A method for extracting vanadium from vanadium slag using barium slag as additive
By using barium slag as an additive in the vanadium slag extraction process and optimizing the conditions during roasting and dilute sulfuric acid leaching, the problems of high pollution and low recovery rate in the vanadium slag extraction technology have been solved, and efficient recovery of vanadium resources has been achieved. and environmentally friendly processes.
Patent Information
- Application Number
- CN202211644963.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-12-20
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2042-12-20
AI Technical Summary
The existing vanadium extraction technology from vanadium slag has problems such as high pollution and low vanadium recovery rate. In particular, the calcification oxidation roasting and sodium oxidation roasting processes have problems such as low vanadium conversion rate, difficulty in utilizing waste liquid tailings, and environmental pollution.
Barium slag is used as an additive, which is evenly mixed with vanadium slag and then roasted to produce clinker, which is then leached in dilute sulfuric acid to achieve efficient recovery of vanadium and reuse of tailings. The particle size and roasting conditions are controlled to improve the oxidation rate and leaching of vanadium. Rate.
It significantly reduces the cost of vanadium extraction, achieves efficient recycling of vanadium resources and barium resources, avoids the generation of pollutants, improves the recovery rate and leaching efficiency of vanadium, and the roasting process is environmentally friendly.
Smart Images

Figure CN116103518B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of comprehensive utilization of industrial waste slags, vanadium slag and barium slag, and specifically relates to a method for extracting vanadium from vanadium slag by taking barium slag as an additive. Background Art
[0002] In modern industry, vanadium is used in various fields, especially in steelmaking, non-ferrous alloys, chemical production and batteries, among which more than 80% of vanadium production comes from vanadium slag.
[0003] The existing vanadium extraction processes mainly include sodium oxidation roasting and calcium oxidation roasting. The sodium oxidation roasting vanadium extraction process is the mainstream vanadium slag vanadium extraction method. Although the sodium oxidation roasting vanadium extraction process is relatively mature and has a series of advantages, it also has problems such as environmental pollution, poor raw material applicability, easy ring formation in the rotary kiln, and difficult utilization of waste liquid and tailings. Calcification oxidation roasting vanadium extraction is another vanadium extraction process used in industrial production. It has the advantages of clean and efficient roasting process, strong raw material applicability, and easy recycling of waste liquid and tailings, but there is a problem of low vanadium conversion rate.
[0004] In view of the above-mentioned shortcomings of calcification roasting and sodium roasting, the prior art has overcome the difficulties of low vanadium leaching rate, long leaching time, difficulty in filtering leached ore pulp, serious equipment corrosion and difficulty in using tailings in calcification roasting by treating calcification clinker and adding oxalic acid to optimize vanadium extraction. The prior art also proposes a blank roasting technology. Specifically, no additives are used during roasting, and a low-alkali solution can be added for leaching and then filtered to obtain vanadium liquid and iron-rich tailings. The blank roasting method shortens the time of high-temperature roasting oxidation, reduces energy consumption, avoids ring formation, and improves the conversion rate of vanadium.
[0005] However, there is no method for extracting vanadium from vanadium slag using barium slag as an additive in the prior art. Summary of the invention
[0006] 1. Technical issues to be resolved
[0007] In order to solve the problems of high pollution and low vanadium recovery rate in the prior art of vanadium slag extraction technology, the present invention provides a vanadium extraction method of vanadium slag using barium slag as an additive.
[0008] (II) Technical solution
[0009] In order to achieve the above object, the main technical solutions adopted by the present invention include:
[0010] A method for extracting vanadium from vanadium slag using barium slag as an additive comprises the following steps:
[0011] S1: uniformly mixing the dried and crushed barium slag and the dried and crushed vanadium slag to obtain a mixture;
[0012] S2: roasting the mixture in air to oxidize the trivalent vanadium into pentavalent vanadium to obtain clinker;
[0013] S3: Cool and crush the clinker, then add dilute sulfuric acid for leaching to obtain a leaching solution and leaching tailings.
[0014] In the above step S2, air oxidizes trivalent vanadium in the vanadium slag into pentavalent vanadium, and barium carbonate further reacts with high-valent vanadium to generate carbon dioxide and calcium vanadate. During the process of carbon dioxide gas overflowing, the contact between the reaction product and air can be further increased.
[0015] In the above step S3, the vanadium-containing leaching solution is used to extract vanadium and produce vanadium products, and the leaching tailings can be recycled. The calcium vanadate is leached with dilute sulfuric acid to obtain a vanadium-containing leaching solution and leaching tailings. The vanadium-containing leaching solution can be used to extract vanadium and produce vanadium products, and the leaching tailings can be recycled. Therefore, no pollutants are generated in the entire vanadium slag vanadium extraction process of the present invention, which is very environmentally friendly.
[0016] In the present invention, both barium slag and vanadium slag are industrial wastes. Compared with pure material additives, the cost of using barium slag is very low, which can significantly reduce the cost of vanadium extraction. In addition, the coordinated treatment of barium slag and vanadium slag can also play the role of treating waste with waste, realizing the efficient recycling of vanadium resources and barium resources.
[0017] In order to further improve the roasting efficiency, make the vanadium slag and barium slag fully contact and generate barium vanadate, the present invention needs to control the particle size of the vanadium slag and barium slag particles. In the above-mentioned vanadium slag vanadium extraction method, preferably, in step S1, in terms of mass fraction, in the barium slag, particles with a particle size of less than 74 μm account for more than 80%, and in the vanadium slag, particles with a particle size of less than 74 μm account for more than 80%. The particle size of the vanadium slag and the barium slag is less than 74 μm, which is conducive to full contact and improves the oxidation rate of vanadium in the vanadium slag and the acid leaching recovery rate.
[0018] More preferably, in step S1, in terms of mass fraction, in the barium slag, particles with a particle size of less than 74 μm account for 100%, and in the vanadium slag, particles with a particle size of less than 74 μm account for 100%.
[0019] In the above-mentioned method for extracting vanadium from vanadium slag, preferably, in step S1, the mass fraction of barium carbonate in the barium slag is 25-35%, and the mass fraction of vanadium pentoxide in the vanadium slag is 5-15% calculated as vanadium pentoxide.
[0020] The barium slag used in the present invention has barium carbonate as an effective component, and also contains barium sulfate, barium silicate, silicon dioxide, ferrous oxide, aluminum oxide, etc. The mass fraction of barium carbonate in the barium slag is generally 25-35%, and the presence of silicon dioxide, ferrous oxide and aluminum oxide will affect the leaching of vanadium.
[0021] In addition to vanadium (in terms of vanadium pentoxide), vanadium slag also contains ferric oxide, silicon dioxide, manganese oxide, titanium dioxide, magnesium oxide, aluminum oxide, calcium oxide and chromium oxide, etc. The mass percentage of vanadium pentoxide in vanadium slag is generally 5-15%, among which the presence of ferric oxide, silicon dioxide and titanium dioxide will affect the leaching of vanadium.
[0022] In the above-mentioned vanadium slag vanadium extraction method, preferably, in step S1, the vanadium in the vanadium slag is converted into vanadium pentoxide, and the molar ratio of barium carbonate in the barium slag to vanadium pentoxide in the vanadium slag is 0.25:1-2:1, specifically 0.25:1, 0.5:1, 0.75:1, 1:1, 1.25:1, 1.5:1, 2:1, etc. The above molar ratio of barium carbonate in the barium slag to vanadium pentoxide in the vanadium slag can ensure that the powder particles of the vanadium slag are in contact with the barium carbonate in the barium slag as much as possible, and the generation of calcium vanadate is as low as possible, thereby improving the recovery rate of vanadium and the subsequent leaching rate.
[0023] In the above-mentioned vanadium slag vanadium extraction method, preferably, in step S2, the roasting temperature is 700-950°C, and specifically can be 700°C, 750°C, 800°C, 825°C, 850°C, 875°C, 900°C, 950°C, etc. In the present invention, the roasting temperature of 700-950°C can ensure that the vanadium is oxidized by oxygen as much as possible, thereby improving the recovery rate of vanadium. If the roasting temperature is lower than 700°C, the vanadium slag may not be roasted completely, resulting in a low recovery rate of vanadium.
[0024] In the above-mentioned method for extracting vanadium from vanadium slag, preferably, in step S2, the roasting time is 0.5-2.5 h, specifically 0.5 h, 1 h, 1.5 h, 1.75 h, 2.0 h, 2.25 h, 2.5 h, etc.
[0025] In the above-mentioned vanadium slag vanadium extraction method, preferably, in step S3, the mass fraction of dilute sulfuric acid is 10-40%, specifically 10%, 15%, 20%, 25%, 30%, 35%, 40%, etc. In addition, the particle size of the clinker after cooling and crushing also needs to be kept below 74 μm, that is, it can pass through a 200-mesh sieve. In step S3, controlling the particle size of the clinker after crushing is conducive to the leaching process and to improving the leaching rate of vanadium.
[0026] In the method for extracting vanadium from vanadium slag as described above, preferably, in step S3, the leaching temperature is 65-95°C, specifically 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, etc.
[0027] (III) Beneficial effects
[0028] The beneficial effects of the present invention are:
[0029] The present invention uses barium slag, a byproduct of the barium salt production process, as an additive, and the barium carbonate in the barium slag and the oxidized high-valent vanadium in the vanadium slag generate calcium vanadate, which is then subjected to acid leaching to obtain a leachate and a leach tailing. The vanadium-containing leachate is used to extract vanadium and produce vanadium products, and the leach tailing can be recycled.
[0030] In the present invention, both barium slag and vanadium slag are industrial wastes with a wide range of sources. Compared with pure material additives, the cost of barium slag is very low, which can significantly reduce the cost of vanadium extraction. In addition, the coordinated treatment of barium slag and vanadium slag can also play a role in treating waste with waste, thus realizing the efficient recycling of vanadium resources and barium resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 The XRD diagram of the clinker and the leached tailings in Example 1;
[0032] Figure 2 a-2f is an electron probe scan of the clinker in Example 1;
[0033] Figure 3 a-3e is an electron probe scan of the leached tailings in Example 1. DETAILED DESCRIPTION
[0034] In order to better explain the present invention and facilitate understanding, the present invention is described in detail below through specific implementation modes in conjunction with the accompanying drawings.
[0035] Example 1
[0036] This embodiment provides a method for extracting vanadium from vanadium slag using barium slag as an additive, comprising the following steps:
[0037] S1: crushing and grinding the dried vanadium slag and barium slag to a particle size of less than 74 μm respectively, uniformly mixing the barium slag fine material with the vanadium slag fine material, so that the molar ratio of barium carbonate in the barium slag to vanadium pentoxide in the vanadium slag is 0.5:1, and obtaining a mixture.
[0038] S2: The mixed material is placed in a muffle furnace and roasted at 875° C. for 2 hours to oxidize the trivalent vanadium into pentavalent vanadium to obtain roasted clinker.
[0039] S3: After the clinker is cooled, it is crushed to a particle size of less than 74 μm. 3 g of the roasted clinker is put into a beaker, and 30 ml of a 25% sulfuric acid solution is added according to a solid-liquid ratio of 10:1. The leaching temperature is maintained at 80°C for leaching, and vanadium-containing leaching solution and leaching tailings are obtained.
[0040] The vanadium content in the vanadium-containing leaching solution was detected, and combined with the vanadium content in the vanadium slag, the vanadium leaching rate was calculated to be 98.4%.
[0041] XRD test was performed on the roasted clinker obtained in step S2 and the leached tailings obtained in step S3. The results are as follows: Figure 1 As shown in the figure, the substances that may appear in the roasted clinker and leaching tailings are Figure 1 The bid is Figure 1 It can be seen that the diffraction peak of barium vanadate is detected in the clinker generated after roasting barium slag and vanadium slag. After sulfuric acid leaching, the diffraction peak of barium vanadate disappears, which indicates that barium vanadate is generated in the clinker and the leaching treatment enriches it in the leachate.
[0042] The roasted clinker obtained in step S2 and the leached tailings obtained in step S3 were tested by electron probe. The results are as follows: Figure 2 a-2f and Figure 3 a-3e, where Figure 2 As shown in a, the area where vanadium and barium appear simultaneously is marked.
[0043] Depend on Figure 2 a-2f and Figure 3 From a-3e, it can be seen that the barium element is distributed in the area where the vanadium element in the roasted clinker exists, which indicates that vanadium and barium form barium vanadate, verifying the above XRD analysis results. In addition, only barium element is detected in the leached tailings, and no vanadium element is detected, which also proves that under the optimal conditions of this embodiment, the vanadium in the roasted clinker is enriched in the leaching solution.
[0044] The components and contents of the barium slag used in this embodiment are shown in Table 1, and the components and contents of the vanadium slag are shown in Table 2.
[0045] Table 1 Composition and content of barium slag
[0046]
[0047] Table 2 Composition and content of vanadium slag
[0048]
[0049] It can be seen from Table 1 that the barium slag contains 30.92% BaCO by mass. 3 , 24.33% SiO 2 , 6.83% Al 2 O 3 , 2.71% FeO. The mass fraction of V in vanadium slag is 8.387%. 2 O 5 , 43.49% Fe 2 O 3 14.62% SiO 2 , 10.27% TiO 2 .
[0050] Example 2
[0051] This embodiment provides a method for extracting vanadium from vanadium slag using barium slag as an additive, which is different from Embodiment 1 in that in step S1, the molar ratio of barium carbonate in the barium slag to vanadium pentoxide in the vanadium slag is 0.25:1.
[0052] The vanadium content in the vanadium-containing leaching solution prepared in this example was detected, and combined with the vanadium content in the vanadium slag, the vanadium leaching rate was calculated to be 91.2%.
[0053] Example 3
[0054] This embodiment provides a method for extracting vanadium from vanadium slag using barium slag as an additive, which is different from Embodiment 1 in that, in step S1, the molar ratio of barium carbonate in the barium slag to vanadium pentoxide in the vanadium slag is 1.5:1.
[0055] The vanadium content in the vanadium-containing leaching solution prepared in this example was detected, and combined with the vanadium content in the vanadium slag, the vanadium leaching rate was calculated to be 92.5%.
[0056] Example 4
[0057] This embodiment provides a method for extracting vanadium from vanadium slag using barium slag as an additive, which is different from Embodiment 1 in that in step S2, the roasting temperature is 800°C.
[0058] The vanadium content in the vanadium-containing leaching solution prepared in this example was detected, and combined with the vanadium content in the vanadium slag, the vanadium leaching rate was calculated to be 92.2%.
[0059] Example 5
[0060] This embodiment provides a method for extracting vanadium from vanadium slag using barium slag as an additive, which is different from Embodiment 1 in that in step S2, the roasting temperature is 950°C.
[0061] The vanadium content in the vanadium-containing leaching solution prepared in this example was detected, and combined with the vanadium content in the vanadium slag, the vanadium leaching rate was calculated to be 95.9%.
[0062] Example 6
[0063] This embodiment provides a method for extracting vanadium from vanadium slag using barium slag as an additive, which is different from Embodiment 1 in that in step S2, the roasting time is 1.5 h.
[0064] The vanadium content in the vanadium-containing leaching solution prepared in this example was detected, and combined with the vanadium content in the vanadium slag, the vanadium leaching rate was calculated to be 96.8%.
[0065] Example 7
[0066] This embodiment provides a method for extracting vanadium from vanadium slag using barium slag as an additive, which is different from Embodiment 1 in that in step S2, the roasting time is 2.5 hours.
[0067] The vanadium content in the vanadium-containing leaching solution prepared in this example was detected, and combined with the vanadium content in the vanadium slag, the vanadium leaching rate was calculated to be 98.1%.
[0068] Example 8
[0069] This embodiment provides a method for extracting vanadium from vanadium slag using barium slag as an additive, which is different from Embodiment 1 in that in step S3, the leaching temperature is 65°C.
[0070] The vanadium content in the vanadium-containing leaching solution prepared in this example was detected, and combined with the vanadium content in the vanadium slag, the vanadium leaching rate was calculated to be 97.6%.
[0071] Example 9
[0072] This embodiment provides a method for extracting vanadium from vanadium slag using barium slag as an additive, which is different from Embodiment 1 in that in step S3, the leaching temperature is 95°C.
[0073] The vanadium content in the vanadium-containing leaching solution prepared in this example was detected, and combined with the vanadium content in the vanadium slag, the vanadium leaching rate was calculated to be 98.1%.
[0074] Example 10
[0075] This embodiment provides a method for extracting vanadium from vanadium slag using barium slag as an additive, which is different from Embodiment 1 in that in step S3, the mass fraction of dilute sulfuric acid is 15%.
[0076] The vanadium content in the vanadium-containing leaching solution prepared in this example was detected, and combined with the vanadium content in the vanadium slag, the vanadium leaching rate was calculated to be 96.3%.
[0077] Embodiment 11
[0078] This embodiment provides a method for extracting vanadium from vanadium slag using barium slag as an additive, which is different from Embodiment 1 in that in step S3, the mass fraction of dilute sulfuric acid is 40%.
[0079] The vanadium content in the vanadium-containing leaching solution prepared in this example was detected, and combined with the vanadium content in the vanadium slag, the vanadium leaching rate was calculated to be 97.9%.
[0080] Comparative Example 1
[0081] This comparative example provides a method for extracting vanadium from vanadium slag using barium slag as an additive, comprising the following steps:
[0082] S1: crushing and grinding the dried vanadium slag and barium slag to a particle size of less than 74 μm respectively, uniformly mixing the barium slag fine material with the vanadium slag fine material, so that the molar ratio of barium carbonate in the barium slag to vanadium pentoxide in the vanadium slag is 2.5:1, and obtaining a mixture.
[0083] S2: placing the mixed material into a muffle furnace and roasting it at 800° C. for 2 hours to oxidize the trivalent vanadium into pentavalent vanadium, thereby obtaining roasted clinker.
[0084] S3: After the clinker is cooled, it is crushed to a particle size of less than 74 μm. 3 g of the roasted clinker is put into a beaker, and 30 ml of a 25% sulfuric acid solution is added according to a solid-liquid ratio of 10:1. The leaching temperature is maintained at 80°C for leaching, and vanadium-containing leaching solution and leaching tailings are obtained.
[0085] The vanadium content in the vanadium-containing leaching solution prepared in this comparative example was detected, and combined with the vanadium content in the vanadium slag, the vanadium leaching rate was calculated to be 90.6%.
[0086] Comparative Example 2
[0087] This comparative example provides a method for extracting vanadium from vanadium slag using barium slag as an additive, which is different from Example 1 in that in step S2, the roasting temperature is 650°C.
[0088] The vanadium content in the vanadium-containing leaching solution prepared in this comparative example was detected, and combined with the vanadium content in the vanadium slag, the vanadium leaching rate was calculated to be 89.8%.
[0089] Comparative Example 3
[0090] This comparative example provides a method for extracting vanadium from vanadium slag using barium slag as an additive, which is different from Example 1 in that in step S2, the mass concentration of dilute sulfuric acid is 5%.
[0091] The vanadium content in the vanadium-containing leaching solution prepared in this comparative example was detected, and combined with the vanadium content in the vanadium slag, the vanadium leaching rate was calculated to be 82.3%.
[0092] Comparative Example 4
[0093] This comparative example provides a method for extracting vanadium from vanadium slag using barium carbonate as an additive. The difference from Example 1 is that barium carbonate with a purity of 99.5% is used as an additive, the barium carbonate is finely ground to a particle size of less than 74 μm, and then mixed with the barium slag.
[0094] The vanadium content in the vanadium-containing leaching solution prepared in this comparative example was detected, and combined with the vanadium content in the vanadium slag, the vanadium leaching rate was calculated to be 88.4%.
[0095] The above is only a preferred embodiment of the present invention, and does not limit the present invention in other forms. Any person skilled in the art can use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still belongs to the protection scope of the technical solution of the present invention.
Claims
1. A method for extracting vanadium from vanadium slag using barium slag as an additive, characterized in that: The steps include: S1: uniformly mixing the dried and crushed barium slag and the dried and crushed vanadium slag to obtain a mixture; in this step, the vanadium in the vanadium slag is converted into vanadium pentoxide, and the molar ratio of barium carbonate in the barium slag to vanadium pentoxide in the vanadium slag is 0.25:1-2:1; S2: roasting the mixture in air to oxidize the trivalent vanadium into pentavalent vanadium to obtain clinker; in this step, the roasting temperature is 700-950°C; S3: cooling and crushing the clinker, and then adding dilute sulfuric acid for leaching to obtain a leaching solution and leaching tailings; The barium slag includes BaCO3, BaSO4, BaSiO3, SiO2, Al2O3 and FeO.
2. The method for extracting vanadium from vanadium slag according to claim 1, characterized in that: In step S1, in terms of mass fraction, particles with a particle size of less than 74 μm account for more than 80% of the barium slag, and particles with a particle size of less than 74 μm account for more than 80% of the vanadium slag.
3. The method for extracting vanadium from vanadium slag according to claim 2, characterized in that: In step S1, in terms of mass fraction, in the barium slag, particles with a particle size of less than 74 μm account for 100%, and in the vanadium slag, particles with a particle size of less than 74 μm account for 100%.
4. The method for extracting vanadium from vanadium slag according to claim 1, characterized in that: In step S1, the mass fraction of barium carbonate in the barium slag is 25-35%, and the mass fraction of vanadium pentoxide in the vanadium slag is 5-15% calculated as vanadium pentoxide.
5. The method for extracting vanadium from vanadium slag according to claim 1, characterized in that: In step S2, the calcination time is 0.5-2.5 hours.
6. The vanadium extraction method according to claim 1, characterized in that: In step S3, the mass fraction of dilute sulfuric acid is 10-40%.
7. The vanadium extraction method according to claim 1, characterized in that: In step S3, the leaching temperature is 65-95°C.