A high-toughness polyphenylene sulfide-based composite material suitable for harsh oil lubrication conditions and a preparation method thereof
By adding polyarylene ether nitrile resin and functional nanofillers to polyphenylene sulfide materials, combined with reinforced fibers and solid lubricants, the brittleness and wear resistance of pure polyphenylene sulfide materials under harsh oil lubrication conditions are solved. Problem, high toughness composite materials were prepared, which significantly improved the tribological properties and heat resistance.
Patent Information
- Application Number
- CN202211705213.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-29
- Publication Date
- 2024-10-08
- Estimated Expiration
- 2042-12-29
AI Technical Summary
The application of pure polyphenylene sulfide materials in high-end equipment suffers from the problems of high brittleness, poor toughness, and insufficient wear resistance, especially insufficient tribological properties under harsh oil lubrication conditions, and there is a lack of effective solutions.
Polyphenylene sulfide resin and polyaryl ether nitrile resin are used as matrix materials, combined with reinforced fibers, solid lubricants and functional nanofillers, to prepare high-toughness composite materials through molding and extrusion injection molding processes. The formula and process are optimized to improve the material's durability. Toughness and tribological properties.
It significantly improves the toughness and tribological properties of the material, reduces the wear rate, enhances the heat resistance and service life in high temperature environments, and is suitable for harsh oil lubrication conditions.
Smart Images

Figure BDA0004026127110000051
Abstract
Description
Technical Field
[0001] The invention relates to the field of engineering materials, and in particular to a high-toughness polyphenylene sulfide-based composite material suitable for harsh oil lubrication conditions and a preparation method thereof. Background Art
[0002] With the continuous development of industrial technology, the service life of transmission parts is constantly extended, and higher requirements are placed on the mechanical and tribological properties of mechanical wear-resistant parts. The design and development of materials with excellent self-lubricating properties and wear resistance has gradually become a research hotspot in various countries. Polymer composites are widely used in various fields such as automobiles, wind power, and military due to their advantages such as light weight, high chemical stability, and strong designability.
[0003] Polyphenylene sulfide (PPS) is a crystalline heat-resistant polymer material with a simple chemical structure composed of benzene rings and sulfur. The resin has a melting point of about 280°C and a long-term use temperature of up to 220°C to 240°C. As one of the special engineering plastics, it is widely used in the fields of electronics, electrical appliances, automobiles, aerospace, etc. In addition, compared with special plastics such as polyetheretherketone (PEEK) and polyimide (PI), its low cost advantage attracts widespread attention. However, pure PPS products have high brittleness, poor toughness, insufficient rigidity and strength, and poor wear resistance, which limits its application in high-end equipment lubricating materials. Studies have shown that PPS can be used to toughen and plasticize polyarylethernitrile (PEN). When PPS is used as a filler and the mass fraction reaches 15%, PEN / PPS exhibits good processing fluidity and heat resistance [Engineering Plastics Application, 2009, 37(12):4-7]. However, there are few public reports on PEN toughened PPS (PPS as matrix material, PEN as filler) to explore the mechanical properties of the composite materials and the tribological properties under harsh oil lubrication conditions. Summary of the invention
[0004] The object of the present invention is to provide a high-toughness polyphenylene sulfide-based composite material suitable for harsh oil lubrication conditions and a preparation method thereof.
[0005] The high-toughness polyphenylene sulfide-based composite material suitable for harsh oil lubrication conditions described in the present invention is characterized in that the composite material includes, in terms of mass fractions, 100 parts of polyphenylene sulfide resin and polyarylether nitrile resin as a matrix material (the mass ratio of the two is 1.5 to 9), 12-55 parts of reinforcing fiber, 6-18 parts of solid lubricant and 1-9 parts of functional nanofiller, etc.
[0006] The polyphenylene sulfide resin is in the form of powder or granules. The powder is used for compression molding, and the granules are used for extrusion injection molding.
[0007] The polyarylethernitrile resin is in the form of powder or granules. The powder is used for compression molding, and the granules are used for extrusion injection molding.
[0008] The reinforcing fiber is any one of carbon fiber, aramid fiber, glass fiber and titanate whisker fiber. The molding process uses ground powder and the extrusion injection molding process uses chopped fiber.
[0009] The solid lubricant is polytetrafluoroethylene, and the average particle size is between 50 μm and 200 μm.
[0010] The functional nano filler is any one of nano alumina, nano titanium dioxide and nano zirconium dioxide, and the average particle size is between 10nm and 100nm.
[0011] The method for preparing a high-toughness polyphenylene sulfide-based composite material suitable for harsh oil lubrication conditions is characterized by:
[0012] (1) Molding process: weigh the raw materials according to different ratios and fully dry them in a blast drying oven; mix the fully dried polyphenylene sulfide powder, polyarylether nitrile powder, reinforcing fiber grinding powder, solid lubricant, and functional nanofiller in a high-speed mixer to ensure that the materials are evenly mixed; put them into a mold and transfer them to a flat vulcanizer, set the temperature to 300°C, keep warm for 1 hour, and set the pressure to 15 MPa.
[0013] (2) Extrusion injection molding process: weigh the raw materials according to different ratios and fully dry them in a blast drying oven; feed the fully dried polyphenylene sulfide pellets and polyarylether nitrile pellets through the main feeding port, the reinforcing fiber through the side feeding port, and the solid lubricant and functional nanofiller through the powder feeding port. The temperature of the twin-screw extruder / injection molding machine 1 to 4 zones is 290-300-320-330°C, the extruder screw speed is 350rpm, the injection pressure of the injection molding machine is 90MPa, the back pressure is 3MPa, and the mold temperature is 150°C.
[0014] The present invention has the advantages that:
[0015] The present invention improves the shortcomings of pure polyphenylene sulfide in actual application conditions, such as poor toughness and brittleness. On the basis of improving the toughness of the material, the formulation is optimized to design and prepare a high-toughness polyphenylene sulfide-based self-lubricating wear-resistant material suitable for use in harsh oil lubrication conditions; in addition, toughening agents such as ethylene methyl acrylate copolymer, maleic anhydride grafted styrene-ethylene-butadiene-styrene block copolymer elastomer and the like will lose the thermal stability of the polyphenylene sulfide composite material itself, while by adding a polyarylether nitrile resin with a similar heat deformation temperature and melting point, the composite material exhibits better heat resistance, so that the prepared material can be better used in a high-temperature environment, thereby improving the service life and reliability of the pairing. DETAILED DESCRIPTION
[0016] The present invention is further described below by means of specific examples, but the examples are not intended to limit the present invention. All similar methods and similar variations of the present invention should be included in the protection scope of the present invention.
[0017] Example 1 A high-toughness polyphenylene sulfide-based composite material suitable for harsh oil lubrication conditions
[0018] According to the mass ratio, a certain amount of polyphenylene sulfide resin and polyarylether nitrile resin powder was weighed as 100 parts of matrix material (60 parts of polyphenylene sulfide, 40 parts of polyarylether nitrile), 55 parts of carbon fiber powder, 18 parts of polytetrafluoroethylene (average particle size 50μm) and 9 parts of nano-alumina (average particle size 10nm). After being fully dried in a blast drying oven, a high-speed stirrer was used to mix the materials to ensure that the materials were evenly mixed; put them into a mold, transferred to a flat vulcanizer, set the temperature to 300℃, keep warm for 1h, and set the pressure to 15MPa. Cool to room temperature to obtain a block material, and then investigate its tribological properties.
[0019] Example 2 A high-toughness polyphenylene sulfide-based composite material suitable for harsh oil lubrication conditions
[0020] According to the mass ratio, a certain amount of polyphenylene sulfide resin and polyarylether nitrile resin pellets were weighed as 100 parts of matrix material (60 parts of polyphenylene sulfide, 40 parts of polyarylether nitrile), 55 parts of chopped carbon fiber, 18 parts of polytetrafluoroethylene (average particle size 50μm) and 9 parts of nano-alumina (average particle size 10nm). Fully dried in a blast drying oven; the fully dried polyphenylene sulfide pellets and polyarylether nitrile pellets were passed through the main feeding port, the carbon fiber was passed through the side feeding port, and the polytetrafluoroethylene and nano-alumina were passed through the powder feeding port. The temperature of the twin-screw extruder / injection molding machine 1 to 4 zones was 290-300-320-330℃, the extruder screw speed was 350rpm, the injection pressure of the injection molding machine was 90MPa, the back pressure was 3MPa, and the mold temperature was 150℃. The sample was obtained by injection molding, and its mechanical properties and tribological properties were then investigated.
[0021] Example 3 A high-toughness polyphenylene sulfide-based composite material suitable for harsh oil lubrication conditions
[0022] According to the mass ratio, a certain amount of polyphenylene sulfide resin and polyarylether nitrile resin powder was weighed as 100 parts of the matrix material (80 parts of polyphenylene sulfide, 20 parts of polyarylether nitrile), 29 parts of carbon fiber powder, 12 parts of polytetrafluoroethylene (average particle size 100μm) and 4 parts of nano-titanium dioxide (average particle size 50nm). After being fully dried in a blast drying oven, a high-speed stirrer was used to mix the materials to ensure that the materials were evenly mixed; put them into a mold, transferred to a flat vulcanizer, set the temperature to 300℃, keep warm for 1h, and set the pressure to 15MPa. Cool to room temperature to obtain a block material, and then investigate its tribological properties.
[0023] Example 4 A high-toughness polyphenylene sulfide-based composite material suitable for harsh oil lubrication conditions
[0024] According to the mass ratio, a certain amount of polyphenylene sulfide resin and polyarylether nitrile resin pellets were weighed as 100 parts of matrix material (80 parts of polyphenylene sulfide, 20 parts of polyarylether nitrile), 29 parts of chopped carbon fiber, 12 parts of polytetrafluoroethylene (average particle size 100μm) and 4 parts of nano-titanium dioxide (average particle size 50nm). Fully dried in a blast drying oven; the fully dried polyphenylene sulfide pellets and polyarylether nitrile pellets were passed through the main feeding port, the carbon fiber was passed through the side feeding port, and polytetrafluoroethylene and nano-titanium dioxide were passed through the powder feeding port. The temperature of the twin-screw extruder / injection molding machine 1 to 4 zones was 290-300-320-330℃, the extruder screw speed was 350rpm, the injection pressure of the injection molding machine was 90MPa, the back pressure was 3MPa, and the mold temperature was 150℃. The sample was obtained by injection molding, and its mechanical properties and tribological properties were then investigated.
[0025] Example 5 A high-toughness polyphenylene sulfide-based composite material suitable for harsh oil lubrication conditions
[0026] According to the mass ratio, a certain amount of polyphenylene sulfide resin and polyarylether nitrile resin powder was weighed as 100 parts of matrix material (90 parts of polyphenylene sulfide, 10 parts of polyarylether nitrile), 12 parts of carbon fiber powder, 6 parts of polytetrafluoroethylene (average particle size 200μm) and 1 part of nano zirconium dioxide (average particle size 100nm). After being fully dried in a blast drying oven, a high-speed stirrer was used to mix the materials to ensure that the materials were evenly mixed; put them into a mold, transferred to a flat vulcanizer, set the temperature to 300℃, keep warm for 1h, and set the pressure to 15MPa. Cool to room temperature to obtain a block material, and then investigate its tribological properties.
[0027] Example 6 A high-toughness polyphenylene sulfide-based composite material suitable for harsh oil lubrication conditions
[0028] According to the mass ratio, a certain amount of polyphenylene sulfide resin and polyarylether nitrile resin pellets were weighed as 100 parts of matrix material (90 parts of polyphenylene sulfide, 10 parts of polyarylether nitrile), 12 parts of chopped carbon fiber, 6 parts of polytetrafluoroethylene (average particle size 200μm) and 1 part of nano zirconium dioxide (average particle size 100nm). Fully dried in a blast drying oven; the fully dried polyphenylene sulfide pellets and polyarylether nitrile pellets were passed through the main feeding port, the carbon fiber was passed through the side feeding port, and polytetrafluoroethylene and nano zirconium dioxide were passed through the powder feeding port. The temperature of the twin-screw extruder / injection molding machine 1 to 4 zones was 290-300-320-330℃, the extruder screw speed was 350rpm, the injection pressure of the injection molding machine was 90MPa, the back pressure was 3MPa, and the mold temperature was 150℃. The sample was obtained by injection molding, and its mechanical properties and tribological properties were then investigated.
[0029] Comparative Example 1: A polyphenylene sulfide material
[0030] According to the mass ratio, a certain amount of polyphenylene sulfide resin powder was weighed, 100 parts, fully dried in a blast drying oven, and mixed with a high-speed mixer to ensure that the materials were mixed evenly; put into a mold, transferred to a flat vulcanizer, set the temperature to 300°C, keep warm for 1h, and set the pressure to 15MPa. Cool to room temperature to obtain a block material, and then examine its tribological properties.
[0031] Comparative Example 2 A polyphenylene sulfide-based composite material
[0032] According to the mass ratio, a certain amount of polyphenylene sulfide resin pellets were weighed as 100 parts of matrix material, 55 parts of short carbon fiber, 18 parts of polytetrafluoroethylene (average particle size 50μm) and 9 parts of nano-alumina (average particle size 10nm). Fully dried in a blast drying oven; the fully dried polyphenylene sulfide pellets were passed through the main feeding port, the carbon fiber through the side feeding port, and the polytetrafluoroethylene and nano-alumina through the powder feeding port. The temperature of the twin-screw extruder / injection molding machine 1 to 4 zones was 290-300-320-330℃, the extruder screw speed was 350rpm, the injection pressure of the injection molding machine was 90MPa, the back pressure was 3MPa, and the mold temperature was 150℃. The sample was obtained by injection molding, and then its mechanical properties and tribological properties were investigated.
[0033] The present invention conducts friction tests on the above examples 1, 2, 3, 4, 5, 6 and comparative examples 1 and 2, using a high-speed ring-block tester for testing. The molded or extruded sample material is machined into 25×10×4 mm 3 The mating part is GCr15 bearing steel, and the test conditions are: load 100N, speed 0.1m / s, duration 2h, and the mating pair is immersed in a cavity filled with PAO oil. After the friction test, the wear scar width is measured using an optical microscope, and the wear rate is calculated using the formula.
[0034] The calculation formula of wear rate is:
[0035]
[0036] Wherein, L′ is the width of the specimen (mm), R is the diameter of the dual steel ring (mm), W is the width of the wear scar (mm), F is the normal force (N), and L is the sliding distance (m).
[0037] The present invention conducts mechanical property tests on the above Examples 2, 4, 6 and Comparative Example 2. According to the determination of impact properties of simply supported beams of plastics in GB / T1043-2018, the samples of the examples and comparative examples are processed into 80×10×4 mm 3 The mechanical impact properties of the embodiments and comparative examples were measured using a CJJX intelligent digital display controlled simple suspension combined impact testing machine.
[0038] The average friction coefficient and wear rate measurement and calculation results of the materials prepared in the examples of the present invention and the comparative examples are shown in Table 1. The impact strength measurement results of the materials prepared in the examples of the present invention and the comparative examples are shown in Table 2.
[0039] Table 1. Calculation results of average friction coefficient and wear rate of materials prepared in Examples and Comparative Examples
[0040] Friction coefficient <![CDATA[Wear rate (10 -6 mm 3 / Nm)]]> Example 1 0.11 3.21 Example 2 0.12 3.32 Example 3 0.15 4.51 Example 4 0.14 5.60 Example 5 0.14 4.64 Example 6 0.13 4.89 Comparative Example 1 0.30 40 Comparative Example 2 0.20 6.53
[0041] Table 2. Unnotched impact strength of materials prepared in Examples and Comparative Examples
[0042] <![CDATA[Izod impact strength (kJ / m 2 )]]> Example 2 35.8 Example 4 23.4 Example 6 20.7 Comparative Example 2 9.6
[0043] As can be seen from Table 1, the high-toughness polyphenylene sulfide-based composite material (Examples 1, 2, 3, 4, 5, 6) obtained by the present invention, which is suitable for harsh oil lubrication conditions, has significant friction reduction and anti-wear properties compared with pure polyphenylene sulfide resin and conventional wear-resistant modified polyphenylene sulfide composite materials (Comparative Examples 1 and 2), and the wear rate is greatly reduced compared with pure resin. As can be seen from Table 2, the toughness of the polyphenylene sulfide composite material modified by polyarylether nitrile is greatly improved compared with the unnotched impact strength without PEN toughening. Through reasonable formula design, a friction pair material with high toughness and excellent tribological properties under harsh oil lubrication conditions can be prepared.
Claims
1. A high-toughness polyphenylene sulfide-based composite material suitable for harsh oil lubrication conditions, characterized in that: The composite material comprises, by weight, 100 parts of polyphenylene sulfide resin and polyarylether nitrile resin as base materials, 12-55 parts of reinforcing fibers, 6-18 parts of solid lubricants, and 1-9 parts of functional nano fillers, wherein the mass ratio of the polyphenylene sulfide resin to the polyarylether nitrile resin is 1.5-9; the heat deformation temperature and melting point of the polyarylether nitrile resin are similar to those of the polyphenylene sulfide resin; The polyphenylene sulfide resin is in the form of powder or granules, the powder is used for compression molding, and the granules are used for extrusion injection molding; The polyarylethernitrile resin is in the form of powder or pellets, the powder is used for compression molding, and the pellets are used for extrusion injection molding; The reinforcing fiber is any one of carbon fiber, aramid fiber, glass fiber, and titanate whisker fiber, the grinding powder is used for the molding process, and the short-cut fiber is used for the extrusion injection molding process; The solid lubricant is polytetrafluoroethylene, and the average particle size is 50 μm to 200 μm; The functional nano filler is any one of nano alumina, nano titanium dioxide and nano zirconium dioxide, and has an average particle size of 10 nm to 100 nm.
2. The method for preparing the high-toughness polyphenylene sulfide-based composite material suitable for harsh oil lubrication conditions according to claim 1, characterized in that: The steps include: Molding process: weigh the raw materials according to different ratios and fully dry them in a blast drying oven; mix the fully dried polyphenylene sulfide powder, polyarylether nitrile powder, reinforcing fiber grinding powder, solid lubricant, and functional nanofiller in a high-speed mixer to ensure that the materials are evenly mixed; put them into the mold, transfer them to a flat vulcanizer, set the temperature to 300°C, keep them warm for 1 hour, and set the pressure to 15 MPa; Or: extrusion injection molding process, weigh the raw materials according to different ratios, and fully dry them in a blast drying oven; feed the fully dried polyphenylene sulfide pellets and polyarylether nitrile pellets through the main feeding port, the reinforcing fiber through the side feeding port, the solid lubricant and the functional nanofiller through the powder feeding port, and use a twin-screw extruder / injection molding machine with a temperature of 290-300-320-330°C in zones 1 to 4, a screw speed of 350 rpm, an injection pressure of 90 MPa, a back pressure of 3 MPa, and a mold temperature of 150°C.