Novel fluorinated diamine monomer and preparation method thereof and application thereof in preparation of polyimide

Through the reaction of a new type of fluorine-containing diamine monomer with alicyclic dianhydride and 9-anthracenemethanol, a highly heat-resistant, transparent, and moisture-resistant anthracene-containing photosensitive polyimide is formed, which solves the problem of photosensitive polyimide in the existing technology. The stability and process efficiency of amine materials are issues, and they are suitable for high-precision components and flexible electronics.

CN116143640BActive Publication Date: 2024-10-18WANHUA CHEM GRP CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310012567.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-01-05
Publication Date
2024-10-18
Estimated Expiration
2043-01-05

AI Technical Summary

Technical Problem

The existing technology cannot effectively obtain highly photosensitive polyimide materials with high transparency, thermal stability, dimensional stability and moisture resistance, and the traditional process is cumbersome and inefficient. High-temperature imidization treatment limits its application in heat-sensitive elements. device applications.

Method used

A new type of fluorine-containing diamine monomer is reacted with alicyclic dianhydride and 9-anthracenemethanol under specific conditions, and a photosensitive group is introduced through esterification to form anthracene-containing photosensitive polyimide with polyfluorine substitution and dicarboxyl structure. Improve its heat resistance and stability.

Benefits of technology

The obtained polyimide material has high heat resistance, transparency, moisture resistance and dimensional stability, and is suitable for high-precision components and flexible electronics, simplifying the process and improving efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116143640B_ABST
    Figure CN116143640B_ABST
Patent Text Reader

Abstract

The present invention discloses a novel fluorine-containing diamine monomer, a preparation method thereof and an application thereof in preparing polyimide. The fluorine-containing diamine monomer has the following structural expression. The fluorine-containing diamine monomer can be used to prepare anthracene-containing photosensitive polyimide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a fluorine-containing diamine and a polyimide, and in particular to a novel fluorine-containing diamine monomer and a preparation method thereof and application thereof in the preparation of polyimide. Background Art

[0002] Polyimide (PI) refers to a class of polymers containing imide rings on the main chain. As a cutting-edge material with outstanding performance, it has been widely used for its excellent electrical insulation, wear resistance, high temperature radiation resistance and physical and mechanical properties. When traditional non-photosensitive polyimide is used as a passivation coating or interlayer insulating medium for integrated circuits or various electronic and microelectronic devices, a layer of photoresist must be applied on the film, and then exposed to obtain a photolithography pattern. The photoresist pattern is used as a masking layer, and the lower layer of polyimide is corroded by an etchant, and then the photoresist layer is removed to obtain the polyimide pattern. This process is cumbersome, has many wastes, and is inefficient.

[0003] The excellent thermal stability, mechanical stability and chemical stability of photosensitive polyimide as well as its good electrical insulation and photosensitivity make it a polymer functional material and process material such as radiation shielding material, sacrificial layer material, insulating dielectric material, buffer material, liquid crystal orientation material, etc. It is widely used in optical devices, optoelectronic devices, microelectronic devices and the corresponding device processing technology.

[0004] At present, the most widely used polyimide photosensitive materials are actually photosensitive polyamic acid solutions. When in use, the polyamic acid pattern is first photoetched, and then the polyimide pattern is formed by thermal imidization. Although the process is greatly simplified, the three wastes are reduced, and the efficiency is improved, the process requires high-temperature imidization treatment, which limits its application in heat-sensitive components. In addition, a large volume shrinkage will occur during the conversion of polyamic acid into polyimide, which limits its use in components with high precision requirements.

[0005] Existing technology has done a lot of work on the research of photosensitive polyimide, such as:

[0006] Patent CN1793200A obtains polyimide by copolymerizing 2,4-dihydroxy-m-phenylenediamine hydrochloride with diamine and dianhydride, introduces hydroxyl groups into the main chain structure of the molecule, and then reacts with acrylic acid and its derivatives to obtain a negative polyamide-imide photosensitive material with higher resolution, good thermal properties and solubility.

[0007] Patent CN113388107A obtains fluorinated polyimide by copolymerizing diamine and dianhydride, and introduces photosensitive groups into the ends of the molecular chains through benzene rings and carboxyl groups to achieve photosensitivity, but the effect of the end-access photosensitive groups is not good.

[0008] It can be seen that there is still no effective and feasible method in the prior art to obtain highly photosensitive polyimide with high transparency, thermal stability, dimensional stability and moisture resistance. Summary of the invention

[0009] In order to solve the above technical problems, the present invention provides a novel fluorine-containing diamine monomer, a preparation method and an application thereof in the preparation of polyimide.

[0010] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0011] Based on the first aspect of the present invention, a novel fluorinated diamine monomer is first provided, and its structural expression is shown in Formula I:

[0012]

[0013] Based on the second aspect of the present invention, a method for preparing a novel fluorinated diamine monomer is also provided, comprising the following steps:

[0014] Under nitrogen protection, the nitrile polyfluorodiamine represented by formula II is added to an alkaline solution to react to generate a fluorine-containing diamine monomer represented by formula I;

[0015]

[0016] In a preferred embodiment, the reaction conditions are: 90-120° C. for 8-14 h.

[0017] In a preferred embodiment, the alkali solution is an aqueous solution of potassium hydroxide and / or sodium hydroxide;

[0018] Preferably, the amount of the alkali solution used is 2-4 times the mass of the nitrile polyfluorodiamine shown in formula II, calculated on the mass of potassium hydroxide and / or sodium hydroxide.

[0019] The nitrile polyfluorodiamine represented by formula II of the present invention can be synthesized by referring to the method provided in patent CN113788769B.

[0020] Preferably, after the reaction is completed, the reactants are poured into water to precipitate a large amount of solid powder, which is filtered, dried, and then recrystallized to obtain the purified fluorine-containing diamine monomer.

[0021] Based on the third aspect of the present invention, there is also provided a use of the novel fluorine-containing diamine monomer as described above or the novel fluorine-containing diamine monomer prepared by the method as described above in the preparation of polyimide.

[0022] Specifically, a method for preparing anthracene-containing photosensitive polyimide comprises the following steps:

[0023] 1) mixing and dissolving the fluorinated diamine monomer represented by formula I and the alicyclic dianhydride monomer represented by formula III in solvent A, adding isoquinoline as a catalyst, and reacting to generate a fluorinated polyimide polymer comprising a structural unit of formula IV;

[0024] 2) mixing and dissolving a fluorinated polyimide polymer containing a structural unit of formula IV and 9-anthracene methanol in a solvent B, and reacting in the presence of a condensing agent and an activating agent to generate an anthracene-containing photosensitive polyimide containing a structural unit of formula V;

[0025]

[0026]

[0027] In a preferred embodiment, in step 1), the molar ratio of the fluorinated diamine monomer represented by formula I to the alicyclic dianhydride monomer represented by formula III is 1:(1-1.2);

[0028] Preferably, in step 1), the amount of isoquinoline added is 0.8-2 times the total molar amount of the fluorinated diamine monomer represented by formula I and the alicyclic dianhydride monomer represented by formula III, in terms of molar amount.

[0029] In a preferred embodiment, in step 1), the reaction conditions are: 185-200° C. for 10-20 h.

[0030] Preferably, in step 1), solvent A is one or more of m-cresol, p-chlorophenol, N-methyl-2-pyrrolidone (NMP), and sulfolane.

[0031] Preferably, after the reaction in step 1) is completed, the reaction solution is added to an alcohol solvent to precipitate a fibrous precipitate, which is then filtered, washed and dried to obtain a purified product.

[0032] In a preferred embodiment, in step 2), the molar ratio of the fluorinated polyimide polymer comprising the structural unit of formula IV to 9-anthracene methanol is 1:(1-2);

[0033] Preferably, the amount of the activator is 0.5-1.5 times the molar amount of 9-anthracene methanol; more preferably, the activator is selected from one or more of 4-dimethylaminopyridine (DMAP), 1-hydroxybenzotriazole (HOBt), and 4-pyrrolidinylpyridine (4-PPY);

[0034] Preferably, the amount of the condensing agent is 0.5-1 times the mass of the fluorinated polyimide polymer containing the structural unit of formula IV; more preferably, the condensing agent is selected from one or more of N,N-dicyclohexylcarbodiimide (DCC), 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC), and diisopropylcarbodiimide (DIC).

[0035] In a preferred embodiment, the reaction conditions in step 2) are: reaction at room temperature for 6-24 hours.

[0036] Preferably, in step 2), solvent B may be one or more of tetrahydrofuran and dichloromethane.

[0037] Preferably, after the reaction in step 2) is completed, alcohol is added to the reaction solution and stirring is continued for 1-3 hours. Solids are precipitated after ice bathing, and the purified product is obtained after filtering, washing and drying.

[0038] In the present invention, the alcohol can be a common solvent such as methanol, ethanol, etc.

[0039] The anthracene-containing photosensitive polyimide obtained by the above preparation method has a number average molecular weight of up to 4×10 4 -2×10 5 .

[0040] The beneficial effects of the present invention are:

[0041] 1. The present invention provides a fluorinated diamine monomer with a polyfluorinated substitution, a dicarboxyl structure and a high content of benzene rings, which has multiple active functional groups and greater rigidity and can be used to prepare polyimide with excellent performance.

[0042] 2. The present invention provides an economical preparation route for a novel fluorinated diamine monomer, which has simple operation, low cost of starting raw materials, and easy purification and separation of products.

[0043] 3. The present invention also provides an anthracene-containing photosensitive polyimide prepared from the fluorine-containing diamine monomer, wherein the main chain of the polyimide contains a large number of alicyclic and benzene ring structures, and the side groups are introduced into the rigid side group structure of the photosensitive group anthracene by esterification, wherein the rigid side groups can improve the heat resistance and have a non-coplanar structure, increase the free volume in the molecular structure, and the polyphenyl ring rigid side groups increase the resistance to interchain movement to ensure the stability of the pattern after photolithography; wherein the alicyclic rings have a low molar polarizability, which will destroy the planarity of the molecular chain, inhibit charge transfer and tight stacking; the perfluorinated structure side groups provide strong hydrophobicity. In summary, the obtained photosensitive fluorinated polyimide has the characteristics of high heat resistance, transparency, high film-forming ductility, moisture resistance, dimensional stability, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 This is the hydrogen nuclear magnetic resonance spectrum of the fluorinated diamine monomer prepared in Example 1.

[0045] Figure 2 To prepare the hydrogen nuclear magnetic resonance spectrum of the alicyclic dianhydride monomer prepared in Example 1. DETAILED DESCRIPTION

[0046] The present invention is further described below by means of specific examples. The examples described in the present invention are only used to illustrate the present invention and do not limit the scope of the present invention.

[0047] Unless otherwise specified, the raw materials and reagents in the following examples of the present invention are purchased from commercial sources. The nitrile polyfluorodiamine represented by formula II of the present invention is synthesized by referring to the method provided by patent CN113788769B; (trifluoromethyl)cyclopentane, CAS: 859204-85-6, is purchased from Chongqing Futeng Pharmaceutical Co., Ltd.

[0048] [Preparation Example 1]

[0049] Preparation of alicyclic dianhydride monomers, the synthetic route is as follows:

[0050]

[0051] (1) Synthesis of Compound A3

[0052] To a 250 ml three-necked flask, add 24.0 g of a 50% aqueous solution of dimethylamine, and under ice-cold conditions, add dropwise 33.2 g of a 30% aqueous solution of hydrochloric acid. After the addition is complete, stir and react for 1 hour to obtain the hydrochloride of dimethylamine. In the three-necked flask, slowly add 9.9 g of polyformaldehyde and 15.0 g of (trifluoromethyl)cyclopentane (Al), raise the temperature to 90°C under nitrogen protection, and react for 3 hours to obtain a reaction solution of compound A3.

[0053] (2) Synthesis of Compound A4

[0054] The reaction solution of the compound A3 prepared above was cooled to 50°C, and 80 ml of methyl cellosolve, 3.8 g of a 50% by mass aqueous solution of dimethylamine, and 25.4 g of cyclopentadiene were slowly added. The mixture was heated to 120°C under nitrogen protection and reacted at this temperature for 1.5 h. The mixture was cooled to room temperature, purified by chromatography, eluted with n-hexane, and short-path distilled to obtain a colorless oily liquid, i.e., 22.8 g of compound A4.

[0055] (3) Synthesis of Compound A5

[0056] To the reaction flask, 50 ml of methanol, 10 ml of chloroform, 0.5 g of copper (II) chloride and 0.8 g of palladium chloride were added, and the mixture was stirred. The mixture was replaced with carbon monoxide three times. A mixture of 20 g of compound A4 and 50 ml of chloroform was added dropwise at a temperature of 20-25 °C. The mixture was added dropwise in about 3 hours. The reaction was continued at the same temperature for 4 hours. The mixture was replaced with nitrogen three times. The solvent was evaporated and purified by silica gel chromatography (hexane: ethyl acetate = 10:1) to obtain a white solid, namely compound A5.

[0057] (4) Synthesis of Compound A6

[0058] Compound A5 25.0 g, formic acid 20.5 g, and p-toluenesulfonic acid monohydrate 25.0 mg were added to the reaction flask, and the reaction was carried out at a temperature of 98° C. for 20 hours. After the reaction was completed, formic acid was distilled off, filtered, and the filter cake was rinsed with toluene. The obtained crude product was recrystallized with acetic anhydride and then recrystallized with N'N'-dimethylacetamide to obtain a white solid, namely compound A6, i.e., alicyclic dianhydride monomer, and its nuclear magnetic resonance hydrogen spectrum is as follows Figure 2 shown.

[0059] The following examples 1-3 are used to provide a method for preparing the fluorinated diamine monomer shown in formula I:

[0060]

[0061] [Example 1]

[0062] In a 250ml dry three-necked flask, under nitrogen protection, add 0.05mol (35.603g) of nitrile-based fluorinated diamine monomer shown in formula II and 71.206g of potassium hydroxide, react at 90°C for 14h under alkaline conditions, and pour the reactants into water after the reaction is terminated to precipitate a large amount of solid powder. The crude product is filtered and dried, and then recrystallized with a mixed solvent of N,N-dimethylformamide / methanol (volume ratio 3:1) to obtain a fluorinated diamine monomer shown in formula I (melting point 195-196°C), with a yield of 95%. The product H NMR spectrum is as follows Figure 1 shown.

[0063] [Example 2]

[0064] In a 250ml dry three-necked flask, under nitrogen protection, 0.05mol (35.603g) of the nitrile-based fluorinated diamine monomer represented by formula II and 106.809g of potassium hydroxide were added, and the reaction was carried out at 100°C under alkaline conditions for 11h. After the reaction was terminated, the reactants were poured into water to precipitate a large amount of solid powder. The crude product was filtered and dried, and then recrystallized with a mixed solvent of N,N-dimethylformamide / methanol (volume ratio 3:1) to obtain a fluorinated diamine monomer represented by formula I with a yield of 96%.

[0065] [Example 3]

[0066] In a 250ml dry three-necked flask, under nitrogen protection, 0.05mol (35.603g) of the nitrile-based fluorinated diamine monomer shown in formula II and 142.412g of sodium hydroxide were added, and the reaction was carried out at 120°C under alkaline conditions for 8h. After the reaction was terminated, the reactants were poured into water to precipitate a large amount of solid powder. The crude product was filtered and dried, and then recrystallized with a mixed solvent of N,N-dimethylformamide / methanol (volume ratio 3:1) to obtain a fluorinated diamine monomer shown in formula I with a yield of 98%.

[0067] The following examples 4-6 are used to provide a method for preparing anthracene-containing photosensitive polyimide:

[0068] [Example 4]

[0069] In a dry 50ml three-necked round-bottom flask filled with nitrogen, add 2mmol (1.4101g) of fluorinated diamine monomer represented by formula I, 2mmol (0.8763g) of alicyclic dianhydride monomer represented by formula III, and then add 8.6ml of m-cresol and 0.4128g of isoquinoline respectively. Heat the reaction system to 185°C and stir for 20h, then terminate the reaction and cool to room temperature. Pour the polymer solution into methanol to obtain fibrous polyimide polymer A1-0, filter, wash and dry.

[0070] 2mmol (2.3644g) of polyimide polymer A1-0 and 2mmol (0.4162g) of 9-anthracene methanol were placed in a round-bottom flask and dissolved in dry tetrahydrofuran. When 2mmol of 4-dimethylaminopyridine was added, 1.1822g of N,N-dicyclohexylcarbodiimide (DCC) solution was added dropwise. Stir at room temperature for 8h under nitrogen atmosphere, then ethanol was added to the reaction solution and continued to stir for 2h. The reaction solution was refrigerated at 0℃ for 2h and filtered. The filtrate was injected with methanol, filtered, and vacuum dried at 60℃ to obtain anthracene-containing photosensitive polyimide A1.

[0071] [Example 5]

[0072] In a dry 50ml three-necked round-bottom flask filled with nitrogen, add 2mmol (1.4101g) of fluorinated diamine monomer represented by formula I, 2.2mmol (0.9639g) of alicyclic dianhydride monomer represented by formula III, and then add 8.6ml of p-chlorophenol and 0.5418g of isoquinoline respectively. After heating the reaction system to 190°C and stirring for 15h, terminate the reaction and cool to room temperature. Pour the polymer solution into methanol to obtain fibrous polyimide polymer A2-0, filter, wash and dry.

[0073] 2mmol (2.3644g) of polyimide polymer A2-0 and 3mmol (0.6243g) of 9-anthracene methanol were placed in a round-bottom flask and dissolved in dry tetrahydrofuran. When 3mmol of HOBt was added, 1.1822g of EDC solution was added dropwise. Stir at room temperature for 16h under nitrogen atmosphere, then add ethanol to the reaction solution and continue stirring for 2h. The reaction solution was refrigerated at 0℃ for 2h and filtered. The filtrate was injected with methanol, filtered, and vacuum dried at 60℃ to obtain anthracene-containing photosensitive polyimide A2.

[0074] [Example 6]

[0075] In a dry 50ml three-necked round-bottom flask filled with nitrogen, add 2mmol (1.4101g) of fluorinated diamine monomer represented by formula I, 2.4mmol (1.0515g) of alicyclic dianhydride monomer represented by formula III, and then add 8.6ml of cyclobutane sulfone and 1.1352g of isoquinoline respectively. Heat the reaction system to 200℃ and stir for 10h, terminate the reaction and cool to room temperature, pour the polymer solution into methanol to obtain fibrous polyimide polymer A3-0, filter, wash and dry.

[0076] 2mmol (2.3644g) of polyimide polymer A3-0 and 4mmol (0.8324g) of 9-anthracene methanol were placed in a round-bottom flask and dissolved in dry dichloromethane. When 4mmol of 4-PPY was added, 1.1822g of DIC solution was added dropwise. Stir at room temperature for 24h under nitrogen atmosphere, then add ethanol to the reaction solution and continue stirring for 2h. The reaction solution was refrigerated at 0℃ for 2h and filtered. The filtrate was injected with methanol, filtered, and vacuum dried at 60℃ to obtain anthracene-containing photosensitive polyimide A3.

[0077] The main testing methods used in the present invention are:

[0078] 1. Glass transition temperature test (Tg, ℃):

[0079] Using a differential scanning calorimeter, 5 mg of a polyimide sample was taken and placed in a crucible cell. The temperature was raised from 30°C to 400°C at a rate of 10°C / min, and the curve changes were recorded.

[0080] 2. Water absorption measurement:

[0081] A fluorinated polyimide film sample (5 cm×5 cm×0.005 cm) was immersed in deionized water at room temperature for 24 h. The film sample was taken out, the surface moisture was wiped off and weighed, and the water absorption rate of the sample was calculated based on the weight difference before and after immersion.

[0082] 3. Coefficient of thermal expansion (CTE):

[0083] The thermal expansion coefficient of the film at 50-250° C. was measured using a thermomechanical analyzer (TMA, manufactured by TA Instrument, model Q400) at a test condition of 5° C. / min, with the temperature rising to 350° C. The temperature was raised and lowered three times, and the average value of the second and third times was calculated.

[0084] 4. Transmittance in visible light region:

[0085] The average light transmittance of the film in the wavelength range of 380-780 nm was measured using an ultraviolet spectrophotometer (manufactured by Hitachi, Ltd., model U-3900).

[0086] 5. Dielectric properties:

[0087] Based on the Agilent 4294A impedance analyzer, the polyimide film was cut into a 2cm diameter circle, and the upper and lower surfaces were coated with conductive silver paste as electrodes. The test fixture was in close contact with the sample surface. Test conditions: 25°C, voltage 500mV, frequency 1x10 2 -1x10 6 Hz.

[0088] The performance test results of polyimide are shown in Table 1.

[0089] Table 1. Performance test data of polyimide

[0090]

[0091] From the data in the table, it can be seen that by introducing high electronegativity, low polarizability fluorine atoms and rigid perfluorinated side groups, the regularity of the molecular chain is destroyed, the molecular chains are prevented from being tightly stacked and strong hydrophobicity is provided; alicyclic dianhydrides inhibit intramolecular electron conjugation and synergistically construct a photosensitive fluorinated polyimide resin with high heat resistance, transparency, high film-forming ductility, moisture resistance and dimensional stability, which can be used in high-demand flexible electronics and photoresist fields.

[0092] The above is only a preferred embodiment of the present invention. It should be pointed out that ordinary technicians in this field can make several improvements and supplements without departing from the method of the present invention. These improvements and supplements should also be regarded as the scope of protection of the present invention.

Claims

1. A novel fluorinated diamine monomer, characterized in that: The structural expression of the fluorinated diamine monomer is shown in Formula I:

2. A method for preparing the novel fluorinated diamine monomer as claimed in claim 1, characterized in that: The following steps are involved: Under nitrogen protection, the nitrile polyfluorodiamine represented by formula II is added to an alkaline solution to react to generate a fluorine-containing diamine monomer represented by formula I; 3. The method for preparing the novel fluorine-containing diamine monomer according to claim 2, characterized in that: The reaction conditions are: 90-120°C for 8-14h.

4. The method for preparing the novel fluorine-containing diamine monomer according to claim 2 or 3, characterized in that: The alkali solution is an aqueous solution of potassium hydroxide and / or sodium hydroxide.

5. The method for preparing the novel fluorine-containing diamine monomer according to claim 4, characterized in that: The amount of the alkali solution used is 2-4 times the mass of the nitrile polyfluorodiamine shown in formula II, based on the mass of potassium hydroxide and / or sodium hydroxide.

6. Use of the novel fluorine-containing diamine monomer according to claim 1 or the novel fluorine-containing diamine monomer prepared by the method according to any one of claims 2 to 5 in the preparation of polyimide.

7. A method for preparing anthracene-containing photosensitive polyimide, characterized in that: The following steps are involved: 1) mixing and dissolving the fluorinated diamine monomer represented by formula I and the alicyclic dianhydride monomer represented by formula III in solvent A, adding isoquinoline as a catalyst, and reacting to generate a fluorinated polyimide polymer comprising a structural unit of formula IV; 2) mixing and dissolving a fluorinated polyimide polymer containing a structural unit of formula IV and 9-anthracene methanol in a solvent B, and reacting in the presence of a condensing agent and an activating agent to generate an anthracene-containing photosensitive polyimide containing a structural unit of formula V; The activator is selected from one or more of 4-dimethylaminopyridine, 1-hydroxybenzotriazole, and 4-pyrrolidinopyridine; The condensing agent is selected from one or more of N,N-dicyclohexylcarbodiimide, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, and diisopropylcarbodiimide.

8. The method for preparing anthracene-containing photosensitive polyimide according to claim 7, characterized in that: In step 1), the molar ratio of the fluorine-containing diamine monomer represented by formula I to the alicyclic dianhydride monomer represented by formula III is 1:(1-1.2).

9. The method for preparing anthracene-containing photosensitive polyimide according to claim 8, characterized in that: In step 1), the amount of isoquinoline added is 0.8-2 times the total molar amount of the fluorinated diamine monomer represented by formula I and the alicyclic dianhydride monomer represented by formula III, in terms of molar amount.

10. The method for preparing anthracene-containing photosensitive polyimide according to any one of claims 7 to 9, characterized in that: In step 1), the reaction conditions are: 185-200° C. for 10-20 h.

11. The method for preparing anthracene-containing photosensitive polyimide according to claim 7, characterized in that: In step 2), the molar ratio of the fluorinated polyimide polymer comprising the structural unit of formula IV to 9-anthracene methanol is 1:(1-2).

12. The method for preparing anthracene-containing photosensitive polyimide according to claim 11, characterized in that: The amount of the activator used is 0.5-1.5 times the molar amount of 9-anthracenemethanol.

13. The method for preparing anthracene-containing photosensitive polyimide according to claim 11, characterized in that: The amount of the condensing agent used is 0.5-1 times the mass of the fluorine-containing polyimide polymer containing the structural unit of formula IV.

14. The method for preparing anthracene-containing photosensitive polyimide according to claim 7 or 11, characterized in that: The reaction conditions in step 2) are: reaction at room temperature for 6-24 hours.

Citation Information

Patent Citations

  • Photosensitive polyimide resin, polyimide photocuring coating and preparation method thereof

    CN113388107A

  • Deuterated fluorine-containing polyimide, polyimide precursor, polyimide film, preparation method and application

    CN113024807A

  • Fluorine-containing diamine monomer and preparation method thereof

    CN113788769A