A mini LED chip contact electrode and preparation method thereof
By using an ohmic contact layer and an etching-through prevention layer with gradually increasing plating rates in the mini LED chip contact electrodes, the problem of increased stress in traditional contact electrodes is solved, cost savings and quality assurance are achieved, and production efficiency is improved.
Patent Information
- Application Number
- CN202310165600.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-24
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-02-24
AI Technical Summary
After the reflective layer, protective layer and conductive layer are removed from the traditional mini LED chip contact electrode, the stress increases dramatically, affecting the chip quality and making it difficult to save production costs.
The mini LED chip contact electrode is composed of an ohmic contact layer and an engraving prevention layer that gradually increases the plating rate. The Pt layer and Ti layer are formed through evaporation to avoid temperature rise and stress increase in the reaction chamber, ensuring chip quality, and Reduce production cycle time.
Without affecting the performance of the mini LED chip, it saves 5 to 10% of production costs, avoids photoresist cracking and edge warping, and improves production capacity and production efficiency.
Smart Images

Figure CN116130576B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to a mini LED chip contact electrode and a preparation method thereof. Background Art
[0002] Traditional flip-chip LED chips are used in lighting and backlight display, etc., with an application current between 120-800mA and a current density between 20-240A / cm 2 The contact electrode includes an ohmic contact layer, a reflective layer, a protective layer, a conductive layer and an anti-etching layer from bottom to top. The ohmic contact layer is used to form an ohmic contact with the underlying material to ensure the flow of electrons; the reflective layer is used to reflect a small part of the light emitted by the light-emitting layer under a large current, increase the brightness of the LED chip, and improve the external quantum efficiency of the LED chip; the protective layer is used to prevent the migration of the metal in the reflective layer from causing chip failure; the conductive layer is used to ensure the lateral expansion capability of the current of the LED chip under large current or large size, reduce the voltage of the LED chip, and reduce power consumption; the anti-etching layer is used to prevent the etching gas from damaging the contact electrode when preparing the Bragg reflective layer through-hole using the plasma gas etching process.
[0003] The flip-chip mini LED chip technology is applied to direct display of small pitch display screens. Mini LED chips are directly used as display pixels. A 1 square meter display screen uses millions of them, and even tens of millions of mini LED chips are used. Therefore, the working current of each mini LED chip is very small, between 0.1-5mA, and the current density is between 0.1-15A / cm 2 The area of miniLED chip is between 500-20000um. 2 Under low operating current, the reflective layer of the traditional flip-chip LED chip contact electrode has little effect on improving the external quantum efficiency, and the conductive layer has little effect on reducing the voltage. Therefore, the traditional LED chip contact electrode will produce excess performance for the mini LED chip.
[0004] In order to save production costs, the contact electrodes of the mini LED chip can be simplified into an ohmic contact layer and an anti-etching layer. However, if the reflective layer, protective layer and conductive layer in the contact electrodes of the traditional LED chip are directly removed, the stress of the contact electrode will increase sharply, causing photoresist cracking, contact electrode warping and other abnormalities, ultimately causing chip failure. Summary of the invention
[0005] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a mini LED chip contact electrode and a preparation method, aiming to solve the technical problem that in the prior art, in order to save the production cost of the mini LED chip, the reflective layer, protective layer and conductive layer in the contact electrode are directly eliminated, resulting in a sharp increase in the stress of the contact electrode and affecting the quality of the chip.
[0006] In order to achieve the above-mentioned objectives, on the one hand, an embodiment of the present invention provides a mini LED chip contact electrode: including an ohmic contact layer and an anti-etching layer arranged on the top of the ohmic contact layer, the anti-etching layer is used to block the etching gas, and the anti-etching layer includes a first layer, a second layer and a third layer formed by evaporation from bottom to top, and the plating rates of the first layer, the second layer and the third layer are gradually increased.
[0007] Compared with the prior art, the beneficial effects of the present invention are as follows: since the working current of the mini LED chip is relatively small, the reflective layer, protective layer and conductive layer in the traditional process are removed, especially for the conductive layer composed of Au or Cu, which can save production costs without affecting the performance of the mini LED chip. When setting the anti-etching layer, different plating rates are used for evaporation, and the first layer is evaporated at a low plating rate near the ohmic contact layer, which can prevent the cavity temperature in the reaction chamber from rising too fast, thereby increasing the metal stress and causing the photoresist to crack. At the same time, the warping caused by stress can be avoided, and the quality of the mini LED chip is guaranteed. As the second layer and the third layer gradually move away from the photoresist, the evaporation plating rate gradually increases, which can save the evaporation time, reduce the production cycle without affecting the stress, and improve the production capacity.
[0008] Furthermore, the first layer is a first Pt layer formed by evaporating Pt, the second layer is a second Pt layer formed by evaporating Pt, and the third layer is a third Pt layer formed by evaporating Pt.
[0009] Furthermore, the thickness of the first Pt layer is 300 angstroms to 500 angstroms, the thickness of the second Pt layer is 500 angstroms to 800 angstroms, and the thickness of the third Pt layer is 1000 angstroms to 2000 angstroms.
[0010] Furthermore, the first layer includes a fourth Pt layer formed by vapor-deposited Pt and a first insertion layer formed by vapor-deposited Ti, the second layer includes a fifth Pt layer formed by vapor-deposited Pt and a second insertion layer formed by vapor-deposited Ti, the third layer is a sixth Pt layer formed by vapor-deposited Pt, the first insertion layer is located between the fourth Pt layer and the fifth Pt layer, and the second insertion layer is located between the fifth Pt layer and the sixth Pt layer.
[0011] Furthermore, the thickness of the first insertion layer is 100 angstroms to 200 angstroms, and the thickness of the second insertion layer is 300 angstroms to 800 angstroms.
[0012] Furthermore, the ohmic contact layer is formed by vapor deposition of any one of Cr and Ni. When the ohmic contact layer is formed by vapor deposition of Cr, the thickness of the ohmic contact layer is 30 to 200 angstroms. When the ohmic contact layer is formed by vapor deposition of Ni, the thickness of the ohmic contact layer is 5 to 50 angstroms.
[0013] On the other hand, an embodiment of the present invention provides a method for preparing a mini LED chip contact electrode, which is used to prepare the above-mentioned mini LED chip contact electrode. The method for preparing the mini LED chip contact electrode comprises the following steps:
[0014] Providing a substrate required for growth, and performing photolithography on the substrate;
[0015] forming the ohmic contact layer on the substrate;
[0016] On the ohmic contact layer, a first layer, a second layer and a third layer are respectively evaporated from bottom to top at a gradually increasing plating rate to form the etching prevention layer, wherein the etching prevention layer is used to block the etching gas;
[0017] Remove scrap metal and photoresist.
[0018] Furthermore, the step of evaporating the first layer, the second layer and the third layer from bottom to top on the ohmic contact layer at a gradually increasing plating rate to form the anti-etching layer specifically includes:
[0019] Vapor-depositing Pt on the ohmic contact layer at a first deposition rate to form the first Pt layer, wherein the first Pt layer is a first layer;
[0020] vapor depositing Pt on the first Pt layer at a second deposition rate to form the second Pt layer, wherein the second Pt layer is the second layer;
[0021] Pt is evaporated on the second Pt layer at a third plating rate to form the third Pt layer, the third Pt layer is the third layer, the first layer, the second layer and the third layer constitute the anti-etching layer, the third plating rate is greater than the second plating rate, and the second plating rate is greater than the first plating rate.
[0022] Further, the first plating rate is 0.3 angstroms / second to 0.8 angstroms / second, the second plating rate is 1 angstroms / second to 1.5 angstroms / second, and the third plating rate is 3 angstroms / second to 5 angstroms / second.
[0023] Furthermore, the step of evaporating the first layer, the second layer and the third layer from bottom to top on the ohmic contact layer at a gradually increasing plating rate to form the anti-etching layer specifically includes:
[0024] Vapor-depositing Pt on the ohmic contact layer at a fourth deposition rate to form the fourth Pt layer;
[0025] vapor depositing Ti on the fourth Pt layer at the fourth deposition rate to form the first insertion layer, wherein the fourth Pt layer and the first insertion layer constitute the first layer;
[0026] vapor-depositing Pt on the first insertion layer at a fifth deposition rate to form the fifth Pt layer;
[0027] vapor depositing Ti on the fifth Pt layer at the fifth deposition rate to form the second insertion layer, wherein the fifth Pt layer and the second insertion layer constitute the second layer;
[0028] Pt is evaporated on the second insertion layer at a sixth plating rate to form the sixth Pt layer, the sixth Pt layer is the third layer, the first layer, the second layer and the third layer constitute the anti-etching layer, the sixth plating rate is greater than the fifth plating rate, and the fifth plating rate is greater than the fourth plating rate.
[0029] Details of one or more embodiments of the present application are set forth in the following drawings and description to make other features, objects, and advantages of the present application more readily apparent. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a schematic diagram of the structure of the mini LED chip contact electrode in the first embodiment of the present invention;
[0031] Figure 2 This is a schematic diagram of the structure of the mini LED chip contact electrode in the second embodiment of the present invention;
[0032] Figure 3 This is a flow chart of a method for preparing a mini LED chip contact electrode in a third embodiment of the present invention;
[0033] Figure 4 Flow chart of the method for preparing the contact electrode of the mini LED chip in the fourth embodiment of the present invention; Description of the main component symbols:
[0034] Ohmic contact layer 10 Preventing the layer from being cut through 20 First Pt layer 210 Second Pt layer 220 The third Pt layer 230 Fourth Pt layer 240 First insertion layer 250 Fifth Pt layer 260 Second insertion layer 270 Sixth Pt layer 280
[0035] The following specific implementation manner will further illustrate the present invention in conjunction with the above-mentioned drawings. DETAILED DESCRIPTION
[0036] In order to facilitate the understanding of the present invention, the present invention will be described more fully below with reference to the relevant drawings. Several embodiments of the present invention are given in the drawings. However, the present invention can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present invention more thorough and comprehensive.
[0037] It should be noted that when an element is referred to as being "fixed to" another element, it may be directly on the other element or there may be a central element. When an element is considered to be "connected to" another element, it may be directly connected to the other element or there may be a central element at the same time. The terms "vertical", "horizontal", "left", "right" and similar expressions used herein are for illustrative purposes only.
[0038] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0039] See also Figure 1 The mini LED chip contact electrode in the first embodiment of the present invention includes an ohmic contact layer 10 and an anti-etching layer 20 arranged on the top of the ohmic contact layer 10. Compared with the existing mini LED chip contact electrode, the mini LED chip contact electrode in this embodiment cancels the setting of the reflective layer, the protective layer and the conductive layer. Since the mini LED chip is generally directly used as a display pixel, a large number of mini LED chips are used in a 1 square meter display screen, so the working current of each mini LED chip is very small, between 0.1-5mA, and the current density is between 0.1-15A / cm 2 The reflective layer, which is used to reflect a small part of the light emitted by the light-emitting layer under high current, increase the brightness of the LED chip, and improve the external quantum efficiency of the LED chip, has a very weak improvement effect in the mini LED chip. The conductive layer, which is used to ensure the lateral expansion capability of the current of the LED chip under high current or large-size applications, reduce the voltage of the LED chip, and reduce power consumption, also has a very weak effect on reducing the voltage. It can be understood that without the need to set up a reflective layer, there is also no need to set up a protective layer for preventing the migration of the metal in the reflective layer. By removing the reflective layer, protective layer and conductive layer, especially for the conductive layer composed of Au or Ag, 5-10% of the production cost can be saved without affecting the performance of the mini LED chip.
[0040] When a semiconductor contacts a metal, a barrier layer is usually formed. However, when the semiconductor doping concentration is very high, electrons can pass through the barrier by tunneling, thereby forming an ohmic contact with low resistance. Ohmic contact is very important for semiconductor devices. Forming a good ohmic contact is conducive to the input and output of current. In this embodiment, the ohmic contact layer 10 is used to form an ohmic contact with the semiconductor to ensure the flow of electrons, thereby realizing the light-emitting function of the mini LED chip. The ohmic contact layer 10 is formed by evaporation of any material of Cr or Ni. When the ohmic contact layer 10 is formed by evaporation of Cr, the thickness of the ohmic contact layer 10 is 30 to 200 angstroms. When the ohmic contact layer is formed by evaporation of Ni, the thickness of the ohmic contact layer 10 is 5 to 50 angstroms.
[0041] The anti-etching layer 20 is used to block the etching gas. The anti-etching layer 20 includes a first layer, a second layer and a third layer formed by evaporation from bottom to top. The first layer is a first Pt layer 210 formed by evaporation of Pt, the second layer is a second Pt layer 220 formed by evaporation of Pt, and the third layer is a third Pt layer 230 formed by evaporation of Pt. Preferably, in order to adapt to the overall thickness of the mini LED, the thickness of the first Pt layer 210 is 300 angstroms to 500 angstroms, the thickness of the second Pt layer 220 is 500 angstroms to 800 angstroms, and the thickness of the third Pt layer 230 is 1000 angstroms to 2000 angstroms. Generally, the insulating protective layer of the flip-chip mini LED chip will be arranged on the top layer of the contact electrode, and an insulating protective layer through hole will be arranged on the top layer of the contact electrode, so that an electrical connection is formed between the pad and the contact electrode, and by evaporating the etching-resistant metal Pt, the etching gas damage to the contact electrode can be avoided when the Bragg reflection layer through hole is prepared by the plasma gas etching process.
[0042] The plating rates of the first layer, the second layer and the third layer are gradually increased. When the penetration prevention layer 20 is set, Pt is deposited at different plating rates. The first Pt layer 210 is deposited at a low plating rate near the ohmic contact layer 10, which can prevent the cavity temperature in the reaction chamber from rising too fast, thereby increasing the metal stress and causing the photoresist to crack. At the same time, it can avoid the warping caused by stress, thereby ensuring the quality of the mini LED chip. As the second Pt layer 220 and the third Pt layer 230 gradually move away from the photoresist, the plating rate of evaporation gradually increases, which can save the time of evaporation, reduce the production cycle without affecting the stress, and improve the production capacity. It can be understood that evaporating more layers with more different plating rates can more effectively reduce the stress caused by evaporation. In order to ensure the production speed and speed up the production time, the first layer, the second layer and the third layer are evaporated in this embodiment.
[0043] See also Figure 2The mini LED chip in the second embodiment of the present invention is different from the mini LED chip in the first embodiment in that the first layer includes a fourth Pt layer 240 formed by evaporating Pt and a first insertion layer 250 formed by evaporating Ti, the second layer includes a fifth Pt layer 260 formed by evaporating Pt and a second insertion layer 270 formed by evaporating Ti, the third layer is a sixth Pt layer 280 formed by evaporating Pt, the first insertion layer 250 is located between the fourth Pt layer 240 and the fifth Pt layer 260, and the second insertion layer 270 is located between the fifth Pt layer 260 and the sixth Pt layer 280. Preferably, the thickness of the first insertion layer 250 is 100 angstroms to 200 angstroms, and the thickness of the second insertion layer 270 is 300 angstroms to 800 angstroms. The first insertion layer 250 and the second insertion layer 270 are both formed by vapor-deposited Ti. The stress of Ti metal is compressive stress when it is less than 2000 angstroms. After completing the small-rate vapor deposition of the fourth Pt layer 240, the first insertion layer 250 formed by vapor-deposited Ti can further reduce the structural stress, and avoid increasing the plating rate directly on the fourth Pt layer 240 to directly evaporate the fifth Pt layer 260, which may still affect the stress due to the increase in temperature, thereby causing the photoresist to crack. It can be understood that the second insertion layer 270 formed by vapor-deposited Ti can also reduce the structural stress, and avoid increasing the plating rate directly on the fifth Pt layer 260 to directly evaporate the sixth Pt layer 280, which may still affect the stress due to the increase in temperature, thereby causing the photoresist to crack. It can be understood that by further evaporating Pt on the sixth Pt layer 280 to form more Pt layers, and evaporating Ti between adjacent Pt layers to form more insertion layers, the stress can be better reduced.
[0044] Preferably, because the thickness of the fourth Pt layer 240 is relatively thin when the first insertion layer 250 is evaporated, the temperature change has a higher impact on the photoresist when the first insertion layer 250 is evaporated. Therefore, the plating rate of the first insertion layer 250 is the same as the plating rate of the fourth Pt layer 240. Without adjusting the plating rate to affect the production efficiency, the first insertion layer 250 is evaporated at the same plating rate, which can achieve a better stress reduction effect. Similarly, when the second insertion layer 270 is evaporated, the plating rate of the second insertion layer 270 is the same as the plating rate of the fifth Pt layer 260. It can be understood that in order to improve the stress reduction effect, more Pt layers and insertion layers can be evaporated at more plating rates, which will not be described in detail in this embodiment.
[0045] See also Figure 3The third embodiment of the present invention provides a method for preparing a mini LED chip contact electrode, which is used to prepare the mini LED chip contact electrode described in the first embodiment. The method for preparing the mini LED chip contact electrode comprises the following steps:
[0046] S10: providing a substrate required for growth, and performing photolithography on the substrate;
[0047] Specifically, after providing a substrate required for growth, a photoresist is coated on the substrate by spin coating. The photoresist is a negative photoresist, which is used to cross-link with the exposure area. It is insoluble in a developer and has the advantages of good adhesion, good blocking effect, and fast photosensitivity. After the photoresist is coated, the substrate is placed on a hot plate and baked using the hot plate. Preferably, the thickness of the photoresist is 4um to 8um, the baking temperature of the hot plate is between 100°C and 130°C, and the baking time of the hot plate is 100S to 200S.
[0048] After baking is completed, the photoresist is exposed through a mask and a photolithography machine. After exposure is completed, pre-development baking, development and post-development baking processes are required to complete all the steps of photolithography. Preferably, the pre-development baking temperature is 110°C to 115°C, the pre-development baking time is 60S to 90S, the post-development baking temperature is 100°C to 130°C, and the post-development baking time is 100S to 200S.
[0049] S20: forming the ohmic contact layer on the substrate;
[0050] Specifically, the ohmic contact layer of the mini LED chip contact electrode is evaporated at room temperature using an electron beam evaporation process. The ohmic contact layer is formed by evaporating Cr or Ni. Metal Cr is metal chromium, which is a silvery white and shiny metal with ductility, corrosion resistance and other characteristics. In the air, even in a red-hot state, it oxidizes very slowly and is insoluble in water. Metal Ni is metal nickel, which is a silvery white metal with magnetism and good plasticity, good corrosion resistance, hardness and ductility, and it can be highly polished and corrosion-resistant. The plating rate of the ohmic contact layer is 0.1A / S-0.2A / S.
[0051] S30: evaporating a first layer, a second layer and a third layer from bottom to top on the ohmic contact layer at a gradually increasing plating rate to form the etching prevention layer, wherein the etching prevention layer is used to block the etching gas;
[0052] Because the working current of the mini LED chip is relatively small, the reflective layer, protective layer and conductive layer in the traditional process are removed, especially for the conductive layer composed of Au or Cu, which can save production costs without affecting the performance of the mini LED chip. Multiple evaporation is performed at a gradually increasing plating rate. The first layer is evaporated at a low plating rate near the ohmic contact layer to avoid the cavity temperature in the reaction chamber from rising too fast, which in turn leads to increased metal stress and cracking of the photoresist. At the same time, it can avoid warping caused by stress, thereby ensuring the quality of the mini LED chip. As the second layer and the third layer gradually move away from the photoresist, the evaporation plating rate gradually increases, which can save evaporation time, reduce the production cycle without affecting stress, and improve production capacity.
[0053] Specifically, the step of evaporating a first layer, a second layer and a third layer from bottom to top on the ohmic contact layer at a gradually increasing plating rate to form the cut-through prevention layer includes:
[0054] S310: evaporating Pt on the ohmic contact layer at a first deposition rate to form the first Pt layer, wherein the first Pt layer is a first layer;
[0055] S320: vapor-depositing Pt on the first Pt layer at a second deposition rate to form the second Pt layer, wherein the second Pt layer is a second layer;
[0056] S330: Vapor-deposit Pt on the second Pt layer at a third plating rate to form the third Pt layer, wherein the third Pt layer is the third layer, and the first layer, the second layer and the third layer constitute the anti-penetration layer, and the third plating rate is greater than the second plating rate, and the second plating rate is greater than the first plating rate.
[0057] It is understandable that the stacked contact layer includes the first layer, the second layer and the third layer. Preferably, the first plating rate is 0.3 angstroms / second, the second plating rate is 1 angstroms / second, and the third plating rate is 3 angstroms / second. The principle of the electron beam evaporation process is, in simple terms, to perform evaporation through an electron gun in the operating space to convert kinetic energy into heat energy. The smaller the plating rate, the smaller the heat energy converted from kinetic energy, and the smaller the stress caused. As the plating rate increases, the evaporation speed will increase accordingly. It is understandable that by adjusting the plating rate, more sub-layers can be evaporated to achieve better stress reduction.
[0058] Furthermore, the method for preparing the contact electrode of the mini LED chip further includes step S40: removing waste metal and photoresist;
[0059] Preferably, the scrap metal and photoresist are removed using a lift-off process.
[0060] See also Figure 4 The method for preparing the mini LED chip contact electrode in the fourth embodiment of the present invention is used to prepare the mini LED chip contact electrode in the second embodiment. The difference between the method for preparing the mini LED chip contact electrode in the third embodiment is that the step S30: evaporating the first layer, the second layer and the third layer from bottom to top on the ohmic contact layer at a gradually increasing plating rate to form the anti-etching layer specifically includes the following steps:
[0061] S301: evaporating Pt on the ohmic contact layer at a fourth deposition rate to form the fourth Pt layer;
[0062] S302: vapor-depositing Ti on the fourth Pt layer at the fourth deposition rate to form the first insertion layer, wherein the fourth Pt layer and the first insertion layer constitute the first layer;
[0063] S303: evaporating Pt on the first insertion layer at a fifth deposition rate to form the fifth Pt layer;
[0064] S304: vapor-depositing Ti on the fifth Pt layer at the fifth deposition rate to form the second insertion layer, wherein the fifth Pt layer and the second insertion layer constitute the second layer;
[0065] S305: evaporating Pt on the second insertion layer at a sixth deposition rate to form the sixth Pt layer, the sixth Pt layer being the third layer, the first layer, the second layer and the third layer constituting the cut-through prevention layer, the sixth deposition rate being greater than the fifth deposition rate, and the fifth deposition rate being greater than the fourth deposition rate;
[0066] In this embodiment, the fourth plating rate is 0.3 Å / s, the fifth plating rate is 1 Å / s, and the sixth plating rate is 3 Å / s. An insertion layer is set between adjacent Pt layers. The compressive stress characteristic of Ti metal when it is less than 2000A can be utilized. The insertion layer is evaporated at the same plating rate as the previous Pt layer. This can better suppress the growth of stress when the plating rate is subsequently increased to speed up the production cycle, thereby ensuring the quality of the mini LED chip.
[0067] The fifth embodiment of the present invention also provides a method for preparing a mini LED chip contact electrode. The method for preparing a mini LED chip contact electrode in this embodiment is different from the method for preparing a mini LED chip contact electrode in the third embodiment in that:
[0068] The first plating rate is 0.8 angstroms / second, the second plating rate is 1.5 angstroms / second, and the third plating rate is 5 angstroms / second.
[0069] The sixth embodiment of the present invention also provides a method for preparing a mini LED chip contact electrode. The method for preparing a mini LED chip contact electrode in this embodiment is different from the method for preparing a mini LED chip contact electrode in the fourth embodiment in that:
[0070] The fourth plating rate is 0.8 angstroms / second, the fifth plating rate is 1.5 angstroms / second, and the sixth plating rate is 5 angstroms / second.
[0071] Comparative Example 1
[0072] A method for preparing a mini LED chip contact electrode. The method for preparing a mini LED chip contact electrode in this embodiment is different from the method for preparing a mini LED chip contact electrode in the third embodiment in that the steps after step S20 are specifically as follows:
[0073] Vapor depositing a reflective layer on the ohmic contact layer;
[0074] Vapor depositing a protective layer on the reflective layer;
[0075] Vapor depositing a conductive layer on the protective layer;
[0076] Pt is evaporated on the conductive layer to form an etching prevention layer.
[0077] Comparative Example 2
[0078] A method for preparing a mini LED chip contact electrode. The method for preparing a mini LED chip contact electrode in this embodiment is different from the method for preparing a mini LED chip contact electrode in the third embodiment in that: step S30 is: evaporating Pt on the ohmic contact layer to form an anti-etching layer.
[0079] The mini LED chip contact electrodes prepared in the above-mentioned Examples 3 to 6 and Comparative Examples 1 to 2 were prepared into mini LED chips for testing, and the corresponding preparation parameters and test results are shown in the following table:
[0080]
[0081] In actual application, the contact electrodes and chips made by the preparation methods of the miniLED chip contact electrodes of the above-mentioned embodiments 3 to 6 of the present invention and the corresponding comparative examples 1 to 2 are tested, and the test data are shown in the above table. It should be noted that in order to ensure the reliability of the verification results, when the contact electrodes and chips of the above-mentioned embodiments 3 to 6 and comparative examples 1 to 2 of the present invention are prepared, except for the above-mentioned parameters, other processes and parameters should be kept consistent.
[0082] It can be concluded from the above table that by eliminating the reflective layer, protective layer and conductive layer, the performance of the contact electrode and the miniLED chip is not affected, and the production cost can be effectively saved. When setting the anti-etching layer, different plating rates are used for evaporation, and the first layer is evaporated at a low plating rate near the ohmic contact layer. This can prevent the cavity temperature in the reaction chamber from rising too quickly, thereby increasing the metal stress and causing the photoresist to crack. At the same time, it can avoid the warping caused by stress, thereby ensuring the quality of the mini LED chip. As the second layer and the third layer gradually move away from the photoresist, the evaporation rate gradually increases, which can save the evaporation time, reduce the production cycle without affecting the stress, and improve the production capacity.
[0083] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.
[0084] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A mini LED chip contact electrode, characterized in that: It includes an ohmic contact layer and a penetration-preventing layer directly arranged on the top of the ohmic contact layer, the penetration-preventing layer is used to block the etching gas, the penetration-preventing layer includes a first layer, a second layer and a third layer formed by evaporation from bottom to top, the plating rates of the first layer, the second layer and the third layer are gradually increased, the first layer includes a fourth Pt layer formed by evaporation of Pt and a first insertion layer formed by evaporation of Ti, the second layer includes a fifth Pt layer formed by evaporation of Pt and a second insertion layer formed by evaporation of Ti, the third layer is a sixth Pt layer formed by evaporation of Pt, the first insertion layer is located between the fourth Pt layer and the fifth Pt layer, and the second insertion layer is located between the fifth Pt layer and the sixth Pt layer.
2. The mini LED chip contact electrode according to claim 1, characterized in that: The thickness of the first insertion layer is 100 angstroms to 200 angstroms, and the thickness of the second insertion layer is 300 angstroms to 800 angstroms.
3. The mini LED chip contact electrode according to claim 1, characterized in that: The ohmic contact layer is formed by vapor deposition of any one of Cr and Ni. When the ohmic contact layer is formed by vapor deposition of Cr, the thickness of the ohmic contact layer is 30 to 200 angstroms. When the ohmic contact layer is formed by vapor deposition of Ni, the thickness of the ohmic contact layer is 5 to 50 angstroms.
4. A method for preparing a mini LED chip contact electrode, used for preparing the mini LED chip contact electrode as claimed in any one of claims 1 to 3, characterized in that: The method for preparing the mini LED chip contact electrode comprises the following steps: Providing a substrate required for growth, and performing photolithography on the substrate; forming the ohmic contact layer on the substrate; On the ohmic contact layer, a first layer, a second layer and a third layer are respectively evaporated from bottom to top at a gradually increasing plating rate to form the etching prevention layer, wherein the etching prevention layer is used to block the etching gas; The step of evaporating a first layer, a second layer and a third layer from bottom to top on the ohmic contact layer at a gradually increasing plating rate to form the cut-through prevention layer comprises: Vapor-depositing Pt on the ohmic contact layer at a fourth deposition rate to form the fourth Pt layer; vapor depositing Ti on the fourth Pt layer at the fourth deposition rate to form the first insertion layer, wherein the fourth Pt layer and the first insertion layer constitute the first layer; vapor-depositing Pt on the first insertion layer at a fifth deposition rate to form the fifth Pt layer; vapor depositing Ti on the fifth Pt layer at the fifth deposition rate to form the second insertion layer, wherein the fifth Pt layer and the second insertion layer constitute the second layer; Vapor depositing Pt on the second insertion layer at a sixth deposition rate to form the sixth Pt layer, the sixth Pt layer being the third layer, the first layer, the second layer and the third layer constituting the cut-through prevention layer, the sixth deposition rate being greater than the fifth deposition rate, and the fifth deposition rate being greater than the fourth deposition rate; Remove scrap metal and photoresist.