used in the low-pressure reverse osmosis membrane module 110. A permeate side flow path material with a dense knitting density can be used in the high-pressure reverse osmosis membrane module 130. It is difficult for the medium-pressure reverse osmosis membrane module 120 to achieve a balance between the structure and the supply pressure. Therefore, by using the spiral membrane element 20 of Embodiment 1 in the medium-pressure reverse osmosis membrane module 120, the salt retention performance of the medium-pressure reverse osmosis membrane module 120 can be maintained for a long time.

[0092] The spiral membrane element can also be used in the low-pressure reverse osmosis membrane module 110 and the high-pressure reverse osmosis membrane module 130 .

[0093] The water treatment system 100 is, for example, a ZLD system. As described above, the operation and stop of the ZLD system are sometimes frequently switched. Therefore, the water treatment system 100 of this embodiment is particularly suitable for ZLD applications.

[0094] The flow path 2a is connected to the inlet of the low-pressure reverse osmosis membrane module 110. The flow path 2b is connected to the concentrated water outlet of the low-pressure reverse osmosis membrane module 110 and the inlet of the medium-pressure reverse osmosis membrane module 120. The flow path 2c is connected to the concentrated water outlet of the medium-pressure reverse osmosis membrane module 120 and the inlet of the high-pressure reverse osmosis membrane module 130.

[0095] The low-pressure reverse osmosis membrane module 110 has at least one low-pressure reverse osmosis membrane element housed in a pressure-resistant container. The low-pressure reverse osmosis membrane module 110 may have a plurality of low-pressure reverse osmosis membrane elements or only one low-pressure reverse osmosis membrane element.

[0096] The medium-pressure reverse osmosis membrane module 120 has at least one medium-pressure reverse osmosis membrane element accommodated in a pressure-resistant container. The medium-pressure reverse osmosis membrane module 120 may have a plurality of medium-pressure reverse osmosis membrane elements or only one medium-pressure reverse osmosis membrane element.

[0097] The high-pressure reverse osmosis membrane module 130 has at least one high-pressure reverse osmosis membrane element housed in a pressure-resistant container. The high-pressure reverse osmosis membrane module 130 may have a plurality of high-pressure reverse osmosis membrane elements or only one high-pressure reverse osmosis membrane element.

[0098] The supply pressure of the low-pressure reverse osmosis membrane module 110 is, for example, greater than or equal to 0.5 MPa and less than 2.0 MPa. The supply pressure of the medium-pressure reverse osmosis membrane module 120 is, for example, greater than 2.0 MPa and less than 4.0 MPa. The supply pressure of the high-pressure reverse osmosis membrane module 130 is, for example, greater than 4.0 MPa and less than or equal to 8.0 MPa. That is, the supply pressure of the low-pressure reverse osmosis membrane module 110 is lower than the supply pressure of the medium-pressure reverse osmosis membrane module 120. The supply pressure of the medium-pressure reverse osmosis membrane module 120 is lower than the supply pressure of the high-pressure reverse osmosis membrane module 130. By appropriately adjusting the supply pressure of each reverse osmosis membrane module and using the spiral membrane element 20 of embodiment 1 in the medium-pressure reverse osmosis membrane module 120, a water treatment system 100 with excellent durability against opening / closing of water pressure can be constructed.

[0099] The low-pressure reverse osmosis membrane module 110, the medium-pressure reverse osmosis membrane module 120, and the high-pressure reverse osmosis membrane module 130 each have a permeate-side flow path material that is a warp knitted fabric. The knitting density of the permeate-side flow path material used in the low-pressure reverse osmosis membrane module 110 is lower than the knitting density of the permeate-side flow path material used in the medium-pressure reverse osmosis membrane module 120. The knitting density of the permeate-side flow path material used in the medium-pressure reverse osmosis membrane module 120 is smaller than the knitting density of the permeate-side flow path material used in the high-pressure reverse osmosis membrane module 130. According to such a structure, while the permeate flux of each module is appropriately ensured, even if the water treatment system 100 is repeatedly operated and stopped, the composite semipermeable membrane in each module is not easily damaged.

[0100] The wastewater subjected to appropriate pretreatment is introduced into the low-pressure reverse osmosis membrane module 110 through the flow path 2a. The wastewater is concentrated in the low-pressure reverse osmosis membrane module 110. As pretreatment, the treatment of wastewater by sand filtration such as silica sand, the treatment of wastewater filtration by UF membrane (ultrafiltration membrane) or MF membrane (microfiltration membrane), etc. can be cited. The wastewater concentrated in the low-pressure reverse osmosis membrane module 110 is introduced into the medium-pressure reverse osmosis membrane module 120 through the flow path 2b. The medium-pressure reverse osmosis membrane module 120 further concentrates the wastewater concentrated in the low-pressure reverse osmosis membrane module 110. The wastewater concentrated in the medium-pressure reverse osmosis membrane module 120 is introduced into the high-pressure reverse osmosis membrane module 130 through the flow path 2c. The high-pressure reverse osmosis membrane module 130 further concentrates the wastewater concentrated in the medium-pressure reverse osmosis membrane module 120.

[0101] The permeate outlet of the low-pressure reverse osmosis membrane module 110, the permeate outlet of the medium-pressure reverse osmosis membrane module 120, and the permeate outlet of the high-pressure reverse osmosis membrane module 130 are connected to the flow path 4a, the flow path 4b, and the flow path 4c, respectively. The permeate water is supplied to a factory or the like through the flow path 4a, the flow path 4b, and the flow path 4c for reuse.

[0102] The water treatment system 100 also includes an ultra-high pressure reverse osmosis membrane module 140, a nanofiltration membrane module 150, and an ultra-high pressure reverse osmosis membrane module 160. The ultra-high pressure reverse osmosis membrane module 140 and the ultra-high pressure reverse osmosis membrane module 160 operate at a supply pressure higher than that of the high pressure reverse osmosis membrane module 130. The flow path 2d is connected to the concentrated water outlet of the high pressure reverse osmosis membrane module 130 and the inlet of the ultra-high pressure reverse osmosis membrane module 140. The flow path 2e is connected to the concentrated water outlet of the high pressure reverse osmosis membrane module 130 and the inlet of the nanofiltration membrane module 150. The flow path 2f is connected to the concentrated water outlet of the ultra-high pressure reverse osmosis membrane module 140. The flow path 2g is connected to the concentrated water outlet of the nanofiltration membrane module 150. The flow path 2h is connected to the permeate water outlet of the nanofiltration membrane module 150 and the inlet of the ultra-high pressure reverse osmosis membrane module 160.

[0103] The wastewater concentrated in the high-pressure reverse osmosis membrane module 130 is introduced into the ultra-high-pressure reverse osmosis membrane module 140 through the flow path 2d. The ultra-high-pressure reverse osmosis membrane module 140 further concentrates the wastewater concentrated in the high-pressure reverse osmosis membrane module 130. The wastewater concentrated in the high-pressure reverse osmosis membrane module 130 is introduced into the nanofiltration membrane module 150 through the flow path 2e. The nanofiltration membrane module selectively removes divalent ions from the wastewater concentrated in the high-pressure reverse osmosis membrane module 130. The permeated water of the nanofiltration membrane module 150 is introduced into the ultra-high-pressure reverse osmosis membrane module 160 through the flow path 2h. The ultra-high-pressure reverse osmosis membrane module 160 further filters the permeated water filtered in the nanofiltration membrane module 150.

[0104] The permeate outlet of the ultra-high pressure reverse osmosis membrane module 140 and the permeate outlet of the ultra-high pressure reverse osmosis membrane module 160 are connected to the flow path 4d and the flow path 4e, respectively. The permeate water is supplied to the factory and the like through the flow path 4d and the flow path 4e for reuse. The concentrated water is sent to the electrolysis device, evaporator and the like for post-processing through the flow path 2f, the flow path 2i and the flow path 2g.

[0105] In each flow path of the water treatment system 100 , a pump, a valve, a sensor, etc. are arranged as necessary.

[0106] It should be noted that the “supply pressure” refers to the pressure applied to the raw water near the inlet of the module. The vicinity of the inlet of the module is, for example, the space between the element located most upstream in the module and the flow path.

[0107] [Example]

[0108] (Manufacturing Example 1: Manufacturing Example of Composite Semipermeable Membrane)

[0109] An amine aqueous solution was prepared by mixing 3.0 mass % of m-phenylenediamine, 0.15 mass % of sodium dodecyl sulfate, 2.15 mass % of triethylamine, 0.31 mass % of sodium hydroxide, 6 mass % of camphorsulfonic acid and 1 mass % of isopropanol. The amine aqueous solution was applied to a polysulfone porous support membrane formed on a polyester nonwoven fabric. Then, an amine-containing layer was formed by removing excess amine aqueous solution. On the other hand, an acid chloride solution was prepared by dissolving 0.20 mass % of trimesoyl chloride in a cycloalkane solvent (manufactured by ExxonMobil, Exxsol D40). The surface of the amine-containing layer was immersed in the acid chloride solution for 7 seconds. Then, the excess acid chloride solution was removed. Thus, an interfacial polymerization reaction was carried out to form a surface layer. The surface layer was air-dried for 20 seconds and then heated in a hot air dryer at 140°C for 3 minutes. After these steps, a composite semipermeable membrane having a nonwoven fabric substrate, a polysulfone porous support membrane and a polyamide surface layer was obtained in sequence.

[0110] A polyvinyl alcohol aqueous solution containing polyvinyl alcohol (PVA) at a concentration of 0.165 mass % (saponification degree of 99% or more, viscosity of 4 mass % solution of 62.0 mPa·s to 72.0 mPa·s (25°C)) was prepared. The surface of the composite semipermeable membrane was contacted with the polyvinyl alcohol aqueous solution for 10 seconds. Then, the composite semipermeable membrane was air-dried for 30 seconds and then heated in a hot air dryer at 120°C for 2 minutes. Thus, a composite semipermeable membrane of Manufacturing Example 1 having a PVA coating was obtained.

[0111] (Calculation of elastic modulus of membrane surface based on force curve measured by AFM in water)

[0112] Figure 5 Figure 1 is a diagram for explaining the method of measuring the force curve using AFM in water. The elastic modulus of the membrane surface of the composite semipermeable membrane of Manufacturing Example 1 was measured by the following method. First, the composite semipermeable membrane of Manufacturing Example 1 was cut into a size of 2 cm×2 cm to obtain a sample piece 101. Then, as Figure 5 As shown, a sample piece 101 is fixed on a glass plate 104 of a fixed jig for in-liquid measurement (Closed Fluid Cell) manufactured by Asylum Technology, a fixed pin 102 and a pressing plate 103. Then, about 100 μL of ultrapure water 105 is dropped on the sample piece 101.

[0113] The sample piece 101 is moved in the vertical direction, and the spherical probe 106 is pressed into the surface of the sample piece 101 while applying a load, and then the spherical probe 106 is separated from the sample piece 101. The deflection or warping (displacement) of the cantilever 107 when the spherical probe 106 is separated from the sample piece 101 is detected by a photodiode in the form of displacement of the laser 108, thereby measuring the force curve. The force curve is converted into the load and the deformation of the membrane surface using the program attached to the device. The force curve is measured in an area of ​​5μm×5μm and at any 5 points. Then, the elastic modulus is calculated by fitting with the Heltz model using the analysis software attached to the device.

[0114] ·Measurement device: MFP-3D-SA (manufactured by Asylum Technology)

[0115] Cantilever: Spring constant 40N / m

[0116] Spherical probe: manufactured by Nanosensor, with a tip radius of curvature of 0.4 μm, silicon (100), Poisson’s ratio of 0.17, and elastic modulus of 150 GPa

[0117] ·Measurement environment: in ultrapure water (28℃~30℃)

[0118] ·Pressing speed, separation speed: 1Hz

[0119] ·Number of measurements: 5

[0120] Elastic modulus E of the membrane surface of the composite semipermeable membrane of Production Example 1 样品 (MPa) The elastic modulus was obtained by substituting each value into the following Hertz elastic contact theory formula and using the attached software. The obtained elastic modulus was 340 MPa.

[0121] (Hertz elastic contact theory formula)

[0122] h=[3 / 4[{(1-ν 探针 2 ) / E 探针}+{(1-ν 样品 2 ) / E 样品}]] 2 / 3 F 2 / 3 r -1 / 3

[0123] h: Deformation of the membrane surface (average value)

[0124] ν 探针 : Poisson's ratio of the probe is 0.17

[0125] ν 样品: Poisson's ratio of the sample piece is 0.33 (0.33 is used as the representative value (fixed value) of the resin)

[0126] E 探针 : Elastic modulus of the probe 150GPa

[0127] E 样品 : Elastic modulus of the specimen (MPa)

[0128] F: Any

[0129] r: The tip curvature radius of the probe is 10 nm

[0130] (Manufacturing Example 2: Manufacturing Example of Composite Semipermeable Membrane)

[0131] A composite semipermeable membrane of Production Example 2 was produced by the same method as Production Example 1 except that a betaine polymer (manufactured by Osaka Organic Chemical Industry Co., Ltd., LAMBIC-1100W) was used instead of PVA.

[0132] (Manufacturing Example 3: Manufacturing Example of Composite Semipermeable Membrane)

[0133] In addition to using PEOX (poly (2-ethyl-2- A composite semipermeable membrane of Production Example 3 was produced by the same method as Production Example 1 except that PVA was replaced with oxazoline).

[0134] (Manufacturing Example 4: Manufacturing Example of Composite Semipermeable Membrane)

[0135] A composite semipermeable membrane of Production Example 4 was produced by the same method as Production Example 1 except that PVA coating was not performed.

[0136] [Turn on / off test]

[0137] The composite semipermeable membrane and the permeate side flow path material were placed in a pressure-resistant container, and the initial NaCl retention rate was measured by the method described above. Then, the process of continuously supplying pressurized reverse osmosis water (25°C) for 90 seconds and the process of stopping the supply of reverse osmosis water were repeated 7000 times. After repeating this 7000 times, the NaCl retention rate was measured.

[0138] (Samples 1 to 4)

[0139] An opening / closing test was performed using the composite semipermeable membrane obtained in Production Example 1, the permeation side flow path material shown in Table 1, and the supply pressure shown in Table 1. The results are shown in Table 1. The permeation side flow path material was laminated on the composite semipermeable membrane in such a manner that the surface (rough surface) having the convex portion of the coil longitudinal row was in contact with the surface of the polyester nonwoven fabric of the composite semipermeable membrane.

[0140] (Sample 5)

[0141] An opening / closing test was carried out using the composite semipermeable membrane obtained in Production Example 2, the permeate-side flow path materials shown in Table 1, and the supply pressures shown in Table 1. Table 1 shows the results.

[0142] (Sample 6)

[0143] An opening / closing test was carried out using the composite semipermeable membrane obtained in Production Example 3, the permeate-side flow path materials shown in Table 1, and the supply pressures shown in Table 1. Table 1 shows the results.

[0144] (Samples 7 and 8)

[0145] An opening / closing test was carried out using the composite semipermeable membrane obtained in Production Example 4, the permeate-side flow path materials shown in Table 1, and the supply pressures shown in Table 1. Table 1 shows the results.

[0146] (Sample 9)

[0147] An opening / closing test was carried out using the composite semipermeable membrane obtained in Production Example 1, the permeate-side flow path materials shown in Table 1, and the supply pressures shown in Table 1. Table 1 shows the results.

[0148] [Table 1]

[0149]

[0150] It can be understood from the results of Sample 1 and Sample 7 that the difference in salt retention rate before and after the opening / closing test of the combination of Sample 1 is smaller than the difference in salt retention rate before and after the opening / closing test of the combination of Sample 7. That is, the combination of Sample 1 is excellent in durability against opening / closing of water pressure. The combination of Sample 1 can be said to be suitable for a system that is frequently opened / closed and repeated like the ZLD system.

[0151] It can be understood from the results of Samples 1 and 2 that when the supply pressure is increased, the degree of reduction in the salt interception rate also increases. However, it can be understood from the results of Samples 2 and 8 that the difference in the salt interception rate before and after the opening / closing test of the combination of Sample 2 is smaller than the difference in the salt interception rate before and after the opening / closing test of the combination of Sample 8. That is, the combination of Sample 2 is excellent in durability against opening / closing of water pressure. It can be said that the combination of Sample 2 is suitable for a system that is frequently opened and closed repeatedly, such as the ZLD system.

[0152] According to the results of Samples 3 and 4, it can be understood that by increasing the knitting density of the permeable side flow path material, the durability of opening / closing to water pressure is improved. In particular, as shown in Sample 4, even if the opening / closing test is performed at a relatively high supply pressure (4.0 MPa), by using the permeable side flow path material with an appropriate knitting density, the reduction in salt retention rate caused by the opening / closing test can be greatly suppressed. This shows that the synergistic effect of the effect brought by the composite semipermeable membrane and the effect brought by the permeable side flow path material is obtained. The combination of Samples 3 and 4 can be said to be suitable for a system such as the ZLD system that is frequently and repeatedly opened / closed.

[0153] The results of Samples 5 and 6 suggest that good results can be obtained even if the coating material is changed.

[0154] In Sample 9, since the supply pressure was too high, the decrease in the salt retention rate before and after the opening / closing test was large.

[0155] [Observation of membrane surface after opening / closing test]

[0156] After the opening / closing test, the membrane surface of the composite semipermeable membrane of sample 1, sample 3 and sample 7 was observed. Specifically, a dye (manufactured by Tokyo Chemical Industry Co., Ltd., basic violet 1) was used to prepare a dye solution with a concentration of 160 mg / L. The composite semipermeable membrane was pressurized at 1.5 MPa and the dye solution was passed for 10 minutes. The composite semipermeable membrane after the dye solution was passed was cleaned with reverse osmosis water, dried at room temperature, and then a digital microscope (manufactured by Keyence Corporation, VHX 6000) was used to observe the membrane surface at a magnification of 50 times. The results are shown in Fig. 6A , Figure 6B and Figure 6C middle.

[0157] Fig. 6A This is an optical microscope image of the composite semipermeable membrane of sample 1 after staining. Figure 6B This is an optical microscope image of the composite semipermeable membrane of sample 3 after staining. Figure 6C This is an optical microscope image of the composite semipermeable membrane of sample 7 after staining. Fig. 6A , Figure 6B and Figure 6C In the figure, the dark part is a part where defects occur and the dye penetrates in. The bright part is a part where the dye penetrates less and there are fewer defects.

[0158] like Fig. 6A As shown in FIG. 1 , the composite semipermeable membrane of sample 1 has few defects. A small number of defects are generated parallel to the longitudinal direction of the coil. Figure 6B As shown in FIG. 1 , almost no defects are generated in the composite semipermeable membrane of sample 3. Figure 6CAs shown, significant defects were generated in the composite semipermeable membrane of Sample 7 along the longitudinal direction of the coils.

[0159] Industrial Applicability

[0160] The invention can be used in wastewater treatment systems such as ZLD systems.

Claims

1. A composite semipermeable membrane, wherein: The composite semipermeable membrane comprises a porous support membrane, a surface layer supported by the porous support membrane, and a coating layer covering the surface layer. The surface layer is made of polyamide, The coating comprises a polymer, The polymer comprises a polymer selected from the group consisting of polyvinyl alcohol, betaine polymer and poly At least one of the group consisting of oxazoline, The elastic modulus of the membrane surface calculated by force curve measurement using AFM in water is 250 MPa or more and 500 MPa or less, The composite semipermeable membrane is used in a zero liquid discharge system.

2. A spiral membrane element, wherein: The spiral membrane element has the composite semipermeable membrane according to claim 1.

3. The spiral membrane element according to claim 2, wherein: The spiral membrane element further comprises a permeate side flow path material, wherein the permeate side flow path material comprises a warp knitted fabric having a knitting density of 31 to 60 wales and 34 to 52 rows, and The composite semipermeable membrane is in contact with the permeate-side flow path material.

4. A water treatment system, wherein: The water treatment system comprises the spiral membrane element according to claim 2 or 3, and the water treatment system is a zero liquid discharge system.

5. The water treatment system according to claim 4, wherein: The water treatment system comprises: Low pressure reverse osmosis membrane module; A medium-pressure reverse osmosis membrane module, wherein the medium-pressure reverse osmosis membrane module further concentrates the wastewater concentrated by the low-pressure reverse osmosis membrane module; and A high-pressure reverse osmosis membrane module, wherein the high-pressure reverse osmosis membrane module further concentrates the wastewater concentrated by the medium-pressure reverse osmosis membrane module, and The medium-pressure reverse osmosis membrane module comprises the spiral membrane element according to claim 2 or 3.

6. A method for treating water, wherein: The water treatment method comprises the following steps: A process for concentrating wastewater using a low-pressure reverse osmosis membrane module; A step of further concentrating the wastewater concentrated by the low-pressure reverse osmosis membrane module by using a medium-pressure reverse osmosis membrane module; and The process of further concentrating the wastewater concentrated by the medium-pressure reverse osmosis membrane module by using a high-pressure reverse osmosis membrane module, The water treatment method is a water treatment method applied to a zero liquid discharge system. The medium-pressure reverse osmosis membrane module comprises the spiral membrane element according to claim 2 or 3, The supply pressure of the low-pressure reverse osmosis membrane module is lower than the supply pressure of the medium-pressure reverse osmosis membrane module. The supply pressure of the medium-pressure reverse osmosis membrane module is lower than the supply pressure of the high-pressure reverse osmosis membrane module, and The supply pressure of the medium-pressure reverse osmosis membrane module is greater than or equal to 2.0 MPa and less than or equal to 4.0 MPa.

Citation Information

Patent Citations

  • Semipermeable composite membrane, spiral separation membrane element, and method for producing same

    CN106999865A

  • Quaternary phosphonium salt antibacterial polyamide water treatment membrane and preparation method thereof

    CN112121646A

  • Surface treatment wastewater zero discharge system

    CN209493453U

  • Spiral membrane element

    EP3199225A1

  • Spiral membrane element

    EP3417928A1