A boron-based electrochromic material and its preparation method and application

CN116178410BActive Publication Date: 2024-11-15INST OF NEW MATERIALS ZHEJIANG UNIV OF TECH PINGHU CITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310144201.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-09
Publication Date
2024-11-15
Estimated Expiration
2043-02-09

AI Technical Summary

Technical Problem

Existing electrochromic materials are difficult to remain transparent without voltage, and long-term voltage application will damage the polymer structure, affect device life, and a single response speed and color display, limiting their application range.

Method used

Boron-based electrochromic material, whose monomer structure includes tripaniline derivatives and boron trifluoride ether, is prepared by electrochemical polymerization to form an electrochromic material with high optical contrast and fast response.

Benefits of technology

The color change from transparent to blue under voltage drive is achieved. The optical contrast ratio at 740nm is as high as 60%, the response times for coloring and fading are 4.8s and 1.8s respectively, and the contrast ratio has almost no attenuation after 150 cycles, which is significantly Improves the stability and application prospects of materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116178410B_ABST
    Figure CN116178410B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of electrochromic materials, and provides a boron-based electrochromic material and a preparation method and application thereof. The boron-based electrochromic material provided by the present invention is centered on boron, and a triphenylamine derivative is a peripheral polymer group. Among them, the triphenylamine derivative has a strong conjugated structure, and the formed electrochromic material can achieve a color change from transparent to blue under the drive of voltage. The optical contrast of the boron-based electrochromic material provided by the present invention is as high as 60% at 740nm, and the response time of coloring and fading is 4.8s and 1.8s respectively. In addition, after 150 cycles, the optical contrast of the boron-based electrochromic material is almost not attenuated. The boron-based electrochromic material provided by the present invention is an electrochromic material with excellent properties, and has broad application prospects in the field of display devices (such as anti-counterfeiting, color-changing glass, mobile phone back shell, electronic label, electronic paper).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrochromic materials, and in particular to a boron-based electrochromic material and a preparation method and application thereof. Background Art

[0002] Electrochromic materials are functional components in electrochromic devices. Existing electrochromic materials are generally divided into inorganic electrochromic materials and organic electrochromic materials. Inorganic electrochromic materials mainly include transition metal oxides (such as oxides of elements such as tungsten, nickel, titanium, molybdenum, iridium, vanadium, cobalt, etc.) and other inorganic materials, but their response speed is slow, the color display is single, and the coloring efficiency is low, which seriously limits their application range, especially in electrochromic display devices, which is almost difficult to achieve. Compared with inorganic electrochromic materials, organic electrochromic materials have the advantages of rich structural types, good processing performance, fast response speed and multiple color changes, and are considered to be the most promising next-generation electrochromic materials. Organic electrochromic materials are mainly divided into two categories: conjugated polymer electrochromic materials and organic small molecule electrochromic materials (viologens). Nowadays, conjugated polymer electrochromic materials have received extensive attention and research, and have become an important development direction for the new generation of electrochromic display materials.

[0003] In conjugated polymer electrochromic materials, the cathode coloring material needs to keep applying voltage to maintain a transparent state, which significantly increases energy consumption. On the other hand, long-term application of voltage will also destroy the structure of the polymer, ultimately affecting the service life of the device. For some displays, we need to present a transparent state without applying voltage, and a short-term colored state under the application of voltage. This is in line with the concept of energy saving and can achieve good confidentiality. The short-term driving voltage will not destroy the polymer structure to achieve the purpose of extending the service life. Therefore, it is of great significance to provide an energy-saving electrochromic material that can achieve the above-mentioned color change. Summary of the invention

[0004] The purpose of the present invention is to overcome the problems existing in the prior art and to provide a boron-based electrochromic material and a preparation method and application thereof.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The present invention provides a boron-based electrochromic material, wherein the structural formula of a monomer of the boron-based electrochromic material is:

[0007]

[0008] The present invention also provides a method for preparing the boron-based electrochromic material, comprising the following steps:

[0009] (1) under a protective atmosphere, diphenylamine, cuprous iodide, 2,2-bipyridine, potassium tert-butoxide, 2,5-dibromo-m-xylene and toluene are mixed and reacted to obtain a triphenylamine derivative;

[0010] (2) under a protective atmosphere, mixing a triphenylamine derivative and diethyl ether to react to obtain a mixture;

[0011] (3) mixing the mixture with tert-butyl lithium and heating to obtain a mixed solution;

[0012] (4) mixing the mixed solution with boron trifluoride etherate to react to obtain a monomer of a boron-based electrochromic material;

[0013] (5) Mixing the monomer of the boron-based electrochromic material, chloroform, acetonitrile and tetrabutylammonium hexafluorophosphate, and performing electrochemical polymerization to obtain the boron-based electrochromic material.

[0014] Preferably, in step (1), the molar ratio of diphenylamine, cuprous iodide, 2,2-bipyridine, potassium tert-butoxide and 2,5-dibromo-meta-xylene is 0.8-1.2: 0.04-0.06: 0.04-0.06: 1.8-2.2: 1.0-1.4; the mass and volume ratio of diphenylamine, cuprous iodide, 2,2-bipyridine, potassium tert-butoxide and 2,5-dibromo-meta-xylene to toluene is 1 g: 10-15 mL.

[0015] Preferably, the reaction temperature in step (1) is 115-135° C., and the reaction time is 22-26 h.

[0016] Preferably, the molar ratio of the triphenylamine derivative in step (2) to the tert-butyl lithium in step (3) and the boron trifluoride ether in step (4) is 0.8-1.2:1.3-1.7:0.23-0.43; the mass and volume ratio of the triphenylamine derivative, tert-butyl lithium and boron trifluoride ether to the ether in step (2) is 1 g:10-15 mL.

[0017] Preferably, the reaction temperature in step (2) is -68 to -88°C and the reaction time is 25 to 35 minutes;

[0018] In step (3), the mixing temperature is -68 to -88°C for 25 to 35 minutes, and the heating temperature is -2 to 2°C for 25 to 35 minutes.

[0019] Preferably, the mixing temperature in step (4) is -2 to 2°C, the time is 25 to 35 min, and the reaction temperature is 20 to 30°C, the time is 14 to 18 h.

[0020] Preferably, in the mixed solution of step (5), the concentration of the monomer of the boron-based electrochromic material is 0.1-2 mmol / L, the concentration of tetrabutylammonium hexafluorophosphate is 0.05-0.5 mol / L, and the volume ratio of chloroform to acetonitrile is 0.8-1.2:2.8-3.2.

[0021] Preferably, the scanning speed of the electrochemical polymerization in step (5) is 90-110 mV / s, the voltage is 0-1.3 V, and the number of cycles is 4-12.

[0022] The present invention also provides application of the boron-based electrochromic material in an electrochromic device.

[0023] The beneficial effects of the present invention are:

[0024] The present invention provides a boron-based electrochromic material, with boron as the center and triphenylamine derivatives as peripheral polymer groups. Among them, the triphenylamine derivative has a strong conjugated structure, and the formed electrochromic material can achieve a color change from transparent to blue under the drive of voltage. The optical contrast of the boron-based electrochromic material provided by the present invention is as high as 60% at 740nm, and the response time of coloring and fading is 4.8s and 1.8s respectively. In addition, after 150 cycles, the optical contrast of the boron-based electrochromic material is almost not attenuated. The boron-based electrochromic material provided by the present invention is an electrochromic material with excellent properties, and has broad application prospects in the field of display devices (such as anti-counterfeiting, color-changing glass, mobile phone back shell, electronic label, electronic paper). BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a synthetic route map of the boron-based electrochromic material in the present invention;

[0026] Figure 2 The cyclic voltammetry curve of the boron-based electrochromic material in Example 1 (abscissa Potential—voltage, ordinate Current—current);

[0027] Figure 3 The electrochemical polymerization curve of the boron-based electrochromic material in Example 1 (abscissa Potential—voltage, ordinate Current—current);

[0028] Figure 4 The UV-visible absorption spectra of the boron-based electrochromic material in Example 1 at different voltages (abscissa: Wavelength, ordinate: UVAbsorption intensity);

[0029] Figure 5This is the electrochromic performance diagram of the boron-based electrochromic material in Example 1 (abscissa Time—time, ordinate T—contrast);

[0030] Figure 6 This is a diagram of the optical contrast and response time of boron-based electrochromic materials (abscissa Time—time, ordinate T—contrast). DETAILED DESCRIPTION

[0031] The present invention provides a boron-based electrochromic material, wherein the structural formula of a monomer of the boron-based electrochromic material is:

[0032]

[0033] The present invention also provides a method for preparing the boron-based electrochromic material, comprising the following steps:

[0034] (1) under a protective atmosphere, diphenylamine, cuprous iodide, 2,2-bipyridine, potassium tert-butoxide, 2,5-dibromo-m-xylene and toluene are mixed and reacted to obtain a triphenylamine derivative;

[0035] (2) under a protective atmosphere, mixing a triphenylamine derivative and diethyl ether to react to obtain a mixture;

[0036] (3) mixing the mixture with tert-butyl lithium and heating to obtain a mixed solution;

[0037] (4) mixing the mixed solution with boron trifluoride etherate to react to obtain a monomer of a boron-based electrochromic material;

[0038] (5) Mixing the monomer of the boron-based electrochromic material, chloroform, acetonitrile and tetrabutylammonium hexafluorophosphate, and performing electrochemical polymerization to obtain the boron-based electrochromic material.

[0039] In the present invention, the molar ratio of diphenylamine, cuprous iodide, 2,2-bipyridine, potassium tert-butoxide and 2,5-dibromo-m-xylene in step (1) is preferably 0.8-1.2: 0.04-0.06: 0.04-0.06: 1.8-2.2: 1.0-1.4, and more preferably 0.85-1.15: 0.045-0.055: 0.045-0.055: 1.85-2.15: 1.0 5~1.35, more preferably 0.9~1.1:0.047~0.053:0.047~0.053:1.9~2.1:1.1~1.3; the mass and volume ratio of the diphenylamine, cuprous iodide, 2,2-bipyridine, potassium tert-butoxide, and 2,5-dibromo-meta-xylene to toluene is preferably 1g:10~15mL, further preferably 1g:11~14mL, and more preferably 1g:12~13mL.

[0040] In the present invention, the protective atmosphere in step (1) is nitrogen, argon, helium or neon.

[0041] In the present invention, the reaction temperature in step (1) is preferably 115-135°C, more preferably 120-130°C, and more preferably 122-128°C; the reaction time is preferably 22-26h, more preferably 23-25h, and more preferably 23.5-24.5h.

[0042] In the present invention, after the reaction in step (1) is completed, post-treatment is preferably performed, and the post-treatment comprises the following steps: extracting the sample obtained by the reaction, concentrating the extract after the reaction, dehydrating with anhydrous sodium sulfate, and then purifying by column chromatography, and finally collecting the obtained sample for rotary evaporation and drying to obtain the triphenylamine derivative.

[0043] In the present invention, the extraction reagents are saturated sodium chloride solution and dichloromethane, the volume ratio of the saturated sodium chloride solution to dichloromethane is preferably 0.8-1.2:0.8-1.2, more preferably 0.85-1.15:0.85-1.15, more preferably 0.9-1.1:0.9-1.1, the number of extractions is preferably 2-4 times, more preferably 3 times; the stationary phase of the column chromatography purification is silica gel, the mobile phase comprises dichloromethane and n-hexane, the volume ratio of dichloromethane to n-hexane is preferably 0.8-1.2:2.8-3.2, more preferably 0.85-1.1:0.85-1.15, more preferably 0.9-1.1:0.9-1.1, the number of extractions is preferably 2-4 times, more preferably 3 times; the stationary phase of the column chromatography purification is silica gel, the mobile phase comprises dichloromethane and n-hexane, the volume ratio of dichloromethane to n-hexane is preferably 0.8-1.2:2.8-3.2, more preferably 0.85-1 .15:2.85~3.15, more preferably 0.9~1.1:2.9~3.1; the rotary evaporation temperature is preferably 60~70°C, more preferably 62~68°C, more preferably 64~66°C; the rotary evaporation time is preferably 35~45min, more preferably 37~43min, more preferably 39~41min; the drying temperature is preferably 50~60°C, more preferably 52~58°C, more preferably 54~56°C; the drying time is preferably 22~26h, more preferably 23~25h, more preferably 23.5~24.5h.

[0044] In the present invention, the purpose of the rotary evaporation is to remove the solvent toluene.

[0045] In the present invention, the molar ratio of the triphenylamine derivative in step (2) to the tert-butyl lithium in step (3) and the boron trifluoride ether in step (4) is preferably 0.8-1.2:1.3-1.7:0.23-0.43, more preferably 0.9-1.1:1.4-1.6:0.25-0.41, and more preferably 0.95-1.05:1.45-1.55:0.27-0.39; the mass ratio of the triphenylamine derivative, tert-butyl lithium and boron trifluoride ether to the volume ratio of the ether in step (2) is preferably 1 g:10-15 mL, more preferably 1 g:11-14 mL, and more preferably 1 g:12-13 mL.

[0046] In the present invention, the protective atmosphere in step (2) is nitrogen, argon, helium or neon.

[0047] In the present invention, the reaction temperature in step (2) is preferably -68 to -88°C, more preferably -70 to -86°C, and more preferably -75 to -81°C; the reaction time is preferably 25 to 35 min, more preferably 27 to 33 min, and more preferably 29 to 31 min;

[0048] The mixing in step (3) is to add tert-butyl lithium dropwise to the mixture; the rate of the dropping is preferably 37 to 43 drops / minute, more preferably 38 to 42 drops / minute, and more preferably 39 to 41 drops / minute; the temperature of the mixing is preferably -68 to -88°C, more preferably -70 to -86°C, and more preferably -75 to -81°C; the time is preferably 25 to 35 minutes, more preferably 27 to 33 minutes, and more preferably 29 to 31 minutes; the heating temperature is preferably -2 to 2°C, more preferably -1 to 1°C, and more preferably -0.5 to 0.5°C; the time is preferably 25 to 35 minutes, more preferably 27 to 33 minutes, and more preferably 29 to 31 minutes.

[0049] In the present invention, the mixing temperature in step (4) is preferably -2 to 2°C, more preferably -1 to 1°C, and more preferably -0.5 to 0.5°C; the time is preferably 25 to 35 min, more preferably 27 to 33 min, and more preferably 29 to 31 min; the reaction temperature is preferably 20 to 30°C, more preferably 22 to 28°C, and more preferably 24 to 26°C; the time is preferably 14 to 18 h, more preferably 15 to 17 h, and more preferably 15.5 to 16.5 h.

[0050] In the present invention, after the reaction of step (4) is completed, post-treatment is preferably performed, and the post-treatment comprises the following steps: extracting the sample obtained by the reaction, concentrating the extract after the reaction, dehydrating with anhydrous sodium sulfate, and then purifying by column chromatography, and finally collecting the obtained sample for rotary evaporation and drying to obtain the triphenylamine derivative.

[0051] In the present invention, the extraction reagents are saturated sodium chloride solution and dichloromethane, the volume ratio of the saturated sodium chloride solution to dichloromethane is preferably 0.8-1.2:0.8-1.2, more preferably 0.85-1.15:0.85-1.15, more preferably 0.9-1.1:0.9-1.1, the number of extractions is preferably 2-4 times, more preferably 3 times; the stationary phase of the column chromatography purification is silica gel, the mobile phase comprises dichloromethane and n-hexane, the volume ratio of dichloromethane to n-hexane is preferably 0.8-1.2:2.8-3.2, more preferably 0.85-1.1:0.85-1.15, more preferably 0.9-1.1:0.9-1.1, the number of extractions is preferably 2-4 times, more preferably 3 times; the stationary phase of the column chromatography purification is silica gel, the mobile phase comprises dichloromethane and n-hexane, the volume ratio of dichloromethane to n-hexane is preferably 0.8-1.2:2.8-3.2, more preferably 0.85-1 .15:2.85~3.15, more preferably 0.9~1.1:2.9~3.1; the rotary evaporation temperature is preferably 60~70°C, more preferably 62~68°C, more preferably 64~66°C; the rotary evaporation time is preferably 35~45min, more preferably 37~43min, more preferably 39~41min; the drying temperature is preferably 50~60°C, more preferably 52~58°C, more preferably 54~56°C; the drying time is preferably 22~26h, more preferably 23~25h, more preferably 23.5~24.5h.

[0052] In the present invention, the purpose of the rotary evaporation is to remove the solvent ether.

[0053] In the present invention, the mixing in step (5) is preferably performed by adding the monomer of the boron-based electrochromic material and tetrabutylammonium hexafluorophosphate to a mixture of chloroform and acetonitrile and performing ultrasound. The frequency of the ultrasound is preferably 35 to 45 kHz, more preferably 37 to 43 kHz, and more preferably 39 to 41 kHz; the time of the ultrasound is preferably 2 to 4 min, more preferably 2.5 to 3.5 min, and more preferably 2.6 to 3.4 min.

[0054] In the present invention, the method of electrochemical polymerization in step (5) is preferably cyclic voltammetry, with tetrabutylammonium hexafluorophosphate as the electrolyte, ITO glass as the working electrode, platinum sheet as the counter electrode, and Ag / AgCl as the reference electrode; the size of the ITO glass is preferably 0.8-1.0 cm×3.5-4.5 cm, more preferably 0.85-0.95 cm×3.6-4.4 cm, and more preferably 0.87-0.93 cm×3.7-4.3 cm.

[0055] In the present invention, the concentration of the monomer of the boron-based electrochromic material in the mixed solution of step (5) is preferably 0.1-2 mmol / L, more preferably 0.5-1.6 mmol / L, and more preferably 0.7-1.4 mmol / L; the concentration of tetrabutylammonium hexafluorophosphate is preferably 0.05-0.5 mol / L, more preferably 0.1-0.45 mol / L, and more preferably 0.2-0.35 mol / L; the volume ratio of chloroform to acetonitrile is preferably 0.8-1.2:2.8-3.2, more preferably 0.85-1.15:2.85-3.15, and more preferably 0.9-1.1:2.9-3.1.

[0056] In the present invention, the scanning speed of the electrochemical polymerization in step (5) is preferably 90 to 110 mV / s, more preferably 95 to 105 mV / s, and more preferably 98 to 103 mV / s; the voltage is preferably 0 to 1.3 V, more preferably 0.5 to 0.8 V, and more preferably 0.6 to 0.7 V; the number of cycles is preferably 4 to 12, more preferably 5 to 11, and more preferably 6 to 10.

[0057] In the present invention, after the polymerization in step (5) is completed, the obtained sample is dedoped in a blank solution, and then washed and dried with nitrogen alternately to remove the electrolyte and oligomers on the membrane surface.

[0058] In the present invention, the blank solution is an acetonitrile solution of tetrabutylammonium hexafluorophosphate, and the mass volume ratio of the tetrabutylammonium hexafluorophosphate to acetonitrile is preferably 0.37-0.40 g: 8-12 mL, more preferably 0.38-0.39 g: 9-11 mL, and more preferably 0.382-0.388 g: 9.5-10.5 mL; the dedoping time is preferably 0.5-1.5 min, more preferably 0.7-1.3 min, and more preferably 0.9-1.1 min.

[0059] In the present invention, the cleaning solution is a mixture of chloroform and acetonitrile, and the volume ratio of chloroform to acetonitrile is preferably 0.8-1.2:0.8-1.2, more preferably 0.85-1.15:0.85-1.15, and more preferably 0.9-1.1:0.9-1.1; the number of alternations is preferably 2-4 times, and more preferably 3 times.

[0060] The present invention also provides application of the boron-based electrochromic material in an electrochromic device.

[0061] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0062] Example 1

[0063] Under nitrogen protection, 6.8mmol diphenylamine, 0.34mmol cuprous iodide, 0.35mmol 2,2-bipyridine, 13mmol potassium tert-butoxide and 8mmol 2,5-dibromo-m-xylene were mixed with 60mL toluene, and reacted at 125°C for 24h. The obtained sample was extracted 3 times with saturated sodium chloride solution and dichloromethane (volume ratio of 1:1), and the obtained extract was concentrated and dehydrated with anhydrous sodium sulfate. Then, column chromatography was performed with silica gel as the stationary phase and dichloromethane and n-hexane as the mobile phase (the volume ratio of dichloromethane to n-hexane was 1:3) for purification. The obtained sample was collected and rotary evaporated at 65°C for 40min, and then dried at 55°C for 24h to obtain a white solid, which is a triphenylamine derivative. The yield of the triphenylamine derivative is 32%, and the characterization structure of the triphenylamine derivative is as follows: 1 HNMR(500MHzCDCl3)δ=7.27~7.21(4H,m), 7.05~7.01(6H,m), 6.81(2H,s);

[0064] Under nitrogen protection, the triphenylamine derivative and diethyl ether were mixed and reacted at -78°C for 30 minutes, and then tert-butyl lithium was added to the mixture at 40 drops / minute, mixed at -78°C for 30 minutes, and then the mixture was heated to 0°C and stirred for 30 minutes, and then boron trifluoride diethyl ether was added (the molar ratio of triphenylamine derivative, tert-butyl lithium and boron trifluoride diethyl ether was 1:1.5:0.33, and the mass and volume ratio of triphenylamine derivative, tert-butyl lithium and boron trifluoride diethyl ether to diethyl ether was 1g:12mL), stirred at 0°C for 30 minutes, and then heated The reaction mixture was heated to 25°C for 16 hours, and the obtained sample was extracted three times with a saturated sodium chloride solution and dichloromethane (volume ratio of 1:1). The obtained extract was concentrated, and water was removed with anhydrous sodium sulfate. Then, column chromatography was performed using silica gel as the stationary phase and dichloromethane and n-hexane as the mobile phase (the volume ratio of dichloromethane to n-hexane was 1:3). The obtained sample was collected and rotary evaporated at 65°C for 40 minutes, and then dried at 55°C for 24 hours to obtain a yellow solid, which is the monomer of the boron-based electrochromic material. The yield of the monomer is 16%, and the characterization structure of the monomer is as follows: 1 HNMR(CDCl3)δ=7.31~7.21(12H,m), 7.09(12H,td), 7.02(6H,tt), 6.63(6H,s);

[0065] The monomer of the boron-based electrochromic material and tetrabutylammonium hexafluorophosphate were added to a mixture of 2.5 mL of chloroform and 7.5 mL of acetonitrile (the concentration of the monomer in the mixture was 0.5 mmol / L, and the concentration of tetrabutylammonium hexafluorophosphate was 0.1 mol / L), and ultrasonicated at 40 kHz for 3 min. Then, electrochemical polymerization was performed by cyclic voltammetry using ITO glass (0.9*4 cm) as the working electrode, platinum sheet as the counter electrode, and Ag / AgCl as the reference electrode. The scanning speed was set to 100 mV / s. , the voltage was 0.6V, the number of cycles was 10, and after the polymerization was completed, the obtained sample was dedoped in an acetonitrile solution of tetrabutylammonium hexafluorophosphate (the mass volume ratio of tetrabutylammonium hexafluorophosphate to acetonitrile was 0.387g:10mL) for 1 min, and then washed with a mixed solution of chloroform and acetonitrile (volume ratio was 1:1), and dried with nitrogen, and the washing and drying were repeated 3 times to obtain the boron-based electrochromic material (denoted as p3TPA-B). The synthesis route of the boron-based electrochromic material in this embodiment is as shown in Figure 1 shown.

[0066] 0.387 g of tetrabutylammonium hexafluorophosphate was added to a 10 mL volumetric flask, and the volume was fixed with acetonitrile. This was used as a blank solution. The ITO glass covered with the boron-based electrochromic material prepared in this example was used as a working electrode, and Ag / AgCl was used as a reference electrode. Electrochemical, optical and electrochromic performance tests were performed to obtain a cyclic voltammetry curve of the boron-based electrochromic material. Figure 2 As shown; the electrochemical polymerization curve of the boron-based electrochromic material, such as Figure 3 As shown; UV-visible absorption spectra of boron-based electrochromic materials at different voltages, such as Figure 4 As shown; the electrochromic performance diagram of boron-based electrochromic materials, such as Figure 5 As shown; The optical contrast and response time diagram of boron-based electrochromic materials, such as Figure 6 shown.

[0067] from Figure 2 It can be seen that the boron-based electrochromic material has a pair of redox peaks at 0-1.3V, that is, the oxidation peak is 1.1V and the reduction peak is 0.6V; Figure 3 It can be seen that the polymerization voltage of the boron-based electrochromic material monomer is 0-1.2V, the scanning speed is 100mV / s, and the number of polymerization cycles is 10; Figure 4 It can be seen that the boron-based electrochromic material can achieve a reversible color change from transparent to blue at a voltage of 0 to 1.2 V; Figure 6 It can be seen that the coloring time of the boron-based electrochromic material at 740nm is 4.8s, the fading time is 1.8s, and the contrast ratio at 740nm is as high as 60%; and from Figure 5It can also be seen that after 150 cycles, the contrast of the boron-based electrochromic material has almost no attenuation, showing good electrochemical stability.

[0068] Example 2

[0069] Under neon protection, 7mmol diphenylamine, 0.35mmol cuprous iodide, 0.36mmol 2,2-bipyridine, 13.2mmol potassium tert-butoxide and 8.4mmol 2,5-dibromo-m-xylene and 56mL toluene were mixed and reacted at 118°C for 25h. The obtained sample was extracted 4 times with saturated sodium chloride solution and dichloromethane (volume ratio of 1:1.1). The obtained extract was concentrated and dehydrated with anhydrous sodium sulfate. Then, column chromatography was performed with silica gel as the stationary phase and dichloromethane and n-hexane as the mobile phase (the volume ratio of dichloromethane to n-hexane was 1:3.2) for purification. The obtained sample was collected and rotary evaporated at 66°C for 38min, and then dried at 57°C for 23h to obtain a white solid, which was a triphenylamine derivative.

[0070] Under neon protection, the triphenylamine derivative and diethyl ether were mixed and reacted at -75°C for 27 minutes, and then tert-butyl lithium was added to the mixture at 41 drops / minute, and mixed at -75°C for 27 minutes. The mixture was then heated to 1°C and stirred for 28 minutes, and then boron trifluoride diethyl ether was added (the molar ratio of the triphenylamine derivative, tert-butyl lithium and boron trifluoride diethyl ether was 1.1:1.55:0.35, and the mass and volume ratio of the triphenylamine derivative, tert-butyl lithium and boron trifluoride diethyl ether to diethyl ether was 1 g:13 mL), and stirred at 1°C. 28min, then heated to 27℃ for reaction for 16.5h, the obtained sample was extracted 4 times with saturated sodium chloride solution and dichloromethane (volume ratio of 1:1.1), the obtained extract was concentrated, dehydrated with anhydrous sodium sulfate, and then purified by column chromatography using silica gel as the stationary phase and dichloromethane and n-hexane as the mobile phase (the volume ratio of dichloromethane and n-hexane was 1:2.8), the obtained sample was collected and rotary evaporated at 66℃ for 38min, and then dried at 57℃ for 23h to obtain a yellow solid, which is the monomer of the boron-based electrochromic material;

[0071] The monomer of the boron-based electrochromic material and tetrabutylammonium hexafluorophosphate were added to a mixture of 2.4 mL of chloroform and 7.6 mL of acetonitrile (the concentration of the monomer in the mixture was 0.7 mmol / L, and the concentration of tetrabutylammonium hexafluorophosphate was 0.3 mol / L), and ultrasonicated at 37 kHz for 2.5 min. Then, electrochemical polymerization was carried out by cyclic voltammetry using ITO glass (0.95*4.2 cm) as the working electrode, platinum sheet as the counter electrode, and Ag / AgCl as the reference electrode. The scanning speed was set to 105 mV / s, the voltage was set to 0.65 V, and the number of cycles was set to 8. After the polymerization was completed, the obtained sample was dedoped in an acetonitrile solution of tetrabutylammonium hexafluorophosphate (the mass volume ratio of tetrabutylammonium hexafluorophosphate to acetonitrile was 0.375 g: 10 mL) for 1.2 min, and then washed with a mixed solution of chloroform and acetonitrile (volume ratio of 1: 1.1), and dried with nitrogen, and the washing and drying were repeated twice to obtain the boron-based electrochromic material.

[0072] The boron-based electrochromic material obtained in this example was tested by the same method as in Example 1, and the results showed that the boron-based electrochromic material obtained in this example could achieve a reversible color change from transparent to blue under a step voltage of 0 to 1.2 V, and its coloring time at 740 nm was 4.6 s, and its fading time was 2.0 s. The contrast at 740 nm was as high as 58%, and after 150 cycles, the contrast was almost not attenuated, showing good electrochemical stability.

[0073] Example 3

[0074] Under nitrogen protection, 6.5mmol diphenylamine, 0.34mmol cuprous iodide, 0.32mmol 2,2-bipyridine, 13mmol potassium tert-butoxide and 6.5mmol 2,5-dibromo-m-xylene and 52mL toluene were mixed and reacted at 127°C for 23h. The obtained sample was extracted 3 times with saturated sodium chloride solution and dichloromethane (volume ratio of 0.9:1). The obtained extract was concentrated and dehydrated with anhydrous sodium sulfate. Then, column chromatography was performed with silica gel as the stationary phase and dichloromethane and n-hexane as the mobile phase (the volume ratio of dichloromethane to n-hexane was 1:2.9) for purification. The obtained sample was collected and rotary evaporated at 63°C for 42min, and then dried at 57°C for 22h to obtain a white solid, which was a triphenylamine derivative.

[0075] Under nitrogen protection, the triphenylamine derivative and diethyl ether were mixed and reacted at -82°C for 31 minutes, and then tert-butyl lithium was added to the mixture at 39 drops / minute, mixed at -82°C for 28 minutes, and then the mixture was heated to -1°C and stirred for 31 minutes, and then boron trifluoride diethyl ether was added (the molar ratio of the triphenylamine derivative, tert-butyl lithium and boron trifluoride diethyl ether was 0.8:1.4:0.27, and the mass and volume ratio of the triphenylamine derivative, tert-butyl lithium and boron trifluoride diethyl ether to diethyl ether was 1 g:11.5 mL) and stirred at 1°C. Stir for 30 minutes, then heat to 24°C and react for 15 hours. The obtained sample is extracted three times with a saturated sodium chloride solution and dichloromethane (volume ratio of 0.9:1), the obtained extract is concentrated, and water is removed with anhydrous sodium sulfate. Then, column chromatography is performed using silica gel as the stationary phase and dichloromethane and n-hexane as the mobile phase (the volume ratio of dichloromethane to n-hexane is 1:2.9) to purify the product. The obtained sample is collected and rotary evaporated at 63°C for 42 minutes, and then dried at 57°C for 22 hours to obtain a yellow solid, which is the monomer of the boron-based electrochromic material.

[0076] The monomer of the boron-based electrochromic material and tetrabutylammonium hexafluorophosphate were added to a mixture of 2.6 mL of chloroform and 7.4 mL of acetonitrile (the concentration of the monomer in the mixture was 1 mmol / L, and the concentration of tetrabutylammonium hexafluorophosphate was 0.25 mol / L), and ultrasonicated at 42 kHz for 3 min. Then, electrochemical polymerization was carried out by cyclic voltammetry using ITO glass (0.8*3.5 cm) as a working electrode, a platinum sheet as a counter electrode, and Ag / AgCl as a reference electrode. The scanning speed was set to 95 mV / s, the voltage was 0.5 V, and the number of cycles was 11. After the polymerization was completed, the obtained sample was dedoped in an acetonitrile solution of tetrabutylammonium hexafluorophosphate (the mass volume ratio of tetrabutylammonium hexafluorophosphate to acetonitrile was 0.39 g:10 mL) for 1 min. After the end, it was washed with a mixture of chloroform and acetonitrile to obtain the boron-based electrochromic material.

[0077] The boron-based electrochromic material obtained in this example was tested by the same method as in Example 1, and the results showed that the boron-based electrochromic material obtained in this example could achieve a reversible color change from transparent to blue under a step voltage of 0 to 1.2 V, and its coloring time at 740 nm was 4.7 s, and its fading time was 1.9 s. The contrast at 740 nm was as high as 57%, and there was almost no contrast attenuation after 150 cycles, showing good electrochemical stability.

[0078] From the above examples, it can be seen that the present invention provides a boron-based electrochromic material, the optical contrast at 740nm is as high as 60%, and the response time of coloring and fading is 4.8s and 1.8s respectively. In addition, after 150 cycles, the optical contrast of the boron-based electrochromic material is almost not attenuated. The boron-based electrochromic material provided by the present invention is an electrochromic material with excellent properties, and has broad application prospects in the field of display devices (such as anti-counterfeiting, color-changing glass, mobile phone back shell, electronic label, electronic paper).

[0079] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A boron-based electrochromic material, characterized in that: The structural formula of the monomer of the boron-based electrochromic material is: The boron-based electrochromic material is obtained by electrochemical polymerization of monomers of the boron-based electrochromic material.

2. The method for preparing the boron-based electrochromic material according to claim 1, characterized in that: It includes the following steps: (1) under a protective atmosphere, diphenylamine, cuprous iodide, 2,2-bipyridine, potassium tert-butoxide, 2,5-dibromo-m-xylene and toluene are mixed and reacted to obtain a triphenylamine derivative; (2) under a protective atmosphere, mixing a triphenylamine derivative and diethyl ether to react to obtain a mixture; (3) mixing the mixture with tert-butyl lithium and heating to obtain a mixed solution; (4) mixing the mixed solution with boron trifluoride etherate to react to obtain a monomer of a boron-based electrochromic material; (5) Mixing the monomer of the boron-based electrochromic material, chloroform, acetonitrile and tetrabutylammonium hexafluorophosphate, and performing electrochemical polymerization to obtain the boron-based electrochromic material.

3. The preparation method according to claim 2, characterized in that: The molar ratio of the diphenylamine, cuprous iodide, 2,2-bipyridine, potassium tert-butoxide and 2,5-dibromo-meta-xylene in step (1) is 0.8-1.2: 0.04-0.06: 0.04-0.06: 1.8-2.2: 1.0-1.4; the mass and volume ratio of the diphenylamine, cuprous iodide, 2,2-bipyridine, potassium tert-butoxide and 2,5-dibromo-meta-xylene to toluene is 1 g: 10-15 mL.

4. The preparation method according to claim 2 or 3, characterized in that: The reaction temperature of step (1) is 115-135° C., and the reaction time is 22-26 hours.

5. The preparation method according to claim 4, characterized in that: The molar ratio of the triphenylamine derivative in step (2) to the tert-butyl lithium in step (3) and the boron trifluoride ether in step (4) is 0.8-1.2:1.3-1.7:0.23-0.43; the mass and volume ratio of the triphenylamine derivative, tert-butyl lithium and boron trifluoride ether to the ether in step (2) is 1 g:10-15 mL.

6. The preparation method according to claim 5, characterized in that: The reaction temperature in step (2) is -68 to -88°C and the reaction time is 25 to 35 minutes; In step (3), the mixing temperature is -68 to -88°C for 25 to 35 minutes, and the heating temperature is -2 to 2°C for 25 to 35 minutes.

7. The preparation method according to claim 5 or 6, characterized in that: The mixing temperature of step (4) is -2 to 2°C, and the time is 25 to 35 minutes. The reaction temperature is 20 to 30°C, and the time is 14 to 18 hours.

8. The preparation method according to claim 7, characterized in that: In the mixed solution of step (5), the concentration of the monomer of the boron-based electrochromic material is 0.1-2 mmol / L, the concentration of tetrabutylammonium hexafluorophosphate is 0.05-0.5 mol / L, and the volume ratio of chloroform to acetonitrile is 0.8-1.2:2.8-3.

2.

9. The preparation method according to claim 8, characterized in that: The scanning speed of the electrochemical polymerization in step (5) is 90-110 mV / s, the voltage is 0-1.3 V, and the number of cycles is 4-12.

10. Use of the boron-based electrochromic material according to claim 1 in an electrochromic device.