Hot rolled steel plate
By controlling the chemical composition and metal structure of the hot-rolled steel plate, the problem of difficulty in achieving high strength and excellent shear processability is solved, a tensile strength of more than 780MPa and stable shear processability are achieved, and the occurrence of cracks within bending is suppressed. Occurrence, suitable for automobiles and mechanical components.
Patent Information
- Application Number
- CN202180052468.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2020-08-27
- Filing Date
- 2021-06-15
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2041-06-15
AI Technical Summary
The existing technology is difficult to provide high strength above 780MPa and excellent shearing processability, especially in terms of stability of shearing end surface collapse after shearing processing.
By controlling the chemical composition and metal structure of the hot-rolled steel plate, including preferred martensite or bainite structure, controlling the standard deviation of the Mn concentration, austenite recrystallization and cooling conditions in the hot rolling process, periodic and uneven formation is achieved The metal structure ensures the tensile strength reaches above 780MPa and stabilizes the shear processability.
It achieves high strength and excellent shear workability while suppressing the occurrence of cracks within bends, making it suitable as an industrial raw material for automotive components and mechanical structures.
Smart Images

Figure CN116113716B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a hot-rolled steel sheet, and more specifically to a hot-rolled steel sheet that can be formed into various shapes by press working or the like, and more particularly to a hot-rolled steel sheet that has high strength and excellent shear workability.
[0002] This application claims priority based on Japanese Patent Application No. 2020-143746 filed on August 27, 2020, the contents of which are cited here. Background Art
[0003] In recent years, from the perspective of protecting the global environment, many fields are trying to reduce carbon dioxide emissions. Even automobile manufacturers are actively developing technologies to reduce vehicle weight for the purpose of reducing fuel consumption. However, since the focus is on improving collision resistance in order to ensure the safety of passengers, it is not easy to reduce the weight of the vehicle.
[0004] In order to balance the lightweight of the vehicle body with the collision resistance, the use of high-strength steel plates to make the components thinner is being studied. Therefore, there is an urgent need for steel plates that have both high strength and excellent formability, and several technologies have been proposed in the past to meet these requirements. Automobile components are formed by press forming, but the press-formed blank plates are mostly manufactured by shearing with high productivity. Since the clearance in the blank processing is not necessarily fixed, it is preferred that the end face accuracy after shearing is stable even if there are multiple clearances. For example, it is preferred that the ratio of the collapsed edge in the sheared end face after shearing is stable and does not depend on the clearance.
[0005] Regarding shear workability, for example, Patent Document 1 discloses a method of increasing the ferrite grain size d of the surface layer by s and the internal ferrite grains d b The ratio of d s / d b The technology of controlling the burr height after punching by controlling it below 0.95.
[0006] Patent Document 2 discloses a technique for improving peeling and curling of the sheet end surface by reducing the P content.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Laid-Open No. 10-168544
[0010] Patent Document 2: Japanese Patent Application Publication No. 2005-298924
[0011] Non-patent literature
[0012] Non-patent document 1: J. Webel, J. Gola, D. Britz, F. Mucklich, Materials Characterization 144 (2018) 584-596
[0013] Non-patent document 2: DL Naik, HU Sajid, R. Kiran, Metals 2019, 9, 546
[0014] Non-patent document 3: K. Zuiderveld, Contrast Limited Adaptive Histogram Equalization, Chapter VIII.5, Graphics Gems IV. PS Heckbert (Eds.), Cambridge, MA, Academic Press, 1994, pp. 474-485 Summary of the invention
[0015] Problems to be solved by the invention
[0016] However, Patent Document 1 targets IF steel and may be difficult to apply to high-strength members of 780 MPa or more. Patent Document 2, although a strength of 780 MPa or more is obtained, does not study the stability of the collapse of the sheared end surface after shearing.
[0017] The present invention has been made in view of the above-mentioned problems in the prior art, and an object of the present invention is to provide a hot-rolled steel sheet having high strength and excellent shear workability.
[0018] Means for solving problems
[0019] In view of the above problems, the inventors of the present invention have repeatedly conducted intensive research on the chemical composition and metal structure of hot-rolled steel sheets and the relationship between mechanical properties. As a result, the following insights (a) to (f) were obtained, thereby completing the present invention. In addition, the term "excellent shear workability" means that the ratio of the collapsed edge in the sheared end surface after shearing is stable regardless of the clearance during shearing. In addition, the term "excellent strength" or "high strength" means that the tensile strength is 780 MPa or more.
[0020] (a) In order to obtain excellent tensile (maximum) strength, it is preferred to use a hard structure. In other words, it is preferred that the metal structure contains martensite or bainite.
[0021] (b) In order to stabilize the edge collapse ratio at the shear edge, it is important to form a metal structure with less Mn segregation, a periodic structure morphology, and a non-uniform (low uniformity) structure.
[0022] (c) Specifically, setting the standard deviation of the Mn concentration to a certain value or less and controlling the periodicity and uniformity of the metal structure are effective in stabilizing the edge collapse ratio in the sheared end surface.
[0023] (d) In order to set the standard deviation of the Mn concentration to a certain value or less, the slab heating process and the subsequent hot rolling process are important. For example, it is effective to hold the temperature in the temperature range of 700 to 850°C for more than 900 seconds, then heat again, hold the temperature in the temperature range of 1100°C or more for more than 6000 seconds, and perform hot rolling in the temperature range of 850°C to 1100°C in such a way that the plate thickness is reduced by a total of 90% or more.
[0024] (e) It is important to control the recrystallization behavior of austenite during hot rolling to improve the periodicity of the metal structure. For example, it is effective to control the reduction rate and rolling temperature in the final stage of hot rolling within a specified range, set the stress applied to the steel plate after the first stage of hot rolling and before the final stage of rolling to 170 kPa or more, and set the stress applied to the steel plate after the final stage of hot rolling and until the steel plate is cooled to 750°C to 200 kPa or more. According to such hot rolling conditions, fine and flat austenite grains can be implanted, and by combining with the subsequent cooling conditions, the periodicity of the metal structure can be improved.
[0025] (f) To reduce the uniformity of the metal structure, it is effective to promote the precipitation of iron carbides by coiling after cooling to a temperature range of 400°C or more and less than 600°C.
[0026] The gist of the present invention completed based on the above findings is as follows.
[0027] (1) One aspect of the present invention relates to a hot-rolled steel sheet, characterized in that:
[0028] The chemical composition contains by mass %:
[0029] C: 0.050~0.250%,
[0030] Si: 0.05-3.00%,
[0031] Mn: 1.00~4.00%,
[0032] One or more of Ti, Nb and V: 0.060 to 0.500% in total,
[0033] Sol.Al: 0.001~2.000%,
[0034] P: 0.100% or less,
[0035] S: 0.0300% or less,
[0036] N: 0.1000% or less,
[0037] O: 0.0100% or less,
[0038] Cu: 0-2.00%,
[0039] Cr: 0~2.00%,
[0040] Mo: 0-1.00%,
[0041] Ni: 0-2.00%,
[0042] B: 0~0.0100%,
[0043] Ca: 0~0.0200%,
[0044] Mg: 0~0.0200%,
[0045] REM: 0~0.1000%、
[0046] Bi: 0~0.020%,
[0047] One or more of Zr, Co, Zn and W: 0 to 1.00% in total, and
[0048] Sn: 0~0.05%,
[0049] The remainder includes Fe and impurities;
[0050] The metal structure is expressed in area % as follows:
[0051] Retained austenite is less than 3.0%, ferrite is less than 15.0%, and pearlite is less than 5.0%;
[0052] The E value indicating the periodicity of the metal structure is lower than 10.7, and the I value indicating the uniformity of the metal structure is lower than 1.020;
[0053] The standard deviation of the Mn concentration is 0.60 mass % or less;
[0054] The tensile strength is above 780 MPa.
[0055] (2) The hot-rolled steel sheet according to (1) above, wherein the ratio of the average grain size ds of the surface layer to the average grain size dq at a depth of 1 / 4 of the sheet thickness from the surface, i.e., ds / dq, may be 0.95 or less.
[0056] (3) The hot-rolled steel sheet according to (1) or (2) above, wherein the chemical composition may contain, in terms of mass %, one or more elements selected from the following:
[0057] Cu: 0.01-2.00%,
[0058] Cr: 0.01~2.00%,
[0059] Mo: 0.01~1.00%,
[0060] Ni: 0.02-2.00%,
[0061] B: 0.0001~0.0100%,
[0062] Ca: 0.0005~0.0200%,
[0063] Mg: 0.0005~0.0200%,
[0064] REM: 0.0005~0.1000%, and
[0065] Bi: 0.0005~0.020%.
[0066] Effects of the Invention
[0067] According to the above embodiment of the present invention, a hot rolled steel sheet having excellent strength and shear workability can be obtained. In addition, according to the above preferred embodiment of the present invention, a hot rolled steel sheet having the above characteristics and excellent bending internal crack resistance can be obtained while suppressing the occurrence of bending internal cracks.
[0068] The hot-rolled steel sheet according to the above aspect of the present invention is suitable as an industrial raw material for automobile components, mechanical structural parts and building components. BRIEF DESCRIPTION OF THE DRAWINGS
[0069] Figure 1 This is a diagram for explaining a method for measuring the edge collapse ratio in a sheared end surface after shearing. DETAILED DESCRIPTION
[0070] The chemical composition and metal structure of the hot-rolled steel sheet (hereinafter sometimes simply referred to as steel sheet) involved in this embodiment are specifically described below. However, the present invention is not limited to the configuration disclosed in this embodiment, and various changes can be made within the scope of the purpose of the present invention.
[0071] In the following numerical ranges between "-", the lower limit and the upper limit are included in the range. In the numerical values expressed as "lower than" or "exceed", the value is not included in the numerical range. In the following description, % of the chemical composition of the steel plate is mass % unless otherwise specified.
[0072] 1. Chemical composition
[0073] The hot-rolled steel sheet according to the present embodiment contains, by mass%, C: 0.050-0.250%, Si: 0.05-3.00%, Mn: 1.00-4.00%, one or more of Ti, Nb and V: 0.060-0.500% in total, sol.Al: 0.001-2.000%, P: 0.100% or less, S: 0.0300% or less, N: 0.1000% or less, O: 0.0100% or less, and the remainder: Fe and impurities. Each element is described in detail below.
[0074] (1-1) C: 0.050~0.250%
[0075] C can increase the fraction of hard phases and increase the strength of ferrite by combining with precipitation strengthening elements such as Ti, Nb, and V. If the C content is less than 0.050%, it is difficult to obtain the desired strength. In addition, the stability of the collapsed edge in the shear end face is reduced. Therefore, the C content is set to 0.050% or more. The C content is preferably 0.060% or more, more preferably 0.070% or more, and further preferably 0.080% or more.
[0076] On the other hand, if the C content exceeds 0.250%, the weldability of the hot-rolled steel sheet decreases. Therefore, the C content is set to 0.250% or less. The C content is preferably 0.150% or less.
[0077] (1-2) Si: 0.05-3.00%
[0078] Si has the effect of improving the strength of hot rolled steel sheets by solid solution strengthening. In addition, Si has the effect of making steel sound by deoxidation (suppressing defects such as pores in steel). If the Si content is less than 0.05%, the above effects cannot be obtained. Therefore, the Si content is set to 0.05% or more. The Si content is preferably 0.50% or more, and more preferably 0.80% or more.
[0079] However, if the Si content exceeds 3.00%, the surface properties and chemical conversion treatment properties of the hot-rolled steel sheet, and further the ductility and weldability, are significantly deteriorated, and the A3 transformation point is significantly increased. As a result, it is difficult to perform hot rolling stably. In addition, the stability of the collapsed edge in the shear end face is reduced. Therefore, the Si content is set to 3.00% or less. The Si content is preferably 2.70% or less, and more preferably 2.50% or less.
[0080] (1-3) Mn: 1.00~4.00%
[0081] Mn has the effect of increasing the strength of hot rolled steel sheets by inhibiting ferrite transformation. If the Mn content is less than 1.00%, a tensile strength of 780 MPa or more cannot be obtained. In addition, the stability of the collapsed edge in the shear end face decreases. Therefore, the Mn content is set to 1.00% or more. The Mn content is preferably 1.30% or more, and more preferably 1.50% or more.
[0082] On the other hand, if the Mn content exceeds 4.00%, cracks will occur near the center of the plate thickness due to the central segregation of Mn, and the shear end surface properties after shearing will deteriorate. Therefore, the Mn content is set to 4.00% or less. The Mn content is preferably 3.70% or less, and more preferably 3.50% or less.
[0083] (1-4) One or more of Ti, Nb and V: 0.060 to 0.500% in total
[0084] Ti, Nb and V are elements that precipitate finely in steel in the form of carbides and nitrides, and improve the strength of steel through precipitation strengthening. In addition, they are also elements that fix C by forming the above-mentioned carbides, thereby suppressing the formation of cementite that is harmful to shear workability. If the total content of Ti, Nb and V is less than 0.060%, these effects cannot be obtained. Therefore, the total content of Ti, Nb and V is set to more than 0.060%. Furthermore, it is not necessary to contain all of Ti, Nb and V, and even any one of them can contain more than 0.060%. When containing two or more of Ti, Nb and V, their total content is preferably more than 0.060%. The total content of Ti, Nb and V is preferably more than 0.080%, and more preferably more than 0.100%.
[0085] On the other hand, if the total content of Ti, Nb and V exceeds 0.500%, the workability of the hot-rolled steel sheet deteriorates. Therefore, the total content of Ti, Nb and V is set to 0.500% or less, preferably 0.300% or less, more preferably 0.250% or less, and further preferably 0.200% or less.
[0086] (1-5)sol.Al: 0.001~2.000%
[0087] Al, like Si, has the function of improving the soundness of steel by deoxidizing it. If the sol.Al content is less than 0.001%, the effect based on the above function cannot be obtained. Therefore, the sol.Al content is set to 0.001% or more. The sol.Al content is preferably 0.010% or more.
[0088] On the other hand, if the sol.Al content exceeds 2.000%, the above effect is saturated and it is not economically preferable, so the sol.Al content is set to 2.000% or less. The sol.Al content is preferably 1.500% or less, more preferably 1.300% or less, and further preferably 1.000% or less.
[0089] In addition, the so-called sol.Al means acid-soluble Al, and refers to solid-solution Al existing in the steel in a solid-solution state.
[0090] (1-6) P: 0.100% or less
[0091] P is an element usually contained as an impurity, but it is also an element that has the effect of improving the strength of hot-rolled steel sheets by solid solution strengthening. Therefore, P can also be actively contained, but P is an element that is easy to segregate. If the P content exceeds 0.100%, the ductility caused by grain boundary segregation decreases significantly. Therefore, the P content is set to 0.100% or less. The P content is preferably 0.030% or less. The lower limit of the P content does not need to be specifically specified, but from the perspective of refining cost, it is preferably set to 0.001%.
[0092] (1-7) S: 0.0300% or less
[0093] S is an element contained as an impurity, and forms sulfide-based inclusions in steel, thereby reducing the ductility of the hot-rolled steel sheet. If the S content exceeds 0.0300%, the ductility of the hot-rolled steel sheet is significantly reduced. Therefore, the S content is set to 0.0300% or less. The S content is preferably 0.0050% or less. The lower limit of the S content does not need to be particularly specified, but from the viewpoint of refining cost, it is preferably set to 0.0001%.
[0094] (1-8) N: 0.1000% or less
[0095] N is an element contained in steel as an impurity, and has the effect of reducing the ductility of hot-rolled steel sheets. If the N content exceeds 0.1000%, the ductility of the hot-rolled steel sheet decreases significantly. Therefore, the N content is set to 0.1000% or less. The N content is preferably 0.0800% or less, more preferably 0.0700% or less, and further preferably 0.0100% or less. The lower limit of the N content does not need to be specifically specified, but in the case of making the metal structure finer by containing one or more of Ti, Nb and V, in order to promote the precipitation of carbonitrides, the N content is preferably set to 0.0010% or more, and more preferably 0.0020% or more.
[0096] (1-9) O: 0.0100% or less
[0097] If O is contained in a large amount in steel, it forms coarse oxides that serve as fracture starting points, causing brittle fracture and hydrogen cracking. Therefore, the O content is set to 0.0100% or less. The O content is preferably 0.0080% or less, and more preferably 0.0050% or less. In order to disperse fine oxides in large quantities during deoxidation of molten steel, the O content may be set to 0.0005% or more or 0.0010% or more.
[0098] The remainder of the chemical composition of the hot-rolled steel sheet involved in the present embodiment may also be Fe and impurities. In the present embodiment, the so-called impurities refer to impurities mixed from the ore and scrap steel materials as raw materials or the manufacturing environment, and / or impurities allowed within the range that do not have adverse effects on the hot-rolled steel sheet involved in the present embodiment.
[0099] The hot-rolled steel sheet according to the present embodiment may also contain Cu, Cr, Mo, Ni, B, Ca, Mg, REM, Bi, Zr, Co, Zn, W and Sn as arbitrary elements instead of a part of Fe. The lower limit of the content when the above arbitrary elements are not contained is 0%. The above arbitrary elements are described in detail below.
[0100] (1-10)Cu: 0.01~2.00%, Cr: 0.01~2.00%, Mo: 0.01~1.00%, Ni: 0.02~2.00% and B: 0.0001~0.0100%
[0101] Cu, Cr, Mo, Ni and B all have the effect of improving the hardenability of hot-rolled steel sheets. In addition, Cu and Mo have the effect of improving the strength of hot-rolled steel sheets by precipitating as carbides in steel. In addition, when Ni contains Cu, it has the effect of effectively suppressing the grain boundary cracks of the slab caused by Cu. Therefore, one or more of these elements may also be contained.
[0102] Cu has the effect of improving the hardenability of hot-rolled steel sheets and the effect of improving the strength of hot-rolled steel sheets by precipitating carbides in steel at low temperatures. In order to more reliably obtain the effects based on the above effects, the Cu content is preferably set to 0.01% or more, and more preferably to 0.05% or more. However, if the Cu content exceeds 2.00%, grain boundary cracks sometimes occur in the slab. Therefore, the Cu content is set to 2.00% or less. The Cu content is preferably 1.50% or less, and more preferably 1.00% or less.
[0103] As mentioned above, Cr has the effect of improving the hardenability of hot-rolled steel sheets. In order to more reliably obtain the above-mentioned effect, it is preferred that the Cr content be set to 0.01% or more, and more preferably to 0.05% or more. However, if the Cr content exceeds 2.00%, the chemical conversion treatability of the hot-rolled steel sheet will be significantly reduced. Therefore, the Cr content is set to 2.00% or less.
[0104] As mentioned above, Mo has the effect of improving the hardenability of hot-rolled steel sheets and the effect of improving the strength of hot-rolled steel sheets by precipitating carbides in steel. In order to more reliably obtain the effects of the above effects, it is preferred that the Mo content be set to 0.01% or more, and more preferably to 0.02% or more. However, even if the Mo content is set to more than 1.00%, the effects based on the above effects are saturated, which is not economically preferred. Therefore, the Mo content is set to 1.00% or less. The Mo content is preferably 0.50% or less, and more preferably 0.20% or less.
[0105] As mentioned above, Ni has the effect of improving the hardenability of hot-rolled steel sheets. In addition, when Ni contains Cu, it has the effect of effectively suppressing the grain boundary cracks of the slab caused by Cu. In order to more reliably obtain the effect based on the above-mentioned effect, it is preferred to set the Ni content to 0.02% or more. Since Ni is a high-priced element, it is not economically preferable to contain a large amount of Ni. Therefore, the Ni content is set to 2.00% or less.
[0106] As mentioned above, B has the effect of improving the hardenability of hot-rolled steel sheets. In order to more reliably obtain the effect based on this effect, it is preferred that the B content be set to 0.0001% or more, and more preferably to 0.0002% or more. However, if the B content exceeds 0.0100%, the formability of the hot-rolled steel sheet is significantly reduced, so the B content is set to 0.0100% or less. It is preferred that the B content be set to 0.0050% or less.
[0107] (1-11) Ca: 0.0005 to 0.0200%, Mg: 0.0005 to 0.0200%, REM: 0.0005 to 0.1000%, and Bi: 0.0005 to 0.020%
[0108] Ca, Mg and REM all have the effect of improving the ductility of hot-rolled steel sheets by adjusting the shape of inclusions in steel to a preferred shape. In addition, Bi has the effect of improving the ductility of hot-rolled steel sheets by refining the solidification structure. Therefore, one or more of these elements may also be contained. In order to more reliably obtain the effect based on the above-mentioned effects, it is preferred to set the content of any one or more of Ca, Mg, REM and Bi to 0.0005% or more. However, if the Ca content or the Mg content exceeds 0.0200%, or the REM content exceeds 0.1000%, inclusions are excessively generated in the steel, which sometimes reduces the ductility of the hot-rolled steel sheet. In addition, even if the Bi content is set to more than 0.020%, the effect of the above-mentioned effect is saturated, which is not economically preferred. Therefore, the Ca content and the Mg content are set to less than 0.0200%, the REM content is set to less than 0.1000%, and the Bi content is set to less than 0.020%. The Bi content is preferably less than 0.010%.
[0109] Here, REM refers to a total of 17 elements including Sc, Y and lanthanoid elements, and the above REM content refers to the total content of these elements. In the case of lanthanoid elements, they are added in the form of mixed rare earth in industry.
[0110] (1-12) One or more of Zr, Co, Zn and W: 0 to 1.00% in total and Sn: 0 to 0.05%
[0111] Regarding Zr, Co, Zn and W, the present inventors have confirmed that even if these elements are contained in a total amount of 1.00% or less, the effect of the hot-rolled steel sheet according to the present embodiment is not impaired. Therefore, one or more of Zr, Co, Zn and W may be contained in a total amount of 1.00% or less.
[0112] The present inventors have also confirmed that even if a small amount of Sn is contained, the effect of the hot-rolled steel sheet according to the present embodiment is not impaired. However, if a large amount of Sn is contained, defects may occur during hot rolling, so the Sn content is set to 0.05% or less.
[0113] The chemical composition of the hot-rolled steel sheet can be measured by ordinary analytical methods. For example, ICP-AES (Inductively Coupled Plasma-Atomic Emission Spectrometry) can be used for measurement. Furthermore, sol.Al can be measured by ICP-AES using the filtrate after the sample is heated and decomposed with acid. C and S can be measured by the combustion-infrared absorption method, N can be measured by the inert gas melting-thermal conductivity method, and O can be measured by the inert gas melting-non-dispersive infrared absorption method.
[0114] 2. Metal structure of hot rolled steel plate
[0115] Next, the metal structure of the hot-rolled steel sheet according to the present embodiment will be described.
[0116] In the hot-rolled steel sheet involved in the present embodiment, the metal structure is less than 3.0% of retained austenite, less than 15.0% of ferrite, less than 5.0% of pearlite in terms of area %, the E value indicating the periodicity of the above-mentioned metal structure is less than 10.7, the I value indicating the uniformity of the above-mentioned metal structure is less than 1.020, and the standard deviation of the Mn concentration is less than 0.60 mass %. Therefore, the hot-rolled steel sheet involved in the present embodiment can obtain high strength and excellent shear workability. Furthermore, in the present embodiment, in the plate thickness section parallel to the rolling direction, the standard deviation of the structure fraction, E value, I value and Mn concentration in the metal structure at a depth position of 1 / 4 of the plate thickness from the surface is specified. The reason is that the metal structure in this position represents a representative metal structure of the steel plate.
[0117] (2-1) Area fraction of retained austenite: less than 3.0%
[0118] In the present invention, if the area fraction of retained austenite is too large, the edge collapse ratio in the shear end face sometimes becomes unstable. Retained austenite improves the work hardening energy of the hot-rolled steel sheet through transformation induced plasticity (TRIP), so it is speculated that the edge collapse ratio in the shear end face is unstable. If the area fraction of retained austenite is 3.0% or more, the shear workability of the hot-rolled steel sheet deteriorates. Therefore, the area fraction of retained austenite is set to less than 3.0%. The area fraction of retained austenite is preferably less than 1.5%, and more preferably less than 1.0%. Since the less retained austenite, the better, the area fraction of retained austenite can also be 0%.
[0119] The area fraction of retained austenite can be measured by X-ray diffraction, EBSP (Electron Back Scattering Diffraction Pattern) analysis, magnetic measurement, etc., and the measured value may differ depending on the measurement method. In the present embodiment, the area fraction of retained austenite is measured by X-ray diffraction.
[0120] In the measurement of the area fraction of retained austenite based on X-ray diffraction in the present embodiment, Co-Kα rays are used at a depth position of 1 / 4 of the plate thickness of the hot-rolled steel plate (the region from 1 / 8 of the plate thickness from the surface to 3 / 8 of the plate thickness from the surface) to obtain the cumulative intensity of a total of 6 peaks of α(110), α(200), α(211), γ(111), γ(200), and γ(220), and the area fraction of retained austenite is calculated by using the intensity averaging method.
[0121] (2-2) Area fraction of ferrite: less than 15.0%
[0122] Ferrite is a structure formed when fcc phase transforms to bcc at a relatively high temperature. Ferrite has high work hardening ability, so if the area fraction of ferrite is too high, the collapse ratio in the shear end face becomes unstable. Therefore, the area fraction of ferrite is set to less than 15.0%. It is preferably less than 12.0%, more preferably less than 10.0%, and further preferably less than 8.0%. The lower the area fraction of ferrite, the better. The lower limit of the area fraction of ferrite can also be 3.0%, 2.0% or 0%.
[0123] (2-3) Area fraction of pearlite: less than 5.0%
[0124] Pearlite is a metal structure in which cementite is precipitated in layers between ferrite. In addition, pearlite is a softer metal structure than bainite and martensite. If the area fraction of pearlite is 5.0% or more, the cementite contained in the pearlite consumes carbon, and the strength of the remaining structure, i.e., martensite and bainite, decreases, and a tensile strength of 780 MPa or more cannot be obtained. Therefore, the area fraction of pearlite is set to less than 5.0%. The area fraction of pearlite is preferably 3.0% or less. In order to improve the stretch flangeability of the hot-rolled steel sheet, it is preferred to reduce the area fraction of pearlite as much as possible, and the lower limit of the area fraction of pearlite is preferably 2.0%, more preferably 1.0%, and further preferably 0%.
[0125] Furthermore, in the hot-rolled steel sheet according to the present embodiment, as the remaining structure other than retained austenite, ferrite, and pearlite, a hard structure composed of one or more of bainite, martensite, and tempered martensite may be included.
[0126] The area fraction of the metal structure is measured in the following manner. The plate thickness section parallel to the rolling direction is finished into a mirror surface and polished with colloidal silica without alkaline solution at room temperature for 8 minutes to remove the strain introduced into the surface layer of the sample. At any position in the length direction of the sample section, an area with a length of 50 μm and a depth of 1 / 4 of the plate thickness from the surface (an area with a depth of 1 / 8 of the plate thickness from the surface to a depth of 3 / 8 of the plate thickness from the surface) is measured by electron backscatter diffraction at a measurement interval of 0.1 μm to obtain crystal orientation information. In the measurement, an EBSD analysis device consisting of a thermal field emission scanning electron microscope (JSM-7001F manufactured by JEOL) and an EBSD detector (DVC5 detector manufactured by TSL) is used. At this time, the vacuum degree in the EBSD analysis device is set to 9.6×10 -5 Pa or less, set the acceleration voltage to 15kV, set the irradiation current level to 13, and set the irradiation level of the electron beam to 62. In addition, take a backscattered electron image in the same field of view. First, from the backscattered electron image, identify the grains in which ferrite and cementite are precipitated in layers, calculate the area fraction of the grains, and thus obtain the area fraction of pearlite. Then, for grains other than the grains identified as pearlite, the "Grain Average Misorientation: Grain Average Orientation Difference" function of the software "OIM Analysis (registered trademark)" attached to the EBSD analysis device is used to analyze the obtained crystal orientation information, and the area with a Grain Average Misorientation value of less than 1.0° is identified as ferrite. The area fraction of ferrite is obtained by calculating the area fraction of the area identified as ferrite.
[0127] Next, in the remaining area (area where the Grain Average Misorientation value exceeds 1.0°), under the condition that the 5° grain boundary is defined as the grain boundary, when the maximum value of the "Grain Average IQ" of the ferrite area is set to Iα, the area exceeding Iα / 2 is extracted as bainite, and the area below Iα / 2 is extracted as "pearlite, martensite and tempered martensite". The area fraction of bainite is obtained by calculating the area ratio of the extracted bainite. In addition, the area fraction of pearlite obtained by the above EBSD analysis is subtracted from the area fraction of the extracted "pearlite, martensite and tempered martensite" to obtain the total area ratio of martensite and tempered martensite.
[0128] (2-4) E value: less than 10.7, I value: less than 1.020
[0129] In order to stabilize the edge collapse ratio in the sheared end surface after shearing, it is important to increase the periodicity of the metal structure and reduce the uniformity of the metal structure. In this embodiment, the edge collapse ratio in the sheared end surface can be stabilized by controlling the E (Entropy) value representing the periodicity of the metal structure and the I (Inverce differenced moment norm) value representing the uniformity of the metal structure.
[0130] The E value represents the periodicity of the metal structure. When the brightness is arranged periodically due to the formation of a banded structure, that is, when the periodicity of the metal structure is high, the E value decreases. In the present embodiment, since it is necessary to form a metal structure with high periodicity, it is necessary to reduce the E value. If the E value is above 10.7, the ratio of the collapsed edge in the shear end face is prone to change and difficult to stabilize. It is inferred that by forming a metal structure arranged periodically, the work hardening energy is reduced, thereby facilitating the stabilization of the ratio of the collapsed edge in the shear end face. Therefore, the E value is set to be lower than 10.7, preferably below 10.6, and more preferably below 10.5. The lower the E value, the more preferred it is. There is no particular lower limit, and it can also be set to be above 8.0, above 9.0, or above 10.0.
[0131] The I value represents the uniformity of the metal structure. The larger the area of the region with a certain brightness, the higher the I value. A low I value means that the uniformity of the metal structure is low. In the present embodiment, since it is necessary to form a metal structure with low uniformity of the metal structure, it is necessary to reduce the I value. If the I value is low and the uniformity of the metal structure is low, the work hardening energy is reduced, so the ratio of the collapsed edge in the shear end face can be stabilized. It is inferred that if the I value is greater than 1.020, the ratio of the collapsed edge in the shear end face cannot be stabilized. Therefore, the I value is set to less than 1.020, preferably less than 1.015, and more preferably less than 1.010. The lower limit of the I value is not particularly specified, and it can also be set to more than 0.900, more than 0.950, or more than 1.000.
[0132] The E value and I value can be obtained by the following method.
[0133] In this embodiment, the shooting area of the SEM image taken for calculating the E value and the I value is set to a depth position of 1 / 4 of the plate thickness from the surface of the steel plate in the plate thickness section parallel to the rolling direction (an area from 1 / 8 of the plate thickness to 3 / 8 of the plate thickness from the surface). In shooting the SEM image, a SU-6600 Schottky electron gun manufactured by Hitachi High-Technologies Corporation is used, the emitter is set to tungsten, and the acceleration voltage is set to 1.5 kV. Based on the above settings, the SEM image is output at a magnification of 1000 times and 256 levels of grayscale.
[0134] Next, the obtained SEM image was cut into 880×880 pixel areas, and the cut images were subjected to the smoothing process described in Non-Patent Document 3, with the contrast enhancement limit magnification set to 2.0 and the block size set to 8×8. The smoothed SEM image was rotated counterclockwise from 0 to 179 degrees at every degree except 90 degrees, and images were created at every degree, thereby obtaining a total of 179 images. Next, for each of these 179 images, the GLCM method described in Non-Patent Document 1 was used to collect the frequency values of the brightness between adjacent pixels in the form of rows and columns.
[0135] Let k be the rotation angle from the original image, and express the rows and columns of the 179 frequency values collected by the above method as p k (k = 0 to 89, 91 to 179). For each image, the generated p k After the sum is calculated, a 256×256 matrix P is normalized so that the sum of each component is 1. In addition, the E value and the I value are calculated using the following formula (1) and formula (2) described in Non-Patent Document 2, respectively. In the following formula (1) and formula (2), the value of the i-th row and j-th column of the matrix P is represented as P ij .
[0136] [Formula 1]
[0137]
[0138] [Formula 2]
[0139]
[0140] (2-5) Standard deviation of Mn concentration: 0.60 mass % or less
[0141] The standard deviation of the Mn concentration at a depth of 1 / 4 of the plate thickness from the surface of the hot-rolled steel sheet involved in the present embodiment is 0.60% by mass or less. As a result, the ratio of collapsed edge in the shear end face can be stabilized. It is speculated that this is because in the periodically arranged structure of the metal structure, by uniformly dispersing the hard phase, the work hardening energy can be reduced. The standard deviation of the Mn concentration is preferably 0.50% by mass or less, and more preferably 0.47% by mass or less. The lower limit of the standard deviation of the Mn concentration is preferably smaller from the viewpoint of suppressing excessive burrs, but due to the constraints of the manufacturing process, the actual lower limit is 0.10% by mass.
[0142] After the thickness section (L section) of the hot-rolled steel plate parallel to the rolling direction is mirror-polished, the position of the steel plate at a depth of 1 / 4 of the plate thickness from the surface (the area from 1 / 8 of the plate thickness to 3 / 8 of the plate thickness from the surface) is measured by an electron probe microanalyzer (EPMA) to determine the standard deviation of the Mn concentration. The measurement conditions set the acceleration voltage to 15 kV, the magnification to 5000 times, and measure the distribution image in the range of 20 μm in the rolling direction of the sample and 20 μm in the plate thickness direction and the plate width direction of the sample. More specifically, the measurement interval is set to 0.1 μm, and the Mn concentration is measured at more than 40,000 locations. Next, the standard deviation is calculated based on the Mn concentration obtained from the total measurement points, thereby obtaining the standard deviation of the Mn concentration.
[0143] (2-6) The ratio of the average grain size ds of the surface layer to the average grain size dq at a depth of 1 / 4 of the plate thickness from the surface, i.e., ds / dq, is 0.95 or less.
[0144] By refining the grain size of the surface layer, the inner cracks in the bend of the hot-rolled steel sheet can be suppressed. The higher the strength of the hot-rolled steel sheet, the easier it is for cracks to form from the inside of the bend during the bending process (hereinafter referred to as inner cracks in the bend). The mechanism of the inner cracks in the bend is inferred to be as follows. Compressive stress is generated on the inside of the bend during the bending process. Initially, the entire inside of the bend is deformed uniformly while the processing is progressing. However, if the processing amount increases, the deformation cannot be borne by uniform deformation alone, and the deformation continues to progress (a shear deformation band occurs) due to the local concentration of strain. The shear deformation band further grows and cracks occur and grow along the shear band from the inner surface of the bend. The reason why inner cracks in the bend are prone to occur with high strength is inferred to be because the deformation develops unevenly due to the decrease in work hardening energy associated with high strength, thereby generating a shear deformation band in the early stage of processing (or under slow processing conditions).
[0145] The inventors of the present invention have found that the finer the grain size of the surface layer of the hot-rolled steel sheet, the more the local strain concentration is suppressed, and the more difficult it is to generate bending internal cracks. In order to obtain the above-mentioned effect, it is preferred that the ratio of the average grain size ds of the surface layer of the hot-rolled steel sheet to the average grain size dq at a depth of 1 / 4 of the plate thickness from the surface, i.e., ds / dq, is set to 0.95 or less. ds / dq is more preferably less than 0.90, and further preferably less than 0.85. The lower limit of ds / dq is not particularly specified, and may also be set to 0.50 or more.
[0146] In addition, the surface layer in the present embodiment refers to a region from the surface of the hot-rolled steel sheet to a depth of 50 μm from the surface.
[0147] The grain size of the surface layer can be measured by EBSP-OIM (Electron Back Scatter Diffraction Pattern-Orientation Image Microscopy). The EBSP-OIM method is performed using a device that combines a scanning electron microscope and an EBSP analysis device and OIM Analysis (registered trademark) manufactured by AMETEK. The analyzable area of the EBSP-OIM method is the area that can be observed by SEM. Although it also depends on the resolution of the SEM, the EBSP-OIM method can be analyzed with a minimum resolution of 20nm.
[0148] In the thickness section of the hot-rolled steel sheet parallel to the rolling direction, in the surface layer of the hot-rolled steel sheet (the area from the surface of the hot-rolled steel sheet to a depth of 50 μm from the surface) and the 1 / 4 depth position from the surface (the area from 1 / 8 of the thickness from the surface to 3 / 8 of the thickness from the surface), the analysis was performed at least in 5 fields of view in an area of 40 μm × 30 μm at a magnification of 1200 times, and the place where the angle difference between adjacent measurement points was 5° or more was defined as the grain boundary, and the area average grain size was calculated. The area average grain size obtained at each measurement position was used as the average grain size of the surface layer and the average grain size at a depth of 1 / 4 from the surface.
[0149] 3. Tensile strength characteristics
[0150] The tensile strength characteristics (tensile strength) among the mechanical properties of the hot-rolled steel sheet were evaluated in accordance with JIS Z2241: 2011. The test piece was a No. 5 test piece of JIS Z2241: 2011. The test direction was a direction perpendicular to the rolling direction.
[0151] The tensile (maximum) strength of the hot-rolled steel sheet of the present embodiment is 780 MPa or more, preferably 980 MPa or more. If the tensile strength is lower than 780 MPa, the applicable parts are limited, and the contribution to the lightweighting of the vehicle body is small. The upper limit does not need to be particularly limited, but from the perspective of suppressing die wear, it can also be set to 1780 MPa.
[0152] 4.Plate thickness
[0153] The plate thickness of the hot-rolled steel plate involved in the present embodiment is not particularly limited, but can also be set to 1.2 to 8.0 mm. If the plate thickness of the hot-rolled steel plate is less than 1.2 mm, it is difficult to ensure the rolling end temperature, and the rolling load is too large, and hot rolling is sometimes difficult. Therefore, the plate thickness of the hot-rolled steel plate involved in the present embodiment can also be set to more than 1.2 mm, preferably more than 1.4 mm. On the other hand, if the plate thickness exceeds 8.0 mm, it is difficult to refine the metal structure, and sometimes it is difficult to obtain the above-mentioned metal structure. Therefore, the plate thickness can also be set to less than 8.0 mm, preferably less than 6.0 mm.
[0154] 5. Others
[0155] (5-1) Plating
[0156] The hot-rolled steel sheet with the above-mentioned chemical composition and metal structure involved in the present embodiment can also be formed into a surface-treated steel sheet by having a coating on the surface for the purpose of improving corrosion resistance, etc. The coating can be an electroplated layer or a hot-dip coating. As the electroplated layer, electrogalvanizing, electroplating Zn-Ni alloy, etc. can be exemplified. As the hot-dip coating, hot-dip galvanizing, alloyed hot-dip galvanizing, hot-dip aluminum plating, hot-dip Zn-Al alloy plating, hot-dip Zn-Al-Mg alloy plating, hot-dip Zn-Al-Mg-Si alloy plating, etc. can be exemplified. The coating adhesion amount is not particularly limited and can be the same as before. In addition, by implementing appropriate chemical conversion treatment (such as coating and drying of chromium-free chemical conversion treatment liquid of silicate system) after plating, corrosion resistance can be further improved.
[0157] 6. Manufacturing conditions
[0158] A preferred method for producing the hot-rolled steel sheet having the above-mentioned chemical composition and metal structure according to the present embodiment is as follows.
[0159] In order to obtain the hot-rolled steel sheet according to the present embodiment, an effective method is to heat the slab under predetermined conditions, perform hot rolling, accelerate cooling to a predetermined temperature range, and then perform slow cooling, thereby controlling the cooling process until coiling.
[0160] In the preferred method for manufacturing the hot-rolled steel sheet according to the present embodiment, the following steps (1) to (8) are performed in sequence. The slab temperature and the steel sheet temperature in the present embodiment refer to the slab surface temperature and the steel sheet surface temperature. In addition, the stress refers to the stress applied to the steel sheet in the rolling direction.
[0161] (1) After the slab is held in a temperature range of 700 to 850° C. for 900 seconds or more, it is heated again and held in a temperature range of 1100° C. or more for 6000 seconds or more.
[0162] (2) Hot rolling is performed in a temperature range of 850 to 1100° C. so that the plate thickness is reduced by a total of 90% or more.
[0163] (3) After the first step of rolling before the final step of hot rolling and before the final step of rolling, a stress of 170 kPa or more is applied to the steel sheet.
[0164] (4) The hot rolling is completed so that the reduction ratio in the final stage of the hot rolling is set to 8% or more and the rolling end temperature Tf is equal to or higher than the temperature T1 (°C) represented by the following formula (A) and lower than 900°C.
[0165] (5) After hot rolling in the final stage and before the steel sheet is cooled to 750° C., the stress applied to the steel sheet is set to 200 kPa or more.
[0166] (6) After the hot rolling is completed, the steel is accelerated cooled to a temperature of 600° C. or less at an average cooling rate of 50° C. / sec. More preferably, the steel is cooled to a temperature range of the hot rolling end temperature Tf-50° C. or less within 1 second after the hot rolling is completed.
[0167] (7) The residence time in the temperature range of 600 to 730° C. is set to 3.0 seconds or less.
[0168] (8) Coiling is performed in a temperature range of 400°C or higher and lower than 600°C.
[0169] T1(℃)=868-396×[C]-68.1×[Mn]+24.6×[Si]-36.1×[Ni]-24.8×[Cr]-20.7×[Cu]+250×[sol.Al] (A)
[0170] In the above formula (A), [element symbol] represents the content (mass %) of each element in steel. If the element is not contained, it is entered as 0.
[0171] By adopting the above-mentioned manufacturing method, a hot-rolled steel sheet having a metal structure with excellent strength and shear workability can be stably manufactured. That is, by appropriately controlling the slab heating conditions and hot rolling conditions, it is possible to reduce the Mn segregation and flatten the austenite before the transformation, and by combining it with the cooling conditions after the hot rolling described later, it is possible to stably manufacture a hot-rolled steel sheet having a metal structure with excellent strength and shear workability.
[0172] (1) Slab temperature and holding time during hot rolling
[0173] The slabs for hot rolling can be slabs obtained by continuous casting and slabs obtained by casting and slab opening, etc., and the slabs that have been hot-worked or cold-worked can be used as needed. The slabs for hot rolling are preferably kept in a temperature range of 700 to 850°C for more than 900 seconds when the slabs are heated, and then heated again and kept in a temperature range of 1100°C or more for more than 6000 seconds. Furthermore, during the maintenance of the temperature range of 700 to 850°C, the temperature of the steel plate can be changed in the temperature range, or it can be set to be fixed. In addition, during the maintenance of more than 1100°C, the temperature of the steel plate can be changed in the temperature range of more than 1100°C, or it can be set to be fixed. In the austenite transformation in the temperature range of 700 to 850°C, Mn can be diffused along the ferrite region by distributing Mn between ferrite and austenite and extending its phase transformation time. As a result, the Mn microsegregation that is unevenly present in the slab can be eliminated, and the standard deviation of the Mn concentration can be significantly reduced. Furthermore, by maintaining the slab in a temperature range of 1100° C. or higher for 6000 seconds or longer, the austenite grains can be made uniform during the slab heating.
[0174] Hot rolling is preferably performed by a reversing mill or a tandem mill as a multi-pass rolling. In particular, from the viewpoint of industrial productivity and the stress load on the steel sheet during rolling, it is more preferable to perform hot rolling by a tandem mill at least in the final two stages.
[0175] (2) Hot rolling reduction rate: The total thickness of the plate is reduced by more than 90% in the temperature range of 850-1100°C
[0176] By hot rolling in a temperature range of 850 to 1100°C, the plate thickness is reduced by a total of 90% or more, and the recrystallized austenite grains can be mainly refined, while promoting the accumulation of strain energy in the non-recrystallized austenite grains. In addition, while promoting the recrystallization of austenite, the atomic diffusion of Mn can also be promoted, and the standard deviation of the Mn concentration can be reduced. Therefore, it is preferred to hot roll in a temperature range of 850 to 1100°C, in which the plate thickness is reduced by a total of 90% or more.
[0177] Furthermore, the so-called plate thickness thinning in the temperature zone of 850 to 1100°C can be expressed by {(t0-t1) / t0}×100(%) when the entrance plate thickness before the initial rolling in the rolling in this temperature zone is set to t0 and the exit plate thickness after the final stage rolling in the rolling in this temperature zone is set to t1.
[0178] (3) Load stress after the first stage of hot rolling and before the final stage of rolling: 170 kPa or more
[0179] It is preferable to set the stress applied to the steel sheet after the first stage of rolling before the final stage of hot rolling to 170 kPa or more. As a result, the {110} <001> The number of grains with the crystal orientation of {110} <001> Since it is a crystal orientation that is difficult to recrystallize, recrystallization based on the final stage of pressing can be effectively suppressed by promoting the formation of this crystal orientation. As a result, a metal structure with a preferably controlled E value can be obtained. The stress applied to the steel sheet is more preferably 190 kPa or more. The stress applied to the steel sheet can be controlled by adjusting the roll speed in the tandem rolling.
[0180] (4) Reduction ratio in the final stage of hot rolling: 8% or more, hot rolling end temperature Tf: T1 (°C) or more and less than 900°C
[0181] It is preferred to set the reduction rate in the final stage of hot rolling to 8% or more, and set the hot rolling end temperature Tf to T1 (°C) or more. By setting the reduction rate in the final stage of hot rolling to 8% or more, the austenite grains can be flattened by the reduction in the final stage, forming a banded structure of the hot-rolled steel sheet, improving the periodicity of the metal structure, and reducing the E value. By setting the hot rolling end temperature Tf to T1 (°C) or more, the excessive increase in the number of ferrite nucleation sites in austenite can be suppressed. As a result, the formation of ferrite in the final structure (the metal structure of the hot-rolled steel sheet after manufacture) can be suppressed, and a high-strength hot-rolled steel sheet can be obtained. In addition, by setting Tf to less than 900°C, the recrystallization and coarsening of austenite can be suppressed, the periodicity of the metal structure can be improved, and a metal structure with preferably controlled E value can be obtained.
[0182] (5) Load stress after hot rolling and until the steel plate is cooled to 750°C: 200 kPa or more
[0183] It is preferred that the stress applied to the steel plate after rolling in the final stage of hot rolling and until the steel plate is cooled to 750°C is set to 200 kPa or more. By setting the stress applied to the steel plate to 200 kPa or more, the flattening of austenite progresses, and the periodicity of the metal structure can be improved. As a result, a metal structure with a preferably controlled E value can be obtained.
[0184] (6) After the hot rolling is completed, the temperature is accelerated to a temperature range of 600°C or less at an average cooling rate of 50°C / s or more, and more preferably, the temperature is cooled to a temperature range of 50°C or less at the hot rolling end temperature Tf within 1 second after the hot rolling is completed.
[0185] In order to suppress the growth of austenite grains refined by hot rolling, it is more preferable to cool by 50°C or more within 1 second after the hot rolling is completed. In order to cool to a temperature range below the hot rolling end temperature Tf-50°C within 1 second after the hot rolling is completed, it is best to perform cooling with a high average cooling rate immediately after the hot rolling is completed, for example, cooling water can be sprayed on the steel plate surface. By cooling to a temperature range below Tf-50°C within 1 second after the hot rolling is completed, the grain size of the surface layer can be refined, and the bending internal crack resistance can be improved.
[0186] In addition, after the hot rolling is completed, the formation of ferrite and pearlite with small precipitation strengthening can be suppressed by accelerating the cooling to a temperature range below 600°C at an average cooling rate of 50°C / second or more. Thus, the strength of the hot-rolled steel sheet is improved. Furthermore, the average cooling rate mentioned here refers to the temperature drop of the steel sheet from the start of accelerated cooling (when the steel sheet is introduced into the cooling equipment) to the end of accelerated cooling (when the steel sheet is exported from the cooling equipment), divided by the time required from the start of accelerated cooling to the end of accelerated cooling.
[0187] There is no particular upper limit on the cooling rate, but if the cooling rate is increased, the cooling equipment will be large-scale, which will increase the equipment cost. Therefore, considering the equipment cost, it is preferably 300°C / second or less. In addition, the cooling stop temperature of the accelerated cooling can be set to 400°C or more in consideration of the relationship with the coiling temperature.
[0188] (7) Retention time in the temperature range of 600-730°C: less than 3.0 seconds
[0189] In order to obtain a tensile strength of 780 MPa or more by suppressing the formation of ferrite and pearlite and making the parent phase structure hard, it is preferred that the retention time in the ferrite transformation temperature range, i.e., the temperature range of 600 to 730°C, be set to 3.0 seconds or less. More preferably, the retention time in the temperature range of 600 to 730°C is set to 2.0 seconds or less.
[0190] (7) Coiling temperature: above 400°C and below 600°C
[0191] The coiling temperature is set to a temperature range of 400° C. or higher and lower than 600° C. By setting the coiling temperature to this temperature range, the precipitation amount of iron carbides can be increased and the deviation of the hardness distribution in the hard phase can be improved. As a result, the I value can be reduced and excellent shear workability can be obtained.
[0192] Example
[0193] Next, the effects of one embodiment of the present invention are described in more detail through an embodiment, but the conditions in the embodiment are a conditional example adopted to confirm the feasibility and effect of the present invention, and the present invention is not limited to this conditional example. The present invention can adopt a variety of conditions within the scope of achieving the purpose of the present invention without departing from the gist of the present invention.
[0194] Steels having the chemical compositions shown in Tables 1 and 2 were melted and continuously cast to produce slabs having a thickness of 240 to 300 mm. The obtained slabs were used to produce hot-rolled steel sheets shown in Tables 4A and 4B under the production conditions shown in Tables 3A and 3B.
[0195] The obtained hot rolled steel sheet was subjected to the above method to obtain the area fraction of the metal structure, the E value, the I value, the standard deviation of the Mn concentration, the ratio of the average crystal grain size ds of the surface layer to the average crystal grain size dq at a depth of 1 / 4 of the plate thickness from the surface, i.e., ds / dq, and the tensile strength TS. The obtained measurement results are shown in Table 4A and Table 4B.
[0196] Furthermore, the remainder of the structure is one or two or more of bainite, martensite and tempered martensite.
[0197] Evaluation method of characteristics of hot-rolled steel sheets
[0198] (1) Tensile strength characteristics
[0199] When the tensile strength TS is 780 MPa or more, the hot-rolled steel sheet is judged as being excellent in strength and is qualified. On the other hand, when the tensile strength TS is less than 780 MPa, the hot-rolled steel sheet is judged as being poor in strength and is unqualified.
[0200] (2) Shear processability
[0201] The shear workability of hot-rolled steel sheets was evaluated by blanking tests to determine the edge collapse ratio (edge collapse ratio) in the end face after blanking. Three punching holes with a clearance of 10% and 20% were made at a hole diameter of 10 mm and a blanking speed of 3 m / s. Then, the state of the end face parallel to the rolling direction (each punching hole has two end faces) of each punching hole was photographed under an optical microscope. In the obtained observation photos, it can be observed that Figure 1 (a) as shown in the end face. Figure 1 As shown in (a) and (b), the edge collapse, shear surface, fracture surface and burr can be observed on the end surface after punching. Figure 1 (a) is a schematic diagram of the end face of the punched hole parallel to the rolling direction. Figure 1(b) is a schematic diagram of the side of the punched hole. The so-called collapsed edge is an R-shaped smooth surface, the so-called shear surface is a punched end surface separated by shear deformation, the so-called fracture surface is a punched end surface separated by a crack generated near the blade tip after the shear deformation is completed, and the so-called burr is a surface with a protrusion protruding from the bottom of the hot-rolled steel plate. In the observation photograph of the obtained end surface, the collapsed edge ratio in the end surface is measured by the method described later. Calculate the value obtained by dividing the collapsed edge ratio of the clearance 20% by the collapsed edge ratio of the clearance 10%. When this value is less than 1.70, the hot-rolled steel plate with a stable collapsed edge ratio in the sheared end surface after shearing, that is, excellent shearing workability, is judged to be qualified. On the other hand, when the above value exceeds 1.70, it is judged to be unqualified as a hot-rolled steel plate with poor shearing workability.
[0202] Furthermore, the edge collapse ratio in the end face is Figure 1 As shown in (a), the ratio of the collapsed edge length d1 to the sum of the collapsed edge length d1, shear surface length d2, fracture surface length d3 and burr length d4 in the straight line 1 can be calculated by drawing a straight line 1 at right angles to the upper and lower surfaces of the hot-rolled steel plate in the end surface observation photograph (= d1 / (d1+d2+d3+d4)×100).
[0203] (3) Resistance to bending cracks
[0204] The bending internal crack resistance was evaluated by the following bending test.
[0205] A rectangular test piece of 100 mm × 30 mm was cut out from the hot-rolled steel plate to obtain a bending test piece. The bending in which the bending ridgeline is parallel to the rolling direction (L direction) (L-axis bending) and the bending in which the bending ridgeline is parallel to the direction perpendicular to the rolling direction (C direction) (C-axis bending) were investigated for bending internal crack resistance according to JIS Z2248:2014 (V-block 90° bending test). The minimum bending radius without cracking was obtained, and the average value of the minimum bending radius of the L axis and the C axis was divided by the plate thickness. The obtained value was used as the limit bending R / t as an index value of bending internal crack resistance. When R / t is 2.5 or less, it is judged to be a hot-rolled steel plate with excellent bending internal crack resistance.
[0206] However, regarding the presence or absence of cracks, the test piece after the V-block 90° bending test was cut with a surface parallel to the bending direction and perpendicular to the plate surface, and the obtained cut surface was mirror-polished and then observed for cracks using an optical microscope. When the length of the crack observed on the inner side of the bend of the test piece exceeded 30 μm, it was judged that cracks were present.
[0207] The obtained results are shown in Table 4A and Table 4B.
[0208]
[0209]
[0210]
[0211]
[0212]
[0213]
[0214] From Table 4A and Table 4B, it is known that the hot rolled steel sheets according to the examples of the present invention have excellent strength and shear workability. In addition, it is known that the hot rolled steel sheets according to the examples of the present invention with ds / dq of 0.95 or less have the above-mentioned properties and excellent bending internal crack resistance.
[0215] On the other hand, it was found that the hot-rolled steel sheets according to the comparative examples did not have any one or more of excellent strength and shear workability.
[0216] Industrial Applicability
[0217] According to the above embodiment of the present invention, a hot rolled steel sheet having excellent strength and shear workability can be provided. In addition, according to the above preferred embodiment of the present invention, a hot rolled steel sheet having the above characteristics and excellent bending internal crack resistance can be obtained while suppressing the occurrence of bending internal cracks.
[0218] The hot-rolled steel sheet of the present invention is suitable as an industrial raw material for automobile components, mechanical structural parts and building components.
Claims
1. A hot rolled steel plate, characterized in that: The chemical composition contains by mass %: C:0.050~0.250%、 Si: 0.05-3.00%, Mn: 1.00~4.00%, One or more of Ti, Nb and V: 0.060 to 0.500% in total, Sol.Al: 0.001~2.000%, P: 0.100% or less, S: 0.0300% or less, N: 0.1000% or less, O: 0.0100% or less, Cu: 0-2.00%, Cr:0~2.00%、 Mo: 0-1.00%, Ni: 0-2.00%, B:0~0.0100%、 Ca: 0~0.0200%, Mg: 0~0.0200%, REM: 0~0.1000%、 Bi: 0~0.020%, One or more of Zr, Co, Zn and W: 0 to 1.00% in total, and Sn: 0~0.05%, The remainder is Fe and impurities; The metal structure is expressed in area % as follows: Retained austenite is less than 3.0%, ferrite is less than 15.0%, and pearlite is less than 5.0%; The E value indicating the periodicity of the metal structure is lower than 10.7, and the I value indicating the uniformity of the metal structure is lower than 1.020; The standard deviation of the Mn concentration is 0.60 mass % or less; Tensile strength is above 780MPa; In the measurement of the E value and the I value, the photographing area of the SEM image taken to calculate the E value and the I value is set to a depth position of 1 / 4 of the plate thickness from the surface of the steel plate in the plate thickness section parallel to the rolling direction. In measuring the standard deviation of Mn concentration, after mirror-polishing the L-section parallel to the rolling direction of the hot-rolled steel sheet, the standard deviation of Mn concentration was measured by EPMA at a depth of 1 / 4 of the sheet thickness from the surface.
2. The hot rolled steel sheet according to claim 1, characterized in that: The ratio of the average grain size ds of the surface layer to the average grain size dq at a depth of 1 / 4 of the plate thickness from the surface, that is, ds / dq, is 0.95 or less.
3. The hot rolled steel sheet according to claim 1 or 2, characterized in that: The chemical composition, in mass%, contains one or more elements selected from the following: Cu: 0.01-2.00%, Cr:0.01~2.00%、 Mo: 0.01~1.00%, Ni: 0.02-2.00%, B:0.0001~0.0100%、 Ca: 0.0005~0.0200%, Mg: 0.0005~0.0200%, REM: 0.0005~0.1000%, and Bi: 0.0005~0.020%.
Citation Information
Patent Citations
Cold rolled steel sheet excellent in blanking property and its production
JP1998168544A
High strength hot rolled steel sheet having excellent stamping workability and its production method
JP2005298924A
Hot-rolled steel sheet
CN110506133A
Hot rolled sheet steel
JP2012251201A
Hot rolled steel sheet
JP2015124410A