Polyethylene
By using metallocene compound catalysts for polyethylene copolymerization in fiber production, the problems of polyethylene molecular weight distribution and dust generation are solved, and the high wear resistance and excellent fiber properties of polyethylene are achieved.
Patent Information
- Application Number
- CN202180057180.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2021-10-20
- Filing Date
- 2021-10-21
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-10-21
AI Technical Summary
In the fiber production, existing polyethylene has problems such as insufficient molecular weight distribution and excessive dust generation, resulting in insufficient wear resistance and affecting the quality and application of fibers.
Develop a polyethylene with a narrow molecular weight distribution and low crystallinity over a similar melt index range, increasing the effective physical crosslinking number of molecules and reducing fluff and dust during stretching produce.
It achieves excellent wear resistance of polyethylene and is suitable for the production of fiber products such as diapers, masks and medical fibers, improving the wear resistance and process yield of fibers.
Smart Images

Figure FDA0004907942910000021 
Figure FDA0004907942910000031 
Figure FDA0004907942910000041
Abstract
Description
Technical Field
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application is based on and claims the benefit of priority of Korean Patent Application Nos. 10-2020-0143717 and 10-2021-0140284, filed on October 30, 2020 and October 20, 2021, respectively, the disclosures of which are incorporated herein by reference in their entirety.
[0003] The present invention relates to a polyethylene. More particularly, the present invention relates to a polyethylene having excellent abrasion resistance and thus suitable for fiber production. Background Art
[0004] Olefin polymerization catalyst systems can be divided into Ziegler-Natta and metallocene catalyst systems, and these two highly active catalyst systems have been developed based on their characteristics. Since the development of Ziegler-Natta catalysts in the 1950s, they have been widely used in existing commercial processes. However, since Ziegler-Natta catalysts are multi-active site catalysts with a mixture of multiple active sites, they are characterized by a wide molecular weight distribution of the polymer. In addition, since the composition distribution of the comonomers is not uniform, there is a problem that there are limitations in ensuring the required physical properties.
[0005] In contrast, a metallocene catalyst is composed of a main catalyst whose main component is a transition metal compound and a cocatalyst whose main component is an organometallic compound whose main component is aluminum. This catalyst is a single-site catalyst, which is a homogeneous composite catalyst and provides a polymer having a narrow molecular weight distribution and a uniform composition distribution of the comonomer due to the characteristics of the single site.
[0006] On the other hand, polypropylene resin used as nonwoven material has excellent chemical resistance and tensile strength and is mainly used as surface material of sanitary products such as diapers, sanitary napkins, etc. However, homopolypropylene resin has a disadvantage of imparting a rough feeling on the surface of nonwoven fabric because it generally has a low content of low molecular weight copolymers and low xylene solubility.
[0007] In order to improve the texture of the surface, a bi-component fiber using polypropylene resin inside and polyethylene resin outside is produced by mixing polypropylene resin with polyethylene resin, which is used as a non-woven material with improved texture and softness. In addition, in order to provide convenience to users by improving the texture and softness of non-woven fabrics, the thickness of the spun yarn used is reduced.
[0008] Therefore, in order to ensure excellent tensile strength and softness in the process of preparing polyethylene for bicomponent fibers, there is a further need to develop polyethylene having a narrow molecular weight distribution and reduced dust generation. Summary of the invention
[0009] In order to solve the above problems in the prior art, a polyethylene is provided, which has a narrow molecular weight distribution and a low crystallinity within a similar melt index (MI) range, thereby having an increased number of effective physical crosslinks of molecules, and having reduced fuzz and dust generation during stretching, thereby having improved wear resistance.
[0010] In order to achieve the above object, a polyethylene satisfying the following conditions 1) to 4) is provided:
[0011] 1) a melt index (MI) of 0.5 to 40 g / 10 min as measured at 190° C. under a load of 2.16 kg according to ASTM D1238;
[0012] 2) molecular weight distribution (MWD) of 2.3 to 2.6;
[0013] 3) a crystallinity of 63% to 71% as measured using a differential scanning calorimeter (DSC) in accordance with ASTM F2625; and
[0014] 4) Crystal relaxation temperature (T) measured using dynamic mechanical analysis (DMA) cr ) is 42°C to 50°C.
[0015] According to the present invention, there is provided a polyethylene having a narrow molecular weight distribution and a low crystallinity, thereby having an increased number of effective physical crosslinks of molecules and having improved wear resistance, compared with existing polyethylenes having a similar melt index (MI).
[0016] Furthermore, the polyethylene of the present invention has reduced fuzz or dust generation during the stretching process and thus also has improved abrasion resistance.
[0017] Therefore, the polyethylene of the present invention can be effectively applied to the production of fiber products such as diapers, masks, various sanitary materials, medical fibers and other general consumer products. DETAILED DESCRIPTION
[0018] In the present invention, the terms "first", "second", etc. are used to describe various components, and these terms are only used to distinguish one component from other components.
[0019] In addition, the terms used in this description are only for explaining exemplary embodiments, and are not intended to limit the present invention. A singular expression may include a plural expression unless there is a different expression in the context. It must be understood that the terms "including", "equipped with" or "having" in this description are only used to indicate the presence of a feature, number, step, component or combination thereof that is active, and do not exclude the presence or possibility of adding one or more different features, numbers, steps, components or combinations thereof in advance.
[0020] The present invention can be modified in various ways and in various forms, and specific exemplary embodiments will be described and explained in detail below. However, it is not intended to limit the present invention to specific exemplary embodiments, and it must be understood that the present invention includes every modification, equivalent or substitute included in the spirit and technical scope of the present invention.
[0021] Hereinafter, the polyethylene of the present invention will be described in detail.
[0022] The polyethylene according to one embodiment of the present invention is characterized in that the following conditions 1) to 4) are satisfied: 1) a melt index (MI) of 0.5 g / 10 min to 40 g / 10 min measured at 190° C. under a load of 2.16 kg according to ASTM D1238; 2) a molecular weight distribution (MWD) of 2.3 to 2.6; 3) a crystallinity of 63% to 71% measured using a differential scanning calorimeter (DSC) according to ASTM F2625; and 4) a crystal relaxation temperature (T ) of 60° to 80° C. measured using dynamic mechanical analysis (DMA). cr ) is 42°C to 50°C.
[0023] In the preparation of polyethylene used in bicomponent fibers in which a polypropylene resin is used for the inner portion and a polyethylene resin is used for the outer portion, it is necessary to develop a polyethylene having a narrow molecular weight distribution and reduced dust generation to ensure excellent tensile strength and softness.
[0024] On the other hand, in the preparation process of polyethylene fiber, when the low molecular weight components in polyethylene are reduced, polymer chain entanglement occurs more effectively, so that wear resistance tends to improve. Therefore, since the low molecular weight components are smaller and the molecular weight distribution is narrower, better wear resistance can be obtained. However, when the low molecular weight components are too small, the filterability during the fiber spinning process will deteriorate, resulting in single yarn and entangled yarn, and there is a problem of reduced surface uniformity of the fiber.
[0025] Since the crystal relaxation temperature, which represents the strength and uniformity of the polyethylene crystal structure, is low and brittle, the generation of fuzz or dust can be reduced during fiber drawing, and the wear resistance of the final fiber product can be increased. Therefore, even between polyethylenes with similar molecular weight distributions, the wear resistance can vary greatly depending on the crystal relaxation temperature.
[0026] Hereinafter, the polyethylene of the present invention will be described in more detail.
[0027] 1) Melt Index (MI)
[0028] The polyethylene according to one embodiment of the present invention has a melt index (MI) of 0.5 to 40 g / 10 min, measured at 190° C. under a load of 2.16 kg according to ASTM D1238.
[0029] More specifically, according to one embodiment of the present invention, the melt index (MI) of the polyethylene can be 0.5 g / 10 min or more, or 1.0 g / 10 min or more, or 5 g / 10 min or more, or 10 g / 10 min or more, or 15 g / 10 min or more, or 18 g / 10 min or more, and 40 g / 10 min or less, or 35 g / 10 min or less, or 30 g / 10 min or less, or 25 g / 10 min or less, or 20 g / 10 min or less.
[0030] By having the above melt index, the molecular weight and viscosity of the polyethylene can be optimized, and the spinnability can be improved during fiber production.
[0031] 2) Molecular weight distribution (MWD)
[0032] The molecular weight distribution (MWD, Mw / Mn) of the polyethylene according to one embodiment of the present invention is 2.3 to 2.6.
[0033] More specifically, the molecular weight distribution of the polyethylene according to one embodiment of the present invention may be 2.3 or more, or 2.35 or more, or 2.4 or more, and 2.6 or less, or 2.55 or less, or 2.5 or less, or 2.45 or less.
[0034] Since the polyethylene of the present invention has a narrower molecular weight distribution relative to a high melt index, polymer chain entanglement can occur more effectively, and thus abrasion resistance can be improved.
[0035] In the present invention, regarding the number average molecular weight (Mn), weight average molecular weight (Mw) and molecular weight distribution, the weight average molecular weight (Mw) and number average molecular weight (Mn) of polyethylene are measured by gel permeation chromatography (GPC), respectively, and the ratio of the weight average molecular weight to the number average molecular weight (Mw / Mn) is calculated as the molecular weight distribution.
[0036] In detail, the polyethylene samples were evaluated using a Polymer Laboratories PLgel MIX-B column with a column length of 300 mm and a Waters PL-GPC220 instrument. The evaluation temperature was 160°C, 1,2,4-trichlorobenzene was used as the solvent, and the flow rate was set to 1 mL / min. The sample was prepared at a concentration of 10 mg / 10 mL and the injection volume was 200 μL. The Mw and Mn values were measured using a calibration curve formed using polystyrene standards. Nine polystyrene standards with weight average molecular weights of 2,000 / 10,000 / 30,000 / 70,000 / 200,000 / 700,000 / 2,000,000 / 4,000,000 / 10,000,000 were used.
[0037] 3) Crystallinity
[0038] The polyethylene according to one embodiment of the present invention has a crystallinity of 63% to 71% as measured using a differential scanning calorimeter (DSC) according to ASTM F2625.
[0039] More specifically, the crystallinity of the polyethylene according to one embodiment of the present invention may be 63% or more, or 65% or more, or 68% or more, and 71% or less, or 70% or less, or 69% or less.
[0040] Crystallinity is an index showing the thermal properties of polyethylene. Since the polyethylene of the present invention has a lower crystallinity than the above-mentioned high melt index, the number of effective physical crosslinks of the molecules increases, and therefore the polyethylene can show better wear resistance.
[0041] For the method of measuring crystallinity, reference may be made to ASTM F2625, which will be described in detail in the examples described later.
[0042] 4) Crystal relaxation temperature (T cr )
[0043] The crystal relaxation temperature (T) of the polyethylene according to one embodiment of the present invention measured using dynamic mechanical analysis (DMA) is cr ) is 42°C to 50°C.
[0044] More specifically, the crystal relaxation temperature (T cr ) can be above 42°C, or above 43°C, or above 44°C, and below 50°C, or below 49°C, or below 48°C, or below 47°C.
[0045] The crystal relaxation temperature is an index that can predict the strength and uniformity of the polyethylene crystal structure. Since the polyethylene of the present invention has a lower crystal relaxation temperature than the above-mentioned high melt index, the brittleness is reduced during the stretching process, thereby reducing the generation of fluff or dust. Therefore, the fiber including the polyethylene of the present invention can show excellent wear resistance.
[0046] The crystal relaxation temperature can be measured by dynamic mechanical analysis (DMA), and will be described in detail in the examples described below.
[0047] The method of measuring the crystal relaxation temperature will be described in detail in the examples described later.
[0048] 5) Wear resistance
[0049] The abrasion resistance of the polyethylene of the present invention measured according to ASTM D5264 is 0.2 mg / cm 3 the following.
[0050] More specifically, the wear resistance of the polyethylene according to one embodiment of the present invention may be 0.1 mg / cm 3 Above, or 0.11mg / cm 3 Above, or 0.12mg / cm 3 Above, and 0.2mg / cm 3 Below, or 0.18mg / cm 3 Below, or 0.16mg / cm 3 Below, or 0.14mg / cm 3 the following.
[0051] As described above, the polyethylene of the present invention has excellent wear resistance and can therefore be effectively applied to the production of fiber products such as diapers, masks, various sanitary materials, medical fibers, and other general consumer products.
[0052] The method for measuring the wear resistance will be described in detail in the examples described later.
[0053] 6) Other physical properties
[0054] The melt flow rate ratio (MFRR, MI5 / MI6) of the polyethylene according to one embodiment of the present invention is 2.16 ) is preferably 2 to 3.
[0055] MFRR is the melt index (MI5) of polyethylene measured at 190°C under a 5 kg load according to ASTM D1238 divided by the melt index (MI5) measured at 190°C under a 2.16 kg load according to ASTM D1238. 2.16 ) to obtain the value.
[0056] More specifically, the melt flow rate ratio (MFRR) of the polyethylene measured at 190° C. according to ASTM D1238 may be 2.2 or more, or 2.3 or more, or 2.4 or more, or 2.5 or more, and 2.90 or less, or 2.85 or less, or 2.7 or less, or 2.56 or less.
[0057] Since the polyethylene has the melt flow rate ratio in the above narrow range, the polyethylene of the present invention can achieve excellent filterability and improved process yield.
[0058] In addition, the polyethylene may satisfy a density (ASTM D1505, 23°C) of 0.945 g / cm 3 Up to 0.965g / cm 3 of high-density polyethylene (HDPE).
[0059] More specifically, the density of polyethylene can be 0.948 g / cm 3 Above, or 0.949g / cm 3 Above, or 0.950g / cm 3 Above, and 0.960g / cm 3 Below, or 0.958g / cm 3 Below, or 0.955g / cm 3 Below, or 0.953g / cm 3 the following.
[0060] According to one embodiment of the present invention, polyethylene can be a copolymer of, for example, ethylene and alpha-olefins. In this regard, alpha-olefins can include propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-eicosene, norbornene, norbornadiene, ethylidene norbornene, phenyl norbornene, vinyl norbornene, dicyclopentadiene, 1,4-butadiene, 1,5-pentadiene, 1,6-hexadiene, styrene, alpha-methylstyrene, divinylbenzene and 3-chloromethylstyrene. Preferably, polyethylene can be a copolymer of ethylene and 1-butene, a copolymer of ethylene and 1-hexene or a copolymer of ethylene and 1-octene.
[0061] Meanwhile, the polyethylene having the above-mentioned physical properties according to one embodiment of the present invention may be prepared by a preparation method including the steps of polymerizing an olefin monomer in the presence of a catalyst composition including a metallocene compound as a catalytically active component.
[0062] More specifically, the polyethylene of the present invention may be prepared by copolymerizing ethylene and α-olefin in the presence of a catalyst composition including a metallocene compound represented by the following Chemical Formula 1, but is not limited thereto.
[0063] [Chemical formula 1]
[0064]
[0065] In Chemical Formula 1,
[0066] B is boron,
[0067] M is a Group 4 transition metal,
[0068] R1 to R4 are each independently hydrogen, C 1-20 Alkyl, C 3-20 Cycloalkyl or C 6-20 Aryl, or R1 and R2 or R3 and R4 are connected to each other to form a C with or without substitution 6-60 Aromatic rings,
[0069] R5 and R6 are each independently C 1-20 Alkyl, C 3-20 Cycloalkyl or C 6-20 Aryl, or R5 and R6 are connected to each other to form a C 3-60 Alicyclic or C 6-60 Aromatic rings,
[0070] X1 and X2 are each independently C 1-20 Alkyl or -O(CO)R', where R' is C 1-20 alkyl,
[0071] Q is a substituted or unsubstituted C containing any one or more selected from the group consisting of N, O and S. 2-60 Heterocyclic rings,
[0072] Y and Y' are the elements that make up Q,
[0073] Y is N, O or S;
[0074] Y' is an element of Q, adjacent to Y, and is either N or C.
[0075] In the specification, unless particularly defined, the following terms may be defined as follows.
[0076] The halogen may be fluorine (F), chlorine (CI), bromine (Br) or iodine (I).
[0077] The alkyl group may be a straight chain or a branched chain. 1-20 The alkyl group can be: C 1-20 Straight chain alkyl; C 1-10Straight chain alkyl; C 1-5 Straight chain alkyl; C 3-20 Branched alkyl; C 3-15 Branched alkyl; or C 3-10 More specifically, C 1-20 The alkyl group may be methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, isopentyl, etc., but is not limited thereto. Meanwhile, in the present specification, "iPr" refers to isopropyl.
[0078] The cycloalkyl group may be a cyclic alkyl group. Specifically, C 3-20 Cycloalkyl can be: C 3-20 Cyclic alkyl; C 3-15 Cyclic alkyl; or C 3-10 Cyclic alkyl. More specifically, the cycloalkyl group may be cyclopropyl, cyclobutyl, cyclopentyl, 3-methylcyclopentyl, 2,3-dimethylcyclopentyl, cyclohexyl, 3-methylcyclohexyl, 4-methylcyclohexyl, 3,4,5-trimethylcyclohexyl, 4-tert-butylcyclohexyl, cycloheptyl, cyclooctyl, etc., but is not limited thereto. Meanwhile, in the present specification, "Cy" refers to a cycloalkyl group having 3 to 6 carbon atoms.
[0079] The alkenyl group may be a straight chain, branched chain or cyclic alkenyl group. 2-20 The alkenyl group may be C 2-20 Straight chain alkenyl, C 2-10 Straight chain alkenyl, C 2-5 Straight chain alkenyl, C 3-20 Branched alkenyl, C 3-15 Branched alkenyl, C 3-10 Branched alkenyl, C 5-20 Cycloalkenyl or C 5-10 More specifically, C 2-20 The alkenyl group may be ethenyl, propenyl, butenyl, pentenyl or cycloalkenyl, etc.
[0080] The alkoxy group may be a straight chain, branched chain or cyclic alkoxy group. 1-20 Alkoxy can be: C 1-20 Straight chain alkoxy; C 1-10 Straight chain alkoxy; C 1-5 Straight chain alkoxy; C 3-20 Branched or cyclic alkoxy; C 3-15 Branched or cyclic alkoxy; or C 3-10 More specifically, C 1-20 The alkoxy group may be methoxy, ethoxy, n-propoxy, isopropoxy, n-butoxy, isobutoxy, tert-butoxy, n-pentyloxy, isopentyloxy, neopentyloxy, cycloheptyloxy, or the like, but is not limited thereto.
[0081] The structure of the alkoxyalkyl group includes -Ra-O-Rb, which may be a substituent in which one or more hydrogen atoms of the alkyl group (-Ra) are replaced by an alkoxy group (-O-Rb). 2-20 The alkoxyalkyl group may be methoxymethyl, methoxyethyl, ethoxymethyl, isopropoxymethyl, isopropoxyethyl, isopropoxyhexyl, tert-butoxymethyl, tert-butoxyethyl, tert-butoxyhexyl, or the like, but is not limited thereto.
[0082] The aryl group includes monocyclic, bicyclic or tricyclic aromatic hydrocarbons. According to one embodiment of the present invention, the aryl group may have 6 to 60 carbon atoms or 6 to 20 carbon atoms, and the aryl group may specifically be phenyl, naphthyl, anthracenyl, dimethylanilino, anisyl, etc., but is not limited thereto.
[0083] The heteroaryl group is a heteroaryl group including one or more of N, O and S as a heteroatom, and the number of carbon atoms may be, but is not specifically limited to, 2 to 60 or 2 to 20. Examples of the heteroaryl group may include xanthene, thioanthene, thiophene, furan, pyrrole, imidazole, thiazole, oxazole, oxadiazole, triazole, pyridyl, bipyridyl, pyridyl, pyrimidyl, triazine, acridinyl, pyridazine, pyrazinyl, quinolyl, quinazolinyl, quinoxalinyl, phthalazinyl, pyridopyrimidinyl, pyridopyrazinyl, pyrazinopyrazinyl, isoquinoline, indole, carbazole, benzoxazole, benzimidazole, benzothiazole, benzocarbazole, benzothiophene, dibenzothiophene, benzofuran, phenanthroline, isoxazole, thiadiazole, phenothiazinyl, dibenzofuranyl and the like, but are not limited thereto.
[0084] Hydrocarbyl refers to a monovalent hydrocarbon compound, including alkyl, alkenyl, alkynyl, aryl, aralkyl, aralkenyl, aralkynyl, alkylaryl, alkenylaryl, alkynylaryl, etc. For example, the hydrocarbyl can be a straight chain, branched or cyclic alkyl. More specifically, the hydrocarbyl having 1 to 30 carbon atoms can be: a straight chain, branched or cyclic alkyl, such as methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, n-hexyl, n-heptyl, cyclohexyl, etc.; or an aryl, such as phenyl, biphenyl, naphthyl, anthracenyl, phenanthrenyl, fluorenyl, etc. In addition, it can be: an alkylaryl, such as methylphenyl, ethylphenyl, methylbiphenyl, methylnaphthyl, etc., or an aryl, such as phenylmethyl, phenylethyl, biphenylmethyl, naphthylmethyl, etc. It can also be an alkenyl, such as allyl, vinyl, propenyl, butenyl, pentenyl, etc.
[0085] The heterocyclic ring includes all alicyclic rings containing any one or more selected from the group consisting of N, O and S and aromatic rings containing any one or more selected from the group consisting of N, O and S.
[0086] In addition, the Group 4 transition metal may be titanium (Ti), zirconium (Zr), hafnium (Hf) or ruthenium (Rf), particularly titanium (Ti), zirconium (Zr) or hafnium (Hf), more particularly zirconium (Zr) or hafnium (Hf), but is not limited thereto.
[0087] The above-mentioned substituents may be optionally substituted with one or more substituents selected from the group consisting of hydroxyl; halogen; alkyl, alkenyl, aryl or alkoxy; alkyl, alkenyl, aryl or alkoxy including one or more heteroatoms among heteroatoms of Groups 14 to 16; amino; silyl; alkylsilyl or alkoxysilyl; phosphine; phosphide; sulfonate; and sulfone, within the range of exhibiting the same or similar effects as the desired effects.
[0088] Unlike the commonly used CGC-type precursor, the metallocene compound represented by Chemical Formula 1 adopts a bridge structure including a boron anion. The conventional CGC-type precursor has a neutral bridge structure including silicon, which makes the ligand unit negatively charged. Due to the structural limitations caused by this, there is a problem that it is difficult to achieve various physical properties in the process of preparing olefin polymers.
[0089] In contrast, metallocene compounds can have neutral ligand units because the bridge structure is negatively charged. The ligand unit of the present invention is a heterocyclic Q of Chemical Formula 1, wherein Y as an element of Q coordinates with a metal, and Y' as an element of Q adjacent to Y is connected to the bridge. Therefore, in the present invention, by using various neutral ligand units satisfying the above structure, a catalyst having higher activity and higher copolymerizability than the existing CGC precursor can be prepared.
[0090] In addition, the metallocene compound contains alkyl or carboxylate as the metal substituent, which acts as a good leaving group, promoting the reaction with the co-catalyst such as MAO, thereby improving the activity.
[0091] Therefore, when using metallocene compounds, the high melt index of polyethylene can be maintained, the low molecular weight components can be reduced, the molecular weight distribution can be very narrow, and the SCB content can be increased to increase the number of effective physical crosslinks of the molecules, thereby preparing polyethylene with excellent wear resistance.
[0092] In Chemical Formula 1, M may preferably be zirconium (Zr).
[0093] Preferably, R1 to R4 are each independently hydrogen, C 1-10 Alkyl or C 6-20 aryl, and R1 and R2 or R3 and R4 are connected to each other to form a C with or without a substituent 6-20 Aromatic ring.
[0094] More preferably, R1 to R4 are each independently hydrogen or methyl, or R1 and R2 or R3 and R4 are connected to each other to form a benzene ring or a 1,2,3,4-tetrahydronaphthalene ring, wherein the benzene ring or the 1,2,3,4-tetrahydronaphthalene ring may have no substituent or be substituted with 1 to 4 substituents selected from the group consisting of methyl, tert-butyl and 4-tert-butylphenyl.
[0095] Preferably, R5 and R6 are each independently C 1-10 Alkyl or C 6-20 Aryl, or R5 and R6 are connected to each other to form a C 3-20 Alicyclic or C 6-20 Aromatic ring.
[0096] More preferably, R5 and R6 are each independently a methyl group or a phenyl group, or R5 and R6 are linked to each other to form a cyclooctane ring.
[0097] Most preferably, R5 and R6 may each be phenyl.
[0098] Preferably, X1 and X2 may each independently be methyl or acetate.
[0099] Preferably, R' may be a methyl group.
[0100] Preferably, X1 and X2 may be identical to each other.
[0101] Preferably, Q may be a substituted or unsubstituted C containing any one or more selected from the group consisting of N, O and S. 2-20 Heterocyclic ring.
[0102] More preferably, Q may be a pyridine ring, a quinoline ring, a 4,5-dihydrooxazole ring, a pyrazole ring or a benzoxazole ring, wherein Q has no substituent or is substituted with 1 to 4 substituents selected from the group consisting of a methyl group, an isopropyl group and a diphenylamino group.
[0103] More preferably, Q may be a pyridine ring, a 4,5-dihydrooxazole ring, a pyrazole ring or a benzoxazole ring, wherein Q has no substituent or is substituted with 1 to 4 substituents selected from the group consisting of a methyl group, an isopropyl group and a diphenylamino group.
[0104] Y is a heteroatom coordinated to the metal M. Preferably, Y may be N.
[0105] Meanwhile, specific examples of the metallocene compound represented by Chemical Formula 1 may include compounds represented by the following structural formulas, but the present invention is not limited thereto:
[0106]
[0107]
[0108]
[0109] For example, when X1 and X2 are the same as each other, the metallocene compound represented by Chemical Formula 1 can be prepared by a preparation method such as the following Reaction Formula 1, but is not limited thereto, and it can be prepared according to a known method for preparing an organic compound and a metallocene compound. The preparation method will be described in more detail in the preparation examples described later.
[0110] [Reaction 1]
[0111]
[0112] In Reaction Formula 1, B, M, R1 to R6, X1, X2, Q, Y and Y′ are the same as defined in Chemical Formula 1.
[0113] The catalyst composition according to one embodiment of the present invention may include the metallocene compound of Chemical Formula 1 as a single catalyst.
[0114] In this regard, the catalyst composition can include the metallocene compound as a single component, or can be in the form of a supported metallocene catalyst comprising the metallocene compound and a carrier. When a supported metallocene catalyst is used, the morphology and physical properties of the polyethylene prepared can be improved, and it can be suitably used in conventional slurry polymerization, bulk polymerization and gas phase polymerization processes.
[0115] Specifically, as a carrier, a carrier having a highly active hydroxyl group, a silanol group or a siloxane group on its surface can be used. For this purpose, those whose surface is modified by calcination or those whose surface is dried to remove moisture can be used. For example, silica prepared by calcining silica gel, silica dried at high temperature, silica-alumina and silica-magnesia can be used. These materials can generally include oxides, carbonates, sulfates and nitrates, such as Na2O, K2CO3, BaSO4, Mg(NO3)2, etc.
[0116] The carrier may be calcined or dried at a temperature of about 200° C. to 600° C. or about 250° C. to 600° C. When the calcination or drying temperature of the carrier is low, too much moisture remains in the carrier, so it is foreseeable that the moisture on the surface may react with the co-catalyst. In addition, due to the excess hydroxyl groups, the co-catalyst loading rate may be relatively high, but this requires a large amount of co-catalyst. When the drying or calcination temperature is too high, the pores on the surface of the carrier may be combined with each other to reduce the surface area, and many hydroxyl groups or silanol groups may be lost from the surface, leaving only siloxane groups. Therefore, it is foreseeable that the reaction sites with the co-catalyst may be reduced.
[0117] The amount of hydroxyl groups on the surface of the carrier is preferably 0.1 mmol / g to 10 mmol / g, more preferably 0.5 mmol / g to 5 mmol / g. The amount of hydroxyl groups on the surface of the carrier can be controlled by the preparation method and preparation conditions or drying conditions (such as temperature, time, vacuum or spray drying, etc.) of the carrier.
[0118] When the hydroxyl amount is less than 0.1 mmol / g, the reaction sites with the co-catalyst may be reduced. When the hydroxyl amount exceeds 10 mmol / g, in addition to the hydroxyl groups existing on the surface of the carrier particles, moisture may also be caused, which is undesirable.
[0119] For example, the amount of hydroxyl groups on the surface of the carrier can be 0.1 mmol / g to 10 mmol / g or 0.5 mmol / g to 5 mmol / g. The amount of hydroxyl groups on the surface of the carrier can be controlled by the preparation method and preparation conditions or drying conditions (such as temperature, time, vacuum or spray drying, etc.) of the carrier. When the amount of hydroxyl groups is too small, the reaction sites with the co-catalyst may be reduced. When the amount of hydroxyl groups is too large, in addition to the hydroxyl groups present on the surface of the carrier particles, it may also be caused by moisture.
[0120] Among the above supports, silica prepared by calcining silica, especially silica gel, releases little catalyst from the support surface during the polymerization of propylene because the functional groups of the compound of Chemical Formula 1 are chemically bonded to and supported on the silica support. Therefore, when polyethylene is prepared by slurry polymerization or gas phase polymerization, the scaling phenomenon in which polymer particles adhere to the reactor wall or to each other can be minimized.
[0121] In addition, when supported on a carrier, the loading amount of the compound of Chemical Formula 1 may be about 10 μmol or more, or about 30 μmol or more, and about 100 μmol or less, or about 80 μmol or less, based on the weight of the carrier, for example, about 1 g of silica. When loaded within the above content range, the supported catalyst may exhibit appropriate activity, which is advantageous in terms of maintaining catalytic activity and economic feasibility.
[0122] The catalyst composition may further include one or more co-catalysts as well as the above-mentioned metallocene compound and support.
[0123] Any cocatalyst can be used as a cocatalyst, as long as it can be used for the polymerization of olefins in the presence of a general metallocene catalyst. Such a cocatalyst allows the hydroxyl groups on the support to bind to the Group 4 transition metal. In addition, since the cocatalyst is only present on the support surface, it can help ensure the unique properties of the specific mixed catalyst composition of the present application without the fouling phenomenon of polymer particles adhering to the reactor wall or to each other.
[0124] Furthermore, the catalyst composition of the present invention may further include one or more co-catalyst compounds selected from the group consisting of compounds represented by the following Chemical Formulae 2 to 4 in addition to the metallocene compound.
[0125] [Chemical formula 2]
[0126] -[Al(R 10 )-O]a-
[0127] In chemical formula 2,
[0128] R 10 is halogen; or substituted with halogen or unsubstituted C 1-20 a hydrocarbon group; and
[0129] a is an integer greater than or equal to 2.
[0130] [Chemical formula 3]
[0131] D(R 11 )3
[0132] In chemical formula 3,
[0133] D is aluminum or boron; and
[0134] R 11 is halogen; or substituted with halogen or unsubstituted C 1-20 Hydrocarbon.
[0135] [Chemical formula 4]
[0136] [LH] + [ZA]4 - or [L] + [ZA]4 -
[0137] In chemical formula 4,
[0138] L is a neutral or cationic Lewis base.
[0139] H is a hydrogen atom.
[0140] Z is a Group 13 element; and
[0141] A is each independently one in which one or more hydrogen atoms are replaced by halogen, C 1-20 Hydrocarbon, C 1-20 Alkoxy or phenoxy substituted C 6-20 Aryl or C 1-20 alkyl.
[0142] The compound represented by Chemical Formula 2 may serve as an alkylating agent and an activating agent, the compound represented by Chemical Formula 3 may serve as an alkylating agent, and the compound represented by Chemical Formula 4 may serve as an activating agent.
[0143] The compound represented by Chemical Formula 2 is not particularly limited as long as it is an alkylaluminoxane, and may be, for example, methylaluminoxane, ethylaluminoxane, isobutylaluminoxane, butylaluminoxane, etc., and preferably methylaluminoxane.
[0144] The compound represented by Chemical Formula 3 is not particularly limited as long as it is an alkyl metal compound, and for example, it may be trimethylaluminum, triethylaluminum, triisobutylaluminum, tripropylaluminum, tributylaluminum, dimethylaluminum chloride, triisopropylaluminum, tri-sec-butylaluminum, tricyclopentylaluminum, tripentylaluminum, triisopentylaluminum, trihexylaluminum, trioctylaluminum, ethyldimethylaluminum, methyldiethylaluminum, triphenylaluminum, tri-p-tolylaluminum, dimethylaluminum methoxide, dimethylaluminum ethoxide, trimethylboron, triethylboron, triisobutylboron, tripropylboron, tributylboron, and the like, and it may be preferably selected from trimethylaluminum, triethylaluminum, and triisobutylaluminum.
[0145] Examples of the compound represented by Chemical Formula 4 may include triethylammonium tetraphenylboron, tributylammonium tetraphenylboron, trimethylammonium tetraphenylboron, tripropylammonium tetraphenylboron, trimethylammonium tetra(p-tolyl)boron, trimethylammonium tetra(o,p-dimethylphenyl)boron, tributylammonium tetra(p-trifluoromethylphenyl)boron, trimethylammonium tetra(p-trifluoromethylphenyl)boron, tributylammonium tetra(pentafluorophenyl)boron, N,N-diethylaniline tetraphenylboron, N,N-diethylaniline tetra(pentafluorophenyl)boron, diethylammonium tetra(pentafluorophenyl)boron, triphenylphosphonium tetraphenylboron, trimethylphosphonium tetraphenylboron, triethylammonium tetraphenylaluminum, tributylammonium tetraphenylaluminum, trimethylammonium tetraphenylaluminum, tripropylammonium tetraphenylaluminum, tri Methylammonium tetra(p-tolyl)aluminum, tripropylammonium tetra(p-tolyl)aluminum, triethylammonium tetra(o,p-dimethylphenyl)aluminum, tributylammonium tetra(p-trifluoromethylphenyl)aluminum, trimethylammonium tetra(p-trifluoromethylphenyl)aluminum, tributylammonium tetra(p-trifluoromethylphenyl)aluminum, N,N-diethylaniline tetraphenylaluminum, N,N-diethylaniline tetra(pentafluorophenyl)aluminum, diethylammonium tetra(pentafluorophenyl)aluminum, triphenylphosphonium tetraphenylaluminum, trimethylphosphonium tetraphenylaluminum, tripropylammonium tetra(p-tolyl)boron, triethylammonium tetra(o,p-dimethylphenyl)boron, tributylammonium tetra(p-trifluoromethylphenyl)boron, triphenylcarbonium tetra(p-trifluoromethylphenyl)boron, or triphenylcarbonium tetra(pentafluorophenyl)boron, etc. Preferably, aluminoxane can be used, and more preferably, methylaluminoxane (MAO) as an alkylaluminoxane can be used.
[0146] The loading amount of the co-catalyst may be about 3 mmol to about 25 mmol, or about 5 mmol to about 20 mmol, based on 1 g of the support.
[0147] Meanwhile, the catalyst composition can be prepared by a method for preparing a catalyst composition comprising a carrier loaded with a co-catalyst and a metallocene compound, the method comprising the steps of loading the co-catalyst on the carrier and loading the metallocene compound on the carrier having the co-catalyst loaded thereon.
[0148] In this method, there is no particular restriction on the loading conditions, and the loading can be carried out within the range known to those skilled in the art. For example, high temperature loading and low temperature loading can be appropriately carried out, and the loading temperature can be, for example, in the range of about -30°C to about 150°C, preferably about 50°C to about 98°C, or about 55°C to about 95°C. The loading time can be appropriately controlled according to the amount of the first metallocene compound to be loaded. The supported catalyst thus reacted can be used as it is after removing the reaction solvent by filtration or reduced pressure distillation, and can be used after Soxhlet filtration with aromatic hydrocarbons such as toluene, if necessary.
[0149] In addition, the preparation of the supported catalyst can be carried out with or without a solvent. When a solvent is used, suitable solvents may include: aliphatic hydrocarbon solvents such as hexane or pentane, aromatic hydrocarbon solvents such as toluene or benzene, hydrocarbon solvents substituted with chlorine atoms such as dichloromethane, ether solvents such as diethyl ether or tetrahydrofuran (THF), and organic solvents such as acetone and ethyl acetate. Hexane, heptane, toluene or dichloromethane are preferred.
[0150] Meanwhile, the polyethylene according to one embodiment of the present invention may be prepared by a method for preparing polyethylene, the method including the step of polymerizing the polyethylene in the presence of a catalyst composition including a metallocene compound.
[0151] The process for preparing polyethylene can be carried out by a slurry polymerization process using ethylene and α-olefin as raw materials in the presence of the above-mentioned catalyst composition and applying conventional apparatuses and contact techniques.
[0152] The method of preparing polyethylene may copolymerize ethylene and α-olefin using a continuous slurry polymerization reactor, a loop reactor, etc., but is not limited thereto.
[0153] Specifically, the copolymerization step may be performed by reacting about 0.45 mol or less, or about 0.1 mol to about 0.45 mol, or about 0.4 mol or less, or about 0.2 mol to about 0.4 mol, or about 0.35 mol or less, or about 0.25 mol to about 0.35 mol of α-olefin based on 1 mol of ethylene.
[0154] The method for preparing polyethylene is characterized in that it is not necessary to increase the comonomer content in order to reduce the density of the product, so the process is stable and the high drop impact strength of the product can be reproduced.
[0155] Furthermore, the α-olefin may be one or more selected from the group consisting of 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-octadecene, 1-eicosene, and mixtures thereof.
[0156] Specifically, in the method for preparing polyethylene, for example, 1-hexene can be used as the α-olefin. Therefore, in the slurry polymerization, an ultra-low density polyethylene copolymer can be prepared by polymerizing ethylene and 1-hexene.
[0157] In addition, the polymerization temperature may be about 25°C to about 500°C, or about 25°C to about 300°C, or about 30°C to about 200°C, or about 50°C to about 150°C, or about 60°C to about 120°C. In addition, the polymerization pressure may be about 1 kgf / cm 2 To about 100kgf / cm 2 , or about 1kgf / cm 2 To about 50kgf / cm 2 , or about 5kgf / cm 2 To about 45kgf / cm 2 , or about 10kgf / cm 2 To about 40kgf / cm 2 , or about 15kgf / cm 2 To about 35kgf / cm 2 .
[0158] The catalyst composition of the present invention comprising the metallocene compound of Chemical Formula 1 can be injected after being dissolved or diluted in an aliphatic hydrocarbon solvent having 5 to 12 carbon atoms (e.g., pentane, hexane, heptane, nonane, decane and isomers thereof) and an aromatic hydrocarbon solvent (e.g., toluene and benzene) or a hydrocarbon solvent substituted with chlorine atoms (e.g., dichloromethane and chlorobenzene). The solvent used here is preferably used after removing a small amount of water or air as a catalyst poison by treating with a small amount of alkyl aluminum. A cocatalyst may be further used.
[0159] For example, the polymerization step may be performed by injecting about 800 ppm or less, or about 0 to about 800 ppm, or about 300 ppm or less, or about 10 ppm to about 300 ppm, or about 100 ppm or less, or about 15 ppm to about 100 ppm of hydrogen based on the amount of ethylene.
[0160] In such ethylene copolymerization process, the catalyst composition comprising the metallocene compound of the present invention can show high catalytic activity. For example, in the ethylene copolymerization process, when calculated as the weight (kg PE) of the polyethylene produced based on the unit time (hr) to the weight (g) of the catalyst composition used, the catalytic activity can be about 4.0kg PE / g·cat·hr or more or about 4.0kg PE / g·cat·hr to about 50kg PE / g·cat·hr. Specifically, the activity of the catalyst composition can be about 4.2kg PE / g·cat·hr or more, or about 4.3kg PE / g·cat·hr or more, or about 4.5kg PE / g·cat·hr or more, or about 40kg PE / g·cat·hr or less, or about 30kg PE / g·cat·hr or less, or about 15kg PE / g·cat·hr or less.
[0161] As described above, according to the present invention, polyethylene may be prepared by copolymerizing ethylene and α-olefin using a catalyst composition including the metallocene compound of Chemical Formula 1 above.
[0162] In this regard, the polyethylene produced may be an ethylene-1-hexene copolymer.
[0163] The method for preparing polyethylene can provide polyethylene having excellent physical properties by conducting slurry polymerization in the presence of the above-mentioned catalyst composition.
[0164] In particular, the catalyst composition comprising the metallocene compound of Chemical Formula 1 of the present invention can exhibit high activity as described above in the copolymerization process of ethylene and α-olefin, and can increase the content of short chain branches (SCB) in the molecule without excessively increasing the content of α-olefin comonomers while having a high molecular weight.
[0165] The polyethylene of the present invention prepared by the preparation method of one embodiment above has a narrow molecular weight distribution and low crystallinity within a similar melt index (MI) range. Therefore, the effective physical crosslink number of the molecule increases, the generation of fluff or dust is reduced during the stretching process, and the wear resistance is improved. Therefore, the polyethylene can be applied to fiber products.
[0166] Below, in order to better understand the present invention, preferred exemplary embodiments are provided. However, the following exemplary embodiments are provided only to make it easier to understand the present invention, but the content of the present invention is not limited thereby.
[0167] <Example>
[0168] Synthesis example 1
[0169]
[0170] 2-Bromopyridine (1 equivalent) was dissolved in tetrahydrofuran (0.1 M), and then n-butyllithium (1 equivalent) was slowly added dropwise at -90°C, followed by stirring at the same temperature for 1 hour. Then, chlorodiphenylborane (1 equivalent) was dissolved in toluene (0.3 M), and then slowly added dropwise to the first reaction product at -78°C, and stirred for another 1 hour. Thereafter, the mixture was stirred at room temperature for 12 hours, vacuum dried to remove the solvent, toluene was added, and the filtrate obtained by removing the solid through a filter was vacuum dried to obtain diphenyl(pyridin-2-yl)borane.
[0171] Diphenyl(pyridin-2-yl)borane (1 equivalent) was dissolved in tetrahydrofuran (0.1 M), and then a solution of tetramethylcyclopentadienyl lithium (Li(CpMe4), 1 equivalent) dissolved in tetrahydrofuran (0.1 M) was slowly added dropwise at 0°C, and then stirred at room temperature overnight. The solvent was removed by drying under vacuum, and toluene / ether (volume ratio of 3 / 1, 0.3 M) was introduced to dissolve, and MCl4 (1 equivalent) was mixed with toluene (0.2 M), and then introduced at -78°C, and then stirred at room temperature overnight. When the reaction was complete, the solvent was removed by drying under vacuum, and dichloromethane was introduced and the salt was removed by filtering. The filtrate was dried under vacuum and then recrystallized by adding dichloromethane / hexane. The resulting solid was filtered and dried under vacuum to obtain dichloro{diphenyl(pyridin-2-yl-κN)(η 5 -2,3,4,5-tetramethylcyclopenta-2,4-dien-1-ylidene)zirconium(IV)borate.
[0172] Dichloro{diphenyl(pyridin-2-yl-κN)(η 5 -2,3,4,5-tetramethylcyclopenta-2,4-diene-1-ylidene) borate} zirconium (IV) (1 equivalent) was dissolved in toluene / ether (volume ratio 3 / 1, 0.3M), and then a solution of methyl lithium (2 equivalents) dissolved in hexane or ether was slowly added dropwise at -78°C and stirred at room temperature for 12 hours. When the reaction was complete, the solvent was dried under vacuum, and dichloromethane was introduced and the salt was removed by a filter. The filtrate was dried under vacuum and then recrystallized by adding dichloromethane / hexane. The resulting solid was filtered and dried under vacuum to obtain the precursor compound.
[0173] 1H NMR (500MHz, CDCl3, ppm)=δ8.32(d,1H),8.05(d,4H),7.70(t,1H),7.42(t,1H ),7.40(t,4H),7.23(d,1H),7.17(t,2H),2.08(s,6H),1.93(s,6H)0.95(s,6H)
[0174] Synthesis example 2
[0175]
[0176] 2-Bromopyridine (1 equivalent) was dissolved in tetrahydrofuran (0.1 M), and then n-butyllithium (1 equivalent) was slowly added dropwise at -90°C, followed by stirring at the same temperature for 1 hour. Then, chlorodiphenylborane (1 equivalent) was dissolved in toluene (0.3 M), and then slowly added dropwise to the first reaction product at -78°C, and stirred for another 1 hour. Thereafter, the mixture was stirred at room temperature for 12 hours, vacuum dried to remove the solvent, toluene was added, and the filtrate obtained by removing the solid through a filter was vacuum dried to obtain diphenyl(pyridin-2-yl)borane.
[0177] Diphenyl(pyridin-2-yl)borane (1 equivalent) was dissolved in tetrahydrofuran (0.1 M), and then a solution of tetramethylcyclopentadienyl lithium (Li(CpMe4), 1 equivalent) dissolved in tetrahydrofuran (0.1 M) was slowly added dropwise at 0°C, and then stirred at room temperature overnight. The solvent was removed by drying under vacuum, and toluene / ether (volume ratio of 3 / 1, 0.3 M) was introduced to dissolve, and MCl4 (1 equivalent) was mixed with toluene (0.2 M), and then introduced at -78°C, and then stirred at room temperature overnight. When the reaction was complete, the solvent was removed by drying under vacuum, dichloromethane was introduced, and the salt was removed by filtering. The filtrate was dried under vacuum, and then recrystallized by adding dichloromethane / hexane. The resulting solid was filtered and dried under vacuum to obtain dichloro{diphenyl(pyridin-2-yl-κN)(η 5 -2,3,4,5-tetramethylcyclopenta-2,4-dien-1-ylidene)zirconium(IV)borate.
[0178] Dichloro{diphenyl(pyridin-2-yl-κN)(η 5 -2,3,4,5-tetramethylcyclopenta-2,4-diene-1-ylidene) borate} zirconium (IV) (1 equivalent) was dissolved in toluene / ether (volume ratio 3 / 1, 0.3M), and then a solution of sodium acetate (2 equivalents) dissolved in hexane or ether was slowly added dropwise at -78°C and stirred at room temperature for 12 hours. When the reaction was complete, the solvent was dried under vacuum, dichloromethane was introduced and the salt was removed by a filter. The filtrate was dried under vacuum and then recrystallized by adding dichloromethane / hexane. The resulting solid was filtered and dried under vacuum to obtain the precursor compound.
[0179] 1H NMR (500MHz, CDCl3, ppm)=δ8.35(d,1H),8.04(d,4H),7.72(t,1H),7.45(t,1H) ,7.35(t,4H),7.20(d,1H),7.11(t,2H),2.12(s,6H),2.01(s,6H),1.88(s,6H)
[0180] Synthesis example 3
[0181]
[0182] Dimethyl{diphenyl(pyridin-2-yl-κN)(η 5 -2-methyl-4-(4-tert-butylphenyl)indene)zirconium(IV) borate precursor compound was obtained in the same manner as in Synthesis Example 1, except that 2-methyl-4-(4-tert-butylphenyl)indene lithium was used instead of tetramethylcyclopentadienyllithium (Li(CpMe4)).
[0183] 1H NMR (500MHz, CDCl3, ppm)=δ8.34(d,1H),8.13(d,4H),8.05(d,1H),7.79-74(m,2H),7.47(t,1H),7.41-7. 39(m,6H),7.35(m,3H),7.23(d,1H),7.20(t,2H),6.66(s,1H),2.09(s,3H),1.49(s,9H),0.94(s,6H)ppm.
[0184] Synthesis example 4
[0185]
[0186] Dimethyl{diphenyl(pyridin-2-yl-κN)(η 5 A zirconium (IV) precursor compound was obtained in the same manner as in Synthesis Example 1, except that 2,7-di-tert-butyl-9H-fluoren-9-ylidene lithium was used instead of tetramethylcyclopentadienyl lithium (Li(CpMe4)).
[0187] 1H NMR (500MHz, CDCl3, ppm)=δ8.40(d,1H),8.12(d,4H),8.09(d,2H),7.73-7.70(m,3H),7 .50(t,1H),7.40-7.36(m,6H),7.19(d,1H),7.14(t,2H),1.44(s,18H),0.90(s,6H)ppm
[0188] Synthesis example 5
[0189]
[0190] Dimethyl{diphenyl(pyridin-2-yl-κN)(η 5 -1,2,3,4,7,8,9,10-octahydro-1,1,4,4,7,7,10,10-octamethyl-12H-dibenzo[b,h]fluoren-12-ylidene)boronic acid}zirconium (IV) precursor compound was obtained in the same manner as in Synthesis Example 1, except that 1,2,3,4,7,8,9,10-octahydro-1,1,4,4,7,7,10,10-octamethyl-12H-dibenzo[b,h]fluoren-12-yllithium was used instead of tetramethylcyclopentadienyllithium (Li(CpMe4)).
[0191] 1H NMR (500MHz, CDCl3, ppm)=δ8.42(d,1H),8.13(d,4H),8.07(s,2H),7.74(t,1H),7.53(s,2H),7.44(t,1 H),7.42(t,4H),7.26(d,1H),7.10(t,2H)1.66(m,4H),1.46(m,4H),1.30-0.99(m,24H),0.94(s,6H)ppm
[0192] Synthesis example 6
[0193]
[0194] A dimethyl{(cyclooctane-1,5-diyl)(pyridin-2-yl-κN)(η5-2,3,4,5-tetramethylcyclopenta-2,4-dien-1-ylidene)boronic acid}zirconium (IV) precursor compound was obtained in the same manner as in Synthesis Example 1, except that (1s,5s)-9-chloro-9-borahicyclo[3.3.1]nonane was used instead of chlorodiphenylborane.
[0195] 1H NMR (500MHz, CDCl3, ppm)=δ8.49(d,1H),7.70(t,1H),7.41(t,1H),7.21(d,1H),2.16(s,6H),2.05-1.85(m,12H),1.69-1.60(m,4H),1.52(br m,2H),1.02(br m,2H),0.93(s,6H)ppm
[0196] <Preparation Example of Supported Catalyst>
[0197] Preparation Example 1
[0198] 50 mL of toluene was placed in a pico reactor, 7 g of silica gel (SYLOPOL 952X, calcined at 250° C.) was added under Ar, 10 mmol of methylaluminoxane (MAO) was slowly introduced at room temperature, and allowed to react for 24 hours under stirring at 95° C. When the reaction was complete, the mixture was cooled to room temperature and allowed to stand for 15 minutes to decante the solvent with a cannula. Toluene (400 mL) was added, stirred for 1 minute, and allowed to stand for 15 minutes to decante the solvent with a cannula.
[0199] 60 μmol of the metallocene compound of Synthesis Example 1 was dissolved in 30 mL of toluene, then transferred to a reactor with a cannula and reacted for 2 hours at 80 ° C under stirring. When the reaction was complete and the precipitation was complete, the product was cooled to room temperature and placed for 15 minutes to decant the solvent with a cannula. The supernatant was removed and the resulting reaction product was washed with toluene. After further washing with hexane, N, N-di(2-hydroxyethyl)pentadecylamine (Atmer163) as an antistatic agent was dissolved in 3 mL of hexane at 2% by weight based on the weight (g) of silica and then stirred at room temperature for 10 minutes. When the reaction was complete and the precipitation was complete, the supernatant was removed and the resulting product was transferred using a glass filter to remove the solvent.
[0200] The primary drying was performed under vacuum at room temperature for 5 hours, and the secondary drying was performed under vacuum at 45° C. for 4 hours to obtain a silica-supported metallocene catalyst in the form of solid particles.
[0201] Preparation Example 2 to Preparation Example 6
[0202] Each silica-supported metallocene catalyst was prepared in the same manner as in Preparation Example 1, except that the metallocene compound of Synthesis Example 2 to Synthesis Example 6 was used instead of the metallocene compound of Synthesis Example 1.
[0203] Comparative Preparation Example 1
[0204] A silica-supported metallocene catalyst was prepared in the same manner as in Preparation Example 1, except that [tBu-O-(CH2)6-C5H4]2ZrCl2 was used instead of the metallocene compound of Synthesis Example 1.
[0205] <Polyethylene Polymerization Example>
[0206] Example 1
[0207] In the presence of the supported catalyst obtained in Preparation Example 1, polyethylene (ethylene-1-hexene copolymer) was prepared according to the following method.
[0208] A 600 mL stainless steel reactor was vacuum dried at 120°C and cooled, and 1 g of trimethylaluminum (TMA) was added to 250 g of hexane at room temperature, followed by stirring for 10 minutes. The reacted hexane was completely removed, and then 250 g of hexane and 0.5 g of triisobutylaluminum (TIBAL) were added, followed by stirring for another 5 minutes. Thereafter, 7 mg of the supported catalyst obtained in Preparation Example 1 was added, followed by stirring while heating to 80°C. After stopping stirring at 80°C, 10 mL of comonomer 1-hexene (C6) was added, ethylene (C2) was filled to 15 bar, and stirring was started. After 30 minutes of polymerization, unreacted C2 was discharged.
[0209] Example 2 to Example 6
[0210] Each polyethylene was prepared in the same manner as in Example 1, except that each supported catalyst of Preparation Example 2 to Preparation Example 6 was used instead of the supported catalyst of Preparation Example 1.
[0211] Comparative Example 1
[0212] ASPUN TM 6835A fiber resin (Dow Chemical Company) was used as the polyethylene for Comparative Example 1.
[0213] Comparative Example 2
[0214] SK MK910 (SK Global Chemical) was used as the polyethylene in Comparative Example 2.
[0215] Comparative Example 3
[0216] ASPUN TM 6850A fiber resin (Dow Chemical Company) was used as the polyethylene for Comparative Example 3.
[0217] Comparative Example 4
[0218] SK MM810 (SK Global Chemical) was used as the polyethylene in Comparative Example 4.
[0219] Comparative Example 5
[0220] Polyethylene was prepared in the same manner as in Example 1, except that the supported catalyst of Comparative Preparation Example 1 was used instead of the supported catalyst of Preparation Example 1.
[0221] <Experimental example>
[0222] The physical properties of the polyethylene prepared in the Examples and Comparative Examples were measured as follows, and the results are shown in Table 1 below.
[0223] (1) Melt index (MI, g / 10min)
[0224] The melt index was measured at 190° C. under a load of 2.16 kg according to ASTM D1238, and the weight (g) of the polymer melted within 10 minutes was recorded as the melt index.
[0225] (2) Molecular weight distribution (MWD, Mw / Mn)
[0226] The molecular weight distribution (MWD, Mw / Mn) is determined by measuring the weight average molecular weight (Mw) and the number average molecular weight (Mn) of polyethylene using gel permeation chromatography (GPC, manufactured by Water), and then dividing the weight average molecular weight by the number average molecular weight.
[0227] Specifically, a PL-GPC220 produced by Waters was used as a gel permeation chromatography (GPC) instrument, and a Polymer Laboratories PLgel MIX-B column with a column length of 300 mm was used. At this time, the measurement temperature was 160 ° C, 1,2,4-trichlorobenzene was used as a solvent, and the flow rate was set to 1 mL / min. The polymer samples of the embodiments and comparative examples were each dissolved in 1,2,4-trichlorobenzene containing 0.0125% BHT at 160 ° C for 10 hours for pretreatment, prepared at a concentration of 10 mg / 10 mL, and the injection volume was 200 μL. The calibration curve formed using polystyrene standards was used to measure the Mw and Mn values. Nine polystyrene standards were used, with weight average molecular weights of 2000 g / mol, 10000 g / mol, 30000 g / mol, 70000 g / mol, 200000 g / mol, 700000 g / mol, 2000000 g / mol, 4000000 g / mol, and 10000000 g / mol.
[0228] (3) Crystallinity
[0229] Crystallinity was measured using a differential scanning calorimeter (DSC) according to ASTM F2625.
[0230] Specifically, using DSC2500 (TA Instruments) as a differential scanning calorimeter (DSC), the polyethylene copolymer was heated to 200°C and maintained for 3 minutes, then cooled to 0°C, and then heated again. At this time, the heating rate and the cooling rate were 10°C / min, respectively, and Tm was obtained from the second heating operation. At this time, the crystallinity was calculated by the following calculation formula 1. Theoretically, it is known that ΔH (at 100%) of PE is 293 J / g.
[0231] [Calculation formula 1]
[0232] Crystallinity (%) = △H (melting heat, endothermic enthalpy measured during the melting phase transition, melting peak width) / △H (at 100%) (endothermic enthalpy of 100% crystallinity material (100%)) = △H (melting heat, endothermic enthalpy measured during the melting phase transition, melting peak width) / 293 J / g.
[0233] (4)T cr (Crystal relaxation temperature).
[0234] The rheological properties of the injection molded specimens were evaluated using a dynamic mechanical analyzer (DMA) and determined as T cr .
[0235] In more detail, the polyethylene samples of the examples and comparative examples were pressed at 190°C to prepare rectangular specimens having a thickness of 0.5 mm, a width of 6 mm, and a length of 30 mm. Each polyethylene specimen was mounted on a Q800 DMA of TA Instruments, and the storage modulus E' and the loss modulus E" were measured by applying a cyclic deformation while increasing the temperature from -80°C to 140°C at a rate of 5°C per minute. Tan (δ), a value obtained by dividing the loss modulus at each temperature by the storage modulus, was obtained, and the temperature at which tan (δ) was maximum was determined as the crystal relaxation temperature.
[0236] (5) Wear resistance
[0237] For the polyethylene in the examples and comparative examples, the masterbatch pellets were extruded into microfiber webs to produce various nonwoven fabrics with reference to the literature [Report No. 4364 of Naval Research Laboratories, published on May 25, 1954, entitled "Manufacture of Superfine Organic Fibers", Wente, Van. A. Boone, CD and Fluharty, EL].
[0238] In detail, the masterbatch was prepared by mixing the polyethylene resin in the embodiment and the comparative example with the IF168 additive (1000ppm), and then pelletized with a 25mm twin-screw extruder. Subsequently, the molten masterbatch composition and the LG H7550 polypropylene were fed into a melt pump (65rpm) at a weight fraction ratio of 1:1 with a 31mm Brabender conical twin-screw extruder, and fed into a 25 cm wide melt-blown die with an orifice (10 holes / cm) and an orifice diameter of 381 microns. The melt temperature was 210°C, the screw speed was 120rpm, the die was maintained at 210°C, the primary air temperature and pressure were 270°C and 54kPa (7.8psi), the polymer throughput rate was 5.2kg / hr, and the collector / die distance was 15.0cm. When the microfibers spun from the orifice fall onto the collector, they are cooled by cooling air using two pumps, and the microfibers collected by the collector undergo a calendering process using upper and lower rollers to produce various nonwoven fabrics. At this time, the temperature of the cooling air is 16°C, and the temperatures of the upper and lower rollers during the calendering process are 160°C / 155°C, respectively.
[0239] The abrasion resistance of the nonwoven fabric thus prepared was measured using Sutherland Ink Rub Tester 2000 with reference to ASTM D5264.
[0240] In more detail, the fibers of each sample of Application Example and Comparative Example were prepared into a swatch having a size of 11.0 cm×4.0 cm, polished with 320-grit sandpaper (Sutherland Ink Rub Tester 2000) (20 cycles, 42 cycles / min), and the amount of loose fibers per unit area was measured.
[0241] In other words, wear resistance is measured by abrasion resistance (mg / cm 2 )=total weight of loose fibers / surface area, and when the amount of loose fibers per unit area is small, it is determined to be high abrasion resistance.
[0242]
Table 1
[0243]
[0244] Referring to Table 1, compared with the polyethylenes of Comparative Examples 1 to 5 having similar melt indexes, the polyethylenes of Examples 1 to 6 of the present invention show a melt index of 0.2 mg / cm 3 Following excellent wear resistance.
Claims
1. A polyethylene satisfying the following conditions 1) to 4): 1) a melt index MI of 0.5 g / 10 min to 40 g / 10 min measured at 190° C. under a load of 2.16 kg according to ASTM D1238; 2) Molecular weight distribution MWD is 2.3 to 2.6; 3) a crystallinity of 63% to 71% as measured using a differential scanning calorimeter (DSC) in accordance with ASTM F2625; and 4) Crystal relaxation temperature T measured using dynamic mechanical analysis (DMA) cr 42℃ to 50℃, among which, The polyethylene sample was pressed at 190°C to prepare a rectangular specimen with a thickness of 0.5 mm, a width of 6 mm and a length of 30 mm; the polyethylene sample was mounted on the Q800 DMA of TA Instruments, and the storage modulus E' and the loss modulus E" were measured by applying periodic deformation while increasing the temperature from -80°C to 140°C at a rate of 5°C per minute; tan(δ) was obtained, i.e., the value obtained by dividing the loss modulus at each temperature by the storage modulus, and the temperature at the maximum tan(δ) was determined as the crystal relaxation temperature.
2. The polyethylene according to claim 1, wherein The melt index MI measured at 190° C. under a load of 2.16 kg according to ASTM D1238 is 18 to 40 g / 10 min.
3. The polyethylene according to claim 1, wherein Abrasion resistance measured according to ASTM D5264: 0.2 mg / cm 2 the following.
4. The polyethylene according to claim 1, wherein The polyethylene is a copolymer of ethylene and α-olefin.
5. The polyethylene according to claim 4, wherein The α-olefin includes one or more selected from the group consisting of propylene, 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-eicosene, styrene and α-methylstyrene.
6. The polyethylene according to claim 1, wherein The polyethylene is prepared by copolymerizing ethylene and α-olefin in the presence of a catalyst composition, the catalyst composition including a metallocene compound represented by the following Chemical Formula 1: [Chemical formula 1] In Chemical Formula 1, B is boron, M is a Group 4 transition metal, R1 to R4 are each independently hydrogen, C 1-20 Alkyl, C 3-20 Cycloalkyl or C 6-20 Aryl, or R1 and R2 or R3 and R4 are connected to each other to form a C with or without substitution 6-60 Aromatic rings, R5 and R6 are each independently C 1-20 Alkyl, C 3-20 Cycloalkyl or C 6-20 Aryl, or R5 and R6 are connected to each other to form a C 3-60 Alicyclic or C 6-60 Aromatic rings, X1 and X2 are each independently C 1-20 Alkyl or -O(CO)R', where R' is C 1-20 alkyl, Q is a substituted or unsubstituted C containing any one or more selected from the group consisting of N, O and S. 2-60 Heterocyclic rings, Y and Y' are the elements that make up Q, Y is N, O or S; Y' is an element of Q, adjacent to Y, and is either N or C.
7. The polyethylene according to claim 6, wherein R1 to R4 are each independently hydrogen or methyl, or R1 and R2 or R3 and R4 are connected to each other to form a benzene ring or a 1,2,3,4-tetrahydronaphthalene ring, wherein the benzene ring or the 1,2,3,4-tetrahydronaphthalene ring has no substituent or is substituted with 1 to 4 substituents selected from the group consisting of methyl, tert-butyl and 4-tert-butylphenyl.
8. The polyethylene according to claim 6, wherein R5 and R6 are each independently a methyl group or a phenyl group, or R5 and R6 are linked to each other to form a cyclooctane ring.
9. The polyethylene according to claim 6, wherein The compound represented by Chemical Formula 1 is any one of the compounds represented by the following structural formulas:
10. The polyethylene according to claim 6, wherein The catalyst composition further comprises one or more co-catalyst compounds selected from the group consisting of compounds represented by the following Chemical Formulae 2 to 4, [Chemical formula 2] -[Al(R 10 )-O]a- In chemical formula 2 R 10 is halogen; or substituted with halogen or unsubstituted C 1-20 a hydrocarbon group; and a is an integer greater than 2; [Chemical formula 3] D(R 11 )3 In chemical formula 3, D is aluminum or boron; and R 11 is halogen; or substituted with halogen or unsubstituted C 1-20 Hydrocarbon, [Chemical formula 4] [LH] + [ZA4] - or [L] + [ZA4] - In chemical formula 4, L is a neutral or cationic Lewis base; H is a hydrogen atom; Z is a Group 13 element; and A is each independently a 1-20 Hydrocarbon, C 1-20 Alkoxy or phenoxy substituted C 6-20 Aryl or C 1-20 alkyl.