Method for resource utilization of all components of smelting slag
By using ammonium salt solution in smelting slag to destroy the combination of Ca-Si and Ca-Fe, combined with magnetic separation and flotation technology, the efficient resource utilization of the entire component of the smelting slag is achieved, and the low resource utilization rate of smelting slag is solved. The problem of CO2 emissions has achieved low carbon and low consumption smelting slag utilization and CO2 emission reduction effects.
Patent Information
- Application Number
- CN202411095150.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
The resource utilization rate of smelting slag is low, especially the residue utilization rate after leaching of calcium and magnesium components, and the CO2 emissions during the smelting process are large, making it difficult to achieve low carbon and low consumption resource utilization.
The smelting slag was leached with an NH4+ concentration of ≤5mol/L to destroy the chemical combination of Ca-Si and Ca-Fe, selectively dissolve the calcium and magnesium components, and separate the iron and silicon components through magnetic separation and flotation. , realize the resource utilization of the entire component of the smelting slag.
It has achieved high efficiency, low carbon, low consumption and harmless and high-value utilization of smelting slag, reduced the consumption of acid and alkali medium and low tailings utilization rate in traditional processes, and has the potential for industrial production.
Smart Images

Figure CN118996129A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for resource utilization of all components of smelting slag, in particular to a method for resource utilization of all components of smelting slag with low carbon and low consumption, belonging to the technical field of comprehensive resource utilization of industrial solid waste. Background Art
[0002] The steel production process produces a large amount of smelting slag such as blast furnace slag, steel slag, and refined slag. The large output of steel slag and the low utilization rate not only occupy a large amount of land, but also cause serious waste of resources and potential ecological environment pollution. The resource utilization of steel slag has become an urgent problem to be solved.
[0003] The existing steel slag resource utilization technology mainly uses it as a building material after fine grinding. However, due to the high content of free calcium oxide (f-CaO) in steel slag, it is easy to cause the volume of building materials to expand, causing quality and structural safety problems.
[0004] In addition, a large amount of CO2 is emitted during the steel production process. Carbon emission reduction is an important challenge facing the high-quality development of the steel industry. The smelting slag has a high content of calcium and magnesium, which can react with CO2 to achieve mineralization and capture of carbon, which is a very promising flue gas carbon capture process.
[0005] The leaching of calcium and magnesium components in smelting slag is a prerequisite for efficient mineralization of CO2. Existing literature has published some methods for leaching calcium and magnesium components in smelting slag. Jo, et al., (Energy, 2017, 884–894) and Tian, et al., (Chem. Sus. Chem., 2015, 3839–3846) used HCl and HNO3 to extract calcium-containing components in steel slag respectively. The study found that although inorganic acid can quickly dissociate calcium and magnesium minerals in smelting slag and achieve the leaching of most of the calcium and magnesium in the smelting slag, a large amount of metal elements will also be leached at the same time. The leachate needs to be treated for impurities before the utilization of all components can be achieved. Chang et al., (ACS Sustain. Chem. Eng., 2012) used short-chain fatty acids to leach calcium-containing components in smelting slag. The existing process mainly focuses on the calcium and magnesium dissolution process. After the calcium and magnesium are dissolved, a large amount of leached slag is produced, and its resource utilization is the key to the utilization of all components of steel slag. However, there are few reports on the low-carbon and low-consumption resource utilization of all components of steel slag. Summary of the invention
[0006] In view of the problems that existing smelting slag is difficult to be recycled and the utilization rate of smelting slag leaching residue is low, the purpose of the invention is to provide a method for recycling all components of smelting slag. This method utilizes the different occurrence forms of calcium, magnesium, iron and silicon components in smelting slag, extracts the carbon-fixing components in smelting slag by solution leaching, and uses a mineral processing process to separate the iron and silicon components, thereby realizing the recycling of all components. This method has the characteristics of low carbon, low consumption and high efficiency, and provides a new way for the harmless, high-value and large-scale utilization of smelting slag.
[0007] In order to achieve the above technical purpose, the present invention provides a method for resource utilization of all components of smelting slag, the method is to use NH4 + The smelting slag is leached with an ammonium salt solution with a concentration of ≤5 mol / L to obtain a calcium-magnesium leaching solution and leaching slag; the leaching slag is separated into an iron-containing component and a silicon-containing component by flotation and / or magnetic separation.
[0008] In the technical solution of the present invention, the dissolution of calcium and magnesium components and the separation of iron and silicon components are the key to the resource utilization of all components of steel slag. The chemical and mineral phase composition of smelting slag is complex, and the main components are Ca, Si, Fe, Mg, etc. These components exist in the form of oxides or silicates, respectively. The content of calcium silicate and calcium ferrite in smelting slag is relatively high, that is, Ca is combined with Si and Fe to form minerals, respectively, and the Fe-Si phase mineral phase is less. Therefore, if calcium is selectively dissolved to destroy the chemical combination of Ca-Si and Ca-Fe, the dissociation of silicon-containing components and iron-containing components from calcium can be achieved. Therefore, the present invention proposes to first use an ammonium salt solution to destroy the chemical combination of Ca-Si and Ca-Fe, and selectively dissolve the calcium and magnesium components in the smelting slag.
[0009] The principle of the technical solution of the present invention is that: first, the ammonium ions in the ammonium salt solution can directly replace the free calcium and magnesium oxides in the smelting slag to form water-soluble calcium chloride and magnesium chloride, thereby achieving the initial leaching of calcium and magnesium components; then, by adjusting NH4 +The concentration can further destroy the chemical bond between metal ions and oxygen atoms in the bound calcium silicate, calcium ferrite and magnesium silicate, promote the dissolution of calcium ions and magnesium ions in the leaching system, and then deeply destroy the chemical bond of Ca-Si and Ca-Fe, and realize the leaching of the bound calcium and magnesium components while releasing and separating the iron and silicon components. After the above treatment, the main components in the leached residue are iron oxide and silicon oxide. The present invention further uses magnetic separation and / or flotation to separate iron oxide and silicon oxide based on the characteristics of the occurrence form and embedding relationship of iron and silicon. Compared with silicon oxide, iron oxide has the characteristics of high density, high conductivity and strong magnetism, and can be separated by magnetic separation. In addition, the surface physical and chemical properties of iron oxide and silicon oxide, such as surface potential and cleavage plane, are significantly different. After the leached residue is slurried by adding water, the separation of iron oxide and silicon oxide can be achieved by adding an appropriate amount of collector. It is further preferred that magnetic separation and flotation are carried out simultaneously.
[0010] In the process of dissolving calcium and magnesium components of the present invention, a high concentration of the ammonium salt solution will cause the calcium and magnesium components in the smelting slag to be leached while iron, aluminum and other components will also be leached, resulting in a decrease in the selectivity of the calcium and magnesium components in the leaching process, and the iron component will also be lost. A low solution concentration will lead to insufficient dissolution of calcium and magnesium, and some calcium and magnesium components will remain in the dissolving slag, affecting the subsequent separation effect of iron and silicon components.
[0011] As a preferred solution, the flotation uses at least one of carboxylic acid agents, halogenated fatty acid agents, sulfonated fatty acid agents, amine agents, quaternary ammonium agents, potassium dodecyl hydroxamate, sodium dodecyl sulfate, and sodium dodecyl acetate as a flotation collector; the addition amount of the flotation collector is 20 to 2000 g / t.
[0012] Further preferably, the carboxylic acid agent is at least one of oleic acid, lauric acid, caprylic acid, capric acid, dodecanoic acid, and tetradecanoic acid, the halogenated fatty acid agent is at least one of RA-315, RA-515, RA-715, and RA-915, the sulfonated fatty acid agent is at least one of sodium dodecylbenzene sulfonate and sodium dodecyl sulfonate, the amine agent is at least one of quaternary ammonium agent, sodium acetate octadecylamide, sodium acetate ether diamine, and ether amine, and the quaternary ammonium agent is at least one of dodecyl trimethyl ammonium bromide and dodecyl ammonium chloride. Further, preferably at least one of lauric acid, sodium acetate octadecylamide and RA-315. The dosage of the agent of the present invention is large, and there are many bubbles in the flotation process. Although the recovery rate of the target mineral can be improved, it is inevitable that other minerals are floated by bubbles, resulting in a decrease in the grade of the flotation concentrate. On the contrary, a certain amount of the target mineral cannot be separated and enters the tailings, resulting in a waste of the target mineral and a decrease in the flotation recovery rate.
[0013] As a preferred solution, the smelting slag includes at least one of blast furnace slag, electric furnace slag, converter slag and ladle refined slag, and the preferred smelting slag contains rich calcium and magnesium components.
[0014] As a preferred solution, the smelting slag is classified according to the cooling method, including at least one of water-quenched slag, hot-splashed slag, air-quenched slag, drum slag, granulated slag, and hot-stifled slag.
[0015] As a preferred solution, the average particle size of the smelting slag after crushing and screening is controlled to be ≤3 mm. If the average particle size of the smelting slag is too coarse, the solid-liquid reaction rate and diffusion rate of the smelting slag leaching process will be seriously reduced, affecting the leaching rate of calcium and magnesium components, resulting in slow leaching rate and low leaching rate.
[0016] As a preferred embodiment, the ammonium salt solution is NH4 + At least one of ammonium chloride, ammonium sulfate and ammonium nitrate with a concentration of 0.1 to 5 mol / l. + Within the concentration range, it can not only ensure the efficient and highly selective leaching of calcium and magnesium bound to the smelting slag, but also avoid the leaching of other metal components. The present invention makes full use of the NH4 + It destroys the chemical bonds between metal ions and oxygen atoms in the bound calcium silicate and magnesium silicate in the smelting slag, and promotes the dissolution of calcium ions and magnesium ions in the leaching system.
[0017] As a preferred solution, the leaching is at least one of conventional leaching, cross-current leaching and countercurrent leaching.
[0018] As a preferred scheme, the leaching conditions are: the mass ratio of smelting slag and leaching agent is 1: (1-20), the leaching temperature is 10-90°C, and stirring is used to assist leaching. The amount of leaching agent determines the leaching rate of calcium and magnesium components in the smelting slag. Properly increasing the amount of leaching agent is conducive to improving the leaching rate of calcium and magnesium components, but when the amount of leaching agent is too high, it will cause a large amount of leaching of components such as iron, thereby increasing the leaching cost and reducing the leaching rate of calcium and magnesium components and the leaching selectivity of calcium and magnesium components. The leaching temperature has a significant effect on the leaching rate. If the leaching temperature is too low, the reaction rate will be slow, affecting the leaching efficiency. Properly increasing the temperature is conducive to improving the leaching rate, but too high a leaching temperature will accelerate the volatilization of the acid solution or ammonium salt solution, which will have an adverse effect on the leaching. Within the preferred temperature range of the present invention, the leaching efficiency of calcium and magnesium components in the smelting slag is relatively good. Stirring can improve the solid-liquid contact effect and improve the leaching efficiency. The stirring method used is at least one of mechanical stirring, airflow stirring, ultrasound, and oscillation.
[0019] As a preferred solution, the magnetic field strength of the magnetic separation is 80-1600 kA / m. Under the preferred magnetic field strength, effective separation of iron and silicon components can be achieved with high efficiency.
[0020] As a preferred solution, the calcium-magnesium leaching solution is used as a calcium-containing chemical raw material after being used for flue gas carbon capture or purification.
[0021] As a preferred solution, the iron-containing components separated from the leached slag are used as raw materials for steel production or iron product processing, and the silicon-containing components are used as building materials or raw materials for silicon-containing product production.
[0022] Compared with the prior art, the technical solution of the present invention has the following beneficial technical effects:
[0023] 1) The low-carbon utilization method of smelting slag of the present invention cleverly utilizes the current situation of high content of calcium and magnesium components and low utilization rate in smelting slag, combined with the characteristics of large CO2 emissions from smelting enterprises, and utilizes the calcium and magnesium components in the smelting slag to mineralize the flue gas CO2, and develops cross-current, countercurrent leaching and other efficient selective leaching processes for calcium and magnesium components, thereby realizing smelting slag utilization and CO2 emission reduction.
[0024] 2) The low-consumption utilization method of smelting slag of the present invention cleverly utilizes the characteristics of the close binding of Ca-Si and Ca-Fe in the smelting slag, selectively dissolves the calcium-containing component by using an ammonium salt solution, destroys the binding of Ca-Si and Ca-Fe, and reduces the association between the iron-containing component and the silicon-containing component, thereby creating favorable conditions for the subsequent separation of iron and silicon, and reducing the material and energy consumption of the magnetic separation or flotation separation recovery process.
[0025] 3) The method for utilizing all components of smelting slag of the present invention cleverly utilizes the principles of mineral processing and metallurgical engineering. Based on the material composition characteristics of the smelting slag, the components in the smelting slag are orderly separated and recycled separately through the mineral processing process, which effectively reduces the problems of large acid and alkali medium consumption and low tailings utilization rate in traditional processes, and is conducive to the efficient and high-quality utilization of smelting slag.
[0026] 4) The present invention requires a small amount of leaching medium and a short processing process, and has the potential for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a process flow chart for the method of resource utilization of all components of smelting slag. DETAILED DESCRIPTION
[0028] In order to facilitate the understanding of the present invention, the present invention will be described in more comprehensive and detailed manner in conjunction with preferred embodiments below, but the protection scope of the present invention is not limited to the following specific embodiments.
[0029] Unless otherwise defined, all the professional terms used below have the same meanings as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.
[0030] Unless otherwise specified, all reagents and raw materials used in the present invention are commercially available products or products that can be prepared by known methods.
[0031] In the following examples, converter slag is used as raw material, and its main components are CaO, SiO2, Fe2O3, MgO, etc. The specific components are shown in Table 1.
[0032] Table 1 Chemical composition of converter slag (%)
[0033]
[0034] Example 1
[0035] The converter slag was crushed and sieved to obtain particles with an average particle size of ≤3 mm. A 3 mol / l ammonium nitrate solution was used as the leaching medium. The mass ratio of converter slag to ammonium nitrate solution was maintained at 1:4. The countercurrent leaching temperature was 30 °C, mechanical stirring was performed, and the speed was 100 rpm. After the leaching was completed, the leaching was filtered and the Ca in the leaching solution was detected by ICP. 2+ Mg 2+ Concentration, calculated based on the initial content in converter slag, Ca 2+ Mg 2+ The leaching rates are 87.9% and 73.7% respectively. Using sodium acetate octadecylamide as flotation agent, the dosage is 50g / t, the iron content of the obtained iron-containing component is 64.7%, and the SiO2 content of the silicon-containing component is 93.7%.
[0036] Example 2
[0037] The converter slag was crushed and sieved to obtain particles with an average particle size of ≤3 mm. Ammonium chloride was used as the leaching medium with a concentration of 0.1 mol / l. The mass ratio of converter slag to ammonium chloride solution was maintained at 1:6. The leaching temperature was 25°C, and the mixture was shaken and stirred. After the leaching was completed, the leaching solution was filtered and the Ca content in the leaching solution was detected. 2+ Mg 2+ Concentration, calculated based on the initial content in converter slag, Ca 2+ Mg 2+ The leaching rates are 96.7% and 92.4% respectively. Lauric acid is used as a flotation agent at a dosage of 2000 g / t. The iron content of the obtained iron-containing component is 68.2%, and the SiO2 content of the silicon-containing component is 91.1%.
[0038] Example 3
[0039] The converter slag was crushed and sieved to obtain particles with an average particle size of ≤3 mm. A 5 mol / l ammonium chloride solution was used as the leaching medium. The mass ratio of converter slag to ammonium chloride solution was maintained at 1:20. The leaching temperature was 80 °C, mechanical stirring was performed, and the speed was 150 rpm. Cross-flow leaching was performed. After the leaching was completed, the leaching solution was filtered and the Ca content in the leaching solution was detected. 2+ Mg 2+ Concentration, calculated based on the initial content in converter slag, Ca 2+ Mg 2+ The leaching rates were 85.1% and 87.1% respectively. The iron-containing components in the leached slag were recovered by strong magnetic separation, with a magnetic field strength of 1600 kA / m. The iron grade of the obtained iron-containing components was 57.9%, and the SiO2 content of the silicon-containing components was 89.8%.
[0040] Example 4
[0041] The converter slag was crushed and sieved to obtain particles with an average particle size of ≤3 mm. 4 mol / l ammonium chloride was used as the leaching medium. The mass ratio of converter slag to ammonium chloride solution was maintained at 1:3. The leaching level was 3, the leaching temperature was 10 °C, the N2 gas flow was stirred, and the gas flow velocity was 1.0 m 3 / (min·m 2 ), countercurrent leaching, filtering after completion of inflow and outflow, and detecting Ca in the leaching solution 2+ Mg 2+ Concentration, calculated based on the initial content in converter slag, Ca 2+ Mg 2+ The leaching rates are 92.4% and 87.5% respectively. The iron-containing components in the leached residue are recovered by magnetic separation-flotation combined process, the magnetic field intensity is 80kA / m, RA-315 is used as reagent, the dosage is 20g / t, the iron grade of the obtained iron-containing components is 68.9%, and the SiO2 content of the silicon-containing components is 98.5%.
[0042] Comparative Example 1
[0043] Compared with Example 1, the only difference is that the concentration of the ammonium nitrate solution is 8 mol / l.
[0044] The final Ca 2+ Mg 2+ The leaching rates were 90.1% and 74.4%, respectively, and Ca 2+ Mg 2+ The leaching rate is slightly higher than that in Example 1, but the iron grade of the iron-containing component after separation of the leached slag is 43.7%, and the SiO2 content of the silicon-containing component is 67.1%, both of which are significantly lower than those in Example 1.
[0045] Comparative Example 2
[0046] Compared with Example 3, the only difference is that the mass ratio of converter slag to ammonium chloride solution is 1:25.
[0047] The final Ca 2+ Mg 2+ The leaching rates were 89.8% and 71.5% respectively. The solution dosage was too high, and the free calcium and magnesium dissolved quickly at the beginning of leaching, but in the subsequent leaching process, the excess leaching solution combined with the iron-containing components, causing a large amount of iron to dissolve, resulting in the iron grade of the iron-containing component being 44.1% and the SiO2 content of the silicon-containing component being 70.0% after the leaching slag was separated.
[0048] Comparative Example 3
[0049] Compared with Example 2, the only difference is that the average particle size of converter slag is greater than 3 mm.
[0050] The final Ca 2+ Mg 2+ The leaching rates were 82.5% and 67.4% respectively. After separation of the leached slag, the iron content of the iron component was 48.9%, and the content of SiO2 of the silicon component was 73.3%. The increase in particle size seriously reduced the solid-liquid reaction and diffusion rate during the leaching process, resulting in Ca 2+ Mg 2+ The leaching rate is greatly reduced, and the iron and silicon parts in the leached slag are in a coated state, resulting in poor separation effect.
[0051] Comparative Example 4
[0052] Compared with Example 2, the only difference is that the leached residue is separated by gravity separation.
[0053] The final Ca 2+ Mg 2+ The leaching rate is the same as that of Example 2. However, due to the small difference in specific gravity between the iron-containing component and the silicon-containing component, gravity separation is difficult, resulting in the iron grade of the iron-containing component obtained after leaching slag separation being 38.5%, and the SiO2 content of the silicon-containing component being 61.8%.
Claims
1. A method for resource utilization of all components of smelting slag, characterized by: NH4 + The smelting slag is leached with an ammonium salt solution with a concentration of ≤5 mol / L to obtain a calcium-magnesium leaching solution and leaching slag; the leaching slag is separated by flotation and / or magnetic separation to obtain an iron-containing component and a silicon-containing component.
2. The method for resource utilization of all components of smelting slag according to claim 1, characterized in that: The smelting slag includes at least one of blast furnace slag, electric furnace slag, converter slag and ladle refining slag.
3. The method for resource utilization of all components of smelting slag according to claim 2, characterized in that: The average particle size of the smelting slag is ≤3mm.
4. The method for resource utilization of all components of smelting slag according to claim 1, characterized in that: The ammonium salt solution is NH4 + At least one of ammonium chloride, ammonium sulfate and ammonium nitrate with a concentration of 0.1 to 5 mol / L.
5. The method for resource utilization of all components of smelting slag according to claim 1, characterized in that: The leaching is at least one of conventional leaching, cross-current leaching and countercurrent leaching.
6. The method for resource utilization of all components of smelting slag according to claim 5, characterized in that: The leaching conditions are as follows: the mass ratio of smelting slag to leaching agent is 1:(1-20), the leaching temperature is 10-90° C., and stirring is used to assist leaching.
7. The method for resource utilization of all components of smelting slag according to claim 1, characterized in that: The magnetic field strength of the magnetic separation is 80-1600 kA / m.
8. The method for resource utilization of all components of smelting slag according to claim 7, characterized in that: The flotation adopts at least one of carboxylic acid agents, halogenated fatty acid agents, sulfonated fatty acid agents, amine agents, quaternary ammonium agents, potassium dodecyl hydroxamate, sodium dodecyl sulfate, and sodium dodecyl acetate as a flotation collector; the addition amount of the flotation collector is 20-2000g / t.
9. A method for resource utilization of all components of smelting slag according to any one of claims 1 to 8, characterized in that: The calcium and magnesium leaching solution is used as a calcium-containing chemical raw material after being used for flue gas carbon capture or purification; The iron-containing component is used as raw material for steel production or iron product processing; The silicon-containing component is used as a raw material for producing building materials or silicon-containing products.
Citation Information
Cited By
Smelting slag high-efficiency low-consumption leaching method based on ammonium salt leaching agent circulation
CN120099291A
A high-efficiency and low-consumption leaching method for smelting slag based on ammonium salt leaching agent circulation
CN120099291B
Efficient resource utilization method for smelting slag calcium and magnesium leaching tailings