An epitaxial structure of an LED device and a preparation method thereof and a semiconductor device
By using metal nanoparticles to etch the n-type GaN layer in the LED device to form a pit structure and grow multiple quantum well layers, the problems of low light extraction efficiency and quantum well structure degradation of single-chip dual-color LED devices are solved, and efficient multi-wavelength devices are achieved. Light emission and structural stability.
Patent Information
- Application Number
- CN202310175595.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-02-28
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-02-28
Smart Images

Figure CN116190506B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of semiconductor technology, and in particular to an epitaxial structure of an LED device and a preparation method thereof, and a semiconductor device. Background Art
[0002] At present, the "direct emission white light technology" can be used to realize white light illumination using light-emitting diodes (LEDs). The single-chip solution in the "direct emission white light technology" uses a stacked quantum well LED structure with multiple active layers on a single chip to emit multi-color light to synthesize white light. In a typical single-chip dual-active layer dual-color LED device structure, the active layer is a 5-period InGaN / GaN multi-quantum well, using different indium (In) components to emit blue light with a wavelength of 460nm and green light with a wavelength of 520nm, respectively, without using fluorescent substances to obtain white light. This solution is the mainstream technical solution in the "direct emission white light technology".
[0003] However, the current monolithic dual-active layer dual-color LED device has the following disadvantages: First, due to the different In components and bandgap widths of the InGaN in the two active layers, the active layer with a higher In component has a longer emission wavelength and a smaller bandgap width, and has a strong absorption effect on short-wavelength light. In conventional device structures, the short-wavelength light emitted downward by the quantum well will be reflected by the substrate and re-emitted from the device surface; but in this dual-active layer dual-color LED device structure, the blue light emitted downward will be absorbed in the process of passing through the yellow light active layer, reducing the final light output efficiency of the device. Second, the long-wavelength quantum well structure is currently placed at the bottom and the short-wavelength quantum well structure is placed at the top. In the process of growing the short-wavelength quantum well structure, the growth temperature is usually higher than the temperature of the long-wavelength quantum well structure. Increasing the temperature will cause the InGaN material to decompose, so the performance of the long-wavelength quantum well structure will degrade. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention provides an epitaxial structure of an LED device, a preparation method thereof and a semiconductor device. In the process of manufacturing the epitaxial structure, an n-type GaN layer is etched by using metal nanoparticles as a mask to obtain a GaN layer containing pits. The subsequently grown InGaN / GaN multiple quantum well can contain different In component contents in a single InGaN layer, thereby obtaining an LED device that can emit two light wavelengths, thereby improving the luminous efficiency of the device.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides a method for preparing an epitaxial structure of an LED device, the method comprising:
[0007] providing a substrate;
[0008] growing a buffer layer on the substrate;
[0009] Growing GaN on the buffer layer to form a basic n-type GaN layer; growing a metal layer on the basic n-type GaN layer, and annealing the metal layer to obtain metal nanoparticles; using the metal nanoparticles as a mask, etching the basic n-type GaN layer, and removing the remaining metal nanoparticles to form an n-type GaN layer containing pits;
[0010] An InGaN layer and a GaN layer are periodically grown on the n-type GaN layer to form a multi-quantum well layer; the InGaN layer contains InGaN pits corresponding to the pits of the n-type GaN layer; the InGaN layer includes a first region and a second region, the first region is a side wall of the InGaN pit; the second region is a bottom plane of the InGaN pit and a peripheral plane of the InGaN pit; the In content in the first region and the second region is different;
[0011] An electron blocking layer and a p-type nitride layer are sequentially grown on the n-type GaN layer.
[0012] The method for preparing the epitaxial structure of the LED device provided by the present invention uses the metal nanoparticles generated after annealing as a mask to selectively etch the basic n-type GaN layer, so that the surface of the n-type GaN layer contains pits and a polar surface and a non-polar surface; then, by growing InGaN on the polar surface and the non-polar surface, an InGaN layer with different In contents in the first region and the second region can be obtained, so that two different wavelengths of light can be emitted. The method provided by the present invention does not involve a photolithography process, and the process flow is simpler; and a single-layer growth can obtain an InGaN layer with different In contents, which solves the problem of degradation of the long-wavelength quantum well structure in the preparation process of the stacked double active layer structure, and improves the light extraction efficiency.
[0013] Preferably, the sidewall of the pit is a non-polar surface, and the bottom plane of the pit and the peripheral plane of the pit are polar surfaces.
[0014] Preferably, the thickness of the metal layer is 20-80 nm, for example, 20 nm, 25 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm or 80 nm.
[0015] Since the metal layer needs to be annealed to form uniformly distributed metal nanoparticles in the present invention, the thickness of the metal layer is critical to the formation of the metal nanoparticles. The present invention preferably controls the thickness of the metal layer within the above range, which can avoid the problem that the diameter of the metal nanoparticles is too small to achieve a better masking effect, and can also avoid the problem that the diameter of the metal nanoparticles is too large and the uniformity is reduced.
[0016] Preferably, the surface roughness of the metal layer is ≤2 nm.
[0017] Preferably, the growth temperature of the metal layer is 80-120°C and the vacuum degree is 10 -5 ~10 -6 Pa or less, the temperature may be, for example, 80°C, 90°C, 100°C, 105°C, 110°C, 115°C or 120°C.
[0018] Since the atomic decomposition efficiency of the material reaction source is reduced under low temperature conditions, the atoms cannot fully migrate within the plane, resulting in poor uniformity of atomic distribution, making it difficult to form a uniform metal layer, and easily forming an etched-like surface under excessively high temperatures. The present invention preferably controls the thickness of the metal layer, and further preferably controls the growth temperature and vacuum degree within the above range, thereby avoiding the appearance of etched-like surfaces and uneven surfaces, and ensuring that a metal layer of uniform thickness can be formed.
[0019] If the thickness of the metal layer is uneven, the particle size of the subsequently generated nanoparticles will be uneven. The present invention can control the surface roughness of the metal layer within 2nm by controlling the growth temperature of the above-mentioned metal layer, thereby providing a basis for the subsequent preparation of metal nanoparticles with uniform particle size.
[0020] Preferably, the metal layer is a nickel metal layer, and the metal nanoparticles are nickel nanoparticles.
[0021] Compared with other metals, the nickel metal layer can better form nickel nanoparticles after annealing. The nickel nanoparticles are evenly distributed and have a moderate particle size, and are more suitable for use as the mask nanoparticles of the present invention. Therefore, the preferred metal layer is a nickel metal layer so that nickel nanoparticles with an ideal mask structure can be obtained later.
[0022] Preferably, the annealing temperature is 700-900°C, and the annealing time is 5-40 min. The annealing temperature can be, for example, 700°C, 720°C, 750°C, 780°C, 800°C, 820°C, 850°C, 880°C or 900°C.
[0023] The technical difficulty of the present invention lies in how to obtain uniformly distributed metal nanoparticles with appropriate particle size without affecting the performance of the original n-type GaN layer. Under the temperature conditions of annealing treatment, the metal layer gradually forms metal nanoparticles in the first stage, and the diameter of the metal nanoparticles decreases continuously with the increase of annealing time. Due to the different saturated vapor pressures of the metal nanoparticles formed in the second stage, the larger metal nanoparticles continuously absorb the surrounding small metal nanoparticles and continue to grow, so that the diameter of the metal nanoparticles increases continuously until all the metal nanoparticles are completely separated. Therefore, the present invention can obtain metal nanoparticles with appropriate particle size by controlling the temperature and time of annealing treatment within the above range, and at the same time expose part of the surface of the n-type GaN layer to provide conditions for subsequent etching.
[0024] Furthermore, the theoretical formula for the continued growth of metal nanoparticles in the second stage during the annealing treatment of the present invention is the Gibbs-Simpson relationship, as shown in formula (1):
[0025] a i =a ∞ exp(2Ωγ / r i kT) formula (1)
[0026] In formula (1): a i is the activity value of the i-th particle, i refers to any particle; r i is the particle size of the ith particle; a ∞ is the activity value of the atoms in the infinite particle; Ω is the atomic volume; γ is the interface energy per unit area; k is the Boltzmann constant; T is the temperature.
[0027] According to the Gibbs-Simpson relationship, smaller particles will have higher activities and therefore higher equilibrium vapor pressures, and vice versa. When two particles of different sizes are close to each other, the atoms in the smaller particle tend to evaporate spontaneously, while the larger particle absorbs the evaporated atoms because of its lower equilibrium vapor pressure. As a result, the larger islands continue to absorb atoms and grow, while the smaller islands continue to lose atoms and disappear.
[0028] Preferably, the flow rate of ammonia gas introduced during the annealing treatment is 1000-2000sccm, for example, it can be 1000sccm, 1100sccm, 1200sccm, 1300sccm, 1400sccm, 1500sccm, 1600sccm, 1700sccm, 1800sccm, 1900sccm or 2000sccm.
[0029] In the present invention, ammonia gas can produce a certain corrosive effect on the metal layer during the annealing process, thereby promoting the heated metal layer to shrink and form metal nanoparticles.
[0030] Since a flow rate that is too high will reduce the uniformity of the particle size of the metal nanoparticles, and a flow rate that is too low will result in an inability to fully react to form metal nanoparticles; therefore, the present invention controls the flow rate of ammonia within the above range to ensure the formation of metal nanoparticles with a suitable particle size.
[0031] Preferably, the particle size of the metal nanoparticles is in the range of 300 to 800 nm, for example, 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 550 nm, 600 nm, 650 nm, 700 nm or 800 nm.
[0032] The present invention controls the particle size range of the metal nanoparticles within 300-800 nm, which is conducive to controlling the size of the subsequent InGaN pits within a preset range, thereby better controlling the area ratio of the polar surface and the non-polar surface.
[0033] For example, the particle size distribution of the metal nanoparticles is D10=450 nm, D90=550 nm.
[0034] Preferably, the etching process includes inductively coupled plasma etching or reactive ion etching.
[0035] Preferably, the power of the inductively coupled plasma etching is 800-1000W, the pressure is 2-5Pa, and the self-bias is 150-200V. The power of the inductively coupled plasma etching is 800-1000W, for example, 800W, 810W, 820W, 850W, 900W, 910W, 920W, 950W, 980W or 1000W. The pressure is 2-5Pa, for example, 2Pa, 2.5Pa, 3Pa, 3.5Pa, 4Pa, 4.5Pa or 5Pa. The self-bias is 150-200V, for example, 150V, 155V, 160V, 165V, 170V, 175V, 180V, 185V, 190V or 200V.
[0036] Preferably, 30-50 sccm of chlorine gas and 5-20 sccm of argon gas are introduced into the inductively coupled plasma etching. The flow rate of chlorine gas may be, for example, 30 sccm, 32 sccm, 35 sccm, 38 sccm, 40 sccm, 42 sccm, 45 sccm, 48 sccm or 50 sccm, etc. The flow rate of argon gas may be, for example, 5 sccm, 6 sccm, 7 sccm, 8 sccm, 10 sccm, 12 sccm, 14 sccm, 15 sccm, 18 sccm or 20 sccm, etc.
[0037] Preferably, the etching depth is 300-800 nm, for example, may be 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 550 nm, 600 nm, 650 nm, 700 nm, 750 nm or 800 nm.
[0038] The present invention etches the surface of n-type GaN with metal nanoparticles as a mask, and the side formed after etching is a non-polar surface, and the etched bottom and the unetched top are polar surfaces. By adjusting the etching depth, GaN polar surfaces and GaN non-polar surfaces with different area ratios can be obtained. Furthermore, if the etching depth is too shallow, the area of the GaN non-polar surface is too small, and the contribution to the subsequent luminescence is too small, and the LED device cannot be obtained; if the etching depth is too deep, the gas flow reaching the bottom of the etching during the subsequent growth process is too small, resulting in a low growth rate at the bottom position, and the deviation between the design value and the actual value of the InGaN / GaN multi-quantum well structure is too large, resulting in a decrease in the luminous efficiency of the device; based on this, the etching depth is preferably within the above range, which can effectively ensure that the area ratio of the GaN polar surface and the GaN non-polar surface is within a reasonable range.
[0039] Preferably, the growth temperature of the multi-quantum well layer is 850-950° C., and the pressure is 300-500 mbar. The growth temperature may be, for example, 850° C., 860° C., 870° C., 880° C., 890° C., 900° C., 910° C., 920° C., 930° C., 940° C., or 950° C. The pressure may be, for example, 300 mbar, 310 mbar, 340 mbar, 350 mbar, 380 mbar, 400 mbar, 420 mbar, 450 mbar, or 500 mbar.
[0040] Preferably, the flow ratio of NH3:TMGa:TMIn during the growth of the InGaN layer of the multi-quantum well layer is (20000-40000):(200-300):(50-150), for example, it can be 20000:200:50, 20000:300:50, 30000:200:150, 20000:250:100, 40000:250:50, 30000:250:50 or 25000:250:100, etc.
[0041] In order to obtain two non-overlapping luminescence wavelengths as much as possible, the present invention needs to widen the difference in In component content between the first region and the second region in the InGaN layer. By controlling the flow ratio of NH3:TMGa:TMIn in the InGaN layer growth within the above range, it can be ensured that the difference in In component content in the InGaN layers grown on different crystal planes reaches an ideal value, thereby achieving emission of two luminescence wavelengths.
[0042] In a second aspect, the present invention provides an epitaxial structure of an LED device, the epitaxial structure comprising:
[0043] substrate;
[0044] a buffer layer located on the substrate;
[0045] An n-type GaN layer located on the buffer layer and containing pits; wherein the n-type GaN layer containing pits is obtained by etching a basic n-type GaN layer located on the buffer layer using metal nanoparticles as a mask, the metal nanoparticles are obtained by annealing a metal layer on the basic n-type GaN layer, and after forming the n-type GaN layer containing pits, the metal nanoparticles are removed;
[0046] A multi-quantum well layer located on the n-type GaN layer; the multi-quantum well layer comprises an InGaN layer and a GaN layer that are periodically and alternately arranged; the InGaN layer comprises an InGaN pit corresponding to the pit of the n-type GaN layer; the InGaN layer comprises a first region and a second region, the first region being a side wall of the InGaN pit; the second region being a bottom plane of the InGaN pit and a peripheral plane of the InGaN pit; the In content in the first region and the second region is different;
[0047] an electron blocking layer located on the multi-quantum well layer;
[0048] A p-type nitride layer is located on the electron blocking layer.
[0049] The present invention provides an n-type GaN layer of an epitaxial structure including pits containing polar and non-polar surfaces, an InGaN layer in a multi-quantum well layer continues to grow on the polar and non-polar surfaces, and different atomic arrangements of different crystal planes affect the efficiency of In atoms being incorporated into the GaN lattice, ultimately resulting in different In component contents in InGaN of different crystal planes, thereby forming a first region and a second region with different In component contents in a single-layer InGaN layer, achieving two light-emitting wavelengths for the same epitaxial wafer, and further achieving the preparation of an LED device.
[0050] Compared with a stacked double active layer structure, the epitaxial wafer structure provided by the present invention can prevent short-wavelength light from being absorbed by the active layer with a high In component content, thereby improving the luminous efficiency of the device; moreover, a single multi-quantum well layer can be used to emit light of two wavelengths, thereby avoiding the problem of performance degradation of the long-wavelength multi-quantum well layer due to the arrangement of two upper and lower multi-quantum well layers, thereby helping to improve the performance of the device.
[0051] Preferably, the metal nanoparticles are nickel nanoparticles.
[0052] Preferably, the depth of the InGaN pit is 300-800 nm, for example, it may be 300 nm, 350 nm, 400 nm, 450 nm, 500 nm, 550 nm, 600 nm, 650 nm, 700 nm, 750 nm or 800 nm.
[0053] Preferably, the area ratio of the first region to the second region is (1:2) to (2:1), for example, it can be 1:2, 1.2:2, 1.5:2, 2:2, 2:1.5, 2:1.2 or 2:1, etc.
[0054] The present invention can adjust the area ratio of the polar surface of GaN and the non-polar surface of GaN within the above range, thereby effectively controlling the intensity ratio of the two luminescent wavelengths.
[0055] Preferably, the thickness of the n-type GaN layer is 2000-4000 nm, for example, 2000 nm, 2300 nm, 2500 nm, 3000 nm, 3200 nm, 3500 nm or 4000 nm.
[0056] When the thickness of the n-type GaN layer is too thick, the growth time will be too long and the device cost will be too high; when the thickness of the n-type GaN layer is too thin, the conductivity of the n-type GaN layer after etching will be poor, the current distribution will be uneven, and the luminescence performance of the device will be reduced; based on this, the present invention controls the thickness of the n-type GaN layer within the above range so that the GaN layer of a specific thickness can provide an area for the non-polar side surface after etching, thereby flexibly adjusting the area ratio of the polar surface of GaN and the non-polar surface of GaN; and after etching, the thickness of the n-type GaN layer can still be moderate, without affecting the original performance (such as: luminescence brightness), and has the advantage of controllable luminescence performance.
[0057] Preferably, the absolute value of the difference between the In content in the first region and the In content in the second region in the InGaN layer is 5% to 10%, for example, it can be 5%, 5.5%, 6%, 6.5%, 7%, 7.5%, 8%, 8.5%, 9% or 10%, etc., preferably 6.5% to 10%.
[0058] Since the higher the In component content, the longer the luminescent wavelength, the present invention can ensure that two luminescent wavelengths with a wavelength difference of 20 to 50 nm are obtained by controlling the difference in In content between the first region and the second region within the range of 5% to 10%, thereby better realizing white light emission technology.
[0059] The epitaxial structure described in the second aspect of the present invention is preferably prepared by the preparation method described in the first aspect, which can avoid the introduction of photolithography process and can more conveniently regulate the luminous intensity of the two lights.
[0060] In a third aspect, the present invention provides a semiconductor device comprising the epitaxial structure of the LED device described in the second aspect.
[0061] Since the semiconductor device provided by the present invention includes the epitaxial structure provided by the first aspect, it can realize the emission of white light and has high light extraction efficiency.
[0062] Compared with the prior art, the present invention has at least the following beneficial effects:
[0063] (1) The epitaxial structure of the LED device provided by the present invention realizes a different design of the In component content in the single-layer InGaN layer, and can emit two wavelengths of light at the same time. In addition, there is no overlapping position relationship between the two active layers. Therefore, when extracting light, there is no process in which short-wavelength light passes through the long-wavelength active layer and is absorbed, thereby improving the light extraction efficiency of the device and thus improving the luminous efficiency of the LED device.
[0064] (2) The epitaxial structure of the LED device provided by the present invention can adjust the ratio of the intensity of light of two emission wavelengths by adjusting the area ratio of the polar surface of GaN and the non-polar surface of GaN within a preset range, thereby being able to meet the preparation of semiconductor devices with different requirements and having strong applicability.
[0065] (3) The method for preparing the epitaxial structure of the LED device provided by the present invention obtains metal nanoparticles by annealing the metal layer. Not only does it not affect the performance of the original n-type GaN layer, but also by controlling the annealing temperature and time, it is possible to obtain metal nanoparticles with uniform particle size and appropriate size, which is helpful for the subsequent preparation of an n-type GaN layer with uniform distribution of polar and non-polar surfaces.
[0066] (4) The method for preparing the epitaxial structure of the LED device provided by the present invention uses metal nanoparticles as a mask to etch the basic n-type GaN to obtain n-type GaN layers with different crystal planes, so that different In components can be grown under the same growth conditions, avoiding the problem of degradation of the long-wavelength quantum well structure due to different growth conditions, which helps to improve the performance of the device.
[0067] (5) The method for preparing the epitaxial structure of the LED device provided by the present invention can adjust the difference in In component content between the first region and the second region in the InGaN layer by adjusting the process parameters, thereby better adjusting the wavelength difference between the emission wavelengths to meet different application requirements. BRIEF DESCRIPTION OF THE DRAWINGS
[0068] Figures 1 to 10 It is a structural schematic diagram corresponding to each step in the method for preparing the epitaxial structure of the LED device provided by the present invention.
[0069] Fig.11It is the luminescence spectrum of the epitaxial structure of the LED device provided by the present invention.
[0070] In the figure: 1-substrate; 2-nitride nucleation layer; 3-unintentionally doped nitride layer; 4-n-type GaN layer; 41-polar surface; 42-non-polar surface; 5-nickel metal layer; 51-nickel nanoparticles; 6-multiple quantum well layer; 61-first region; 62-second region; 7-electron blocking layer; 8-p-type nitride layer. DETAILED DESCRIPTION
[0071] The technical solution of the present invention is further described below with reference to the accompanying drawings and through specific implementation methods.
[0072] It should be noted that in the description of the present invention, unless otherwise clearly specified and limited, the terms "disposed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood by specific circumstances.
[0073] The present invention provides an epitaxial structure of an LED device, the epitaxial structure comprising: a substrate, a buffer layer located on the substrate, an n-type GaN layer located on the buffer layer, a multi-quantum well layer located on the n-type GaN layer, an electron blocking layer located on the multi-quantum well layer, and a p-type nitride layer located on the electron blocking layer.
[0074] Further, the n-type GaN layer has a pit, the side wall of the pit is a non-polar plane, and the bottom plane of the pit and the peripheral plane of the pit are polar planes. The multi-quantum well layer includes an InGaN layer and a GaN layer that are periodically alternately arranged; the InGaN layer contains InGaN pits corresponding to the pits of the n-type GaN layer, and the InGaN layer includes a first region and a second region, the first region is the side wall of the InGaN pit; the second region is the bottom plane of the InGaN pit and the peripheral plane of the InGaN pit; the In content in the first region and the second region is different. Similarly, the GaN layer contains a GaN pit corresponding to the n-type GaN layer; the GaN layer includes a third region and a fourth region, the third region is the side wall of the GaN pit; the fourth region is the bottom plane of the GaN pit and the peripheral plane of the GaN pit. It can be understood that this embodiment does not specifically limit the division of the InGaN layer, and is not limited to the first region and the second region mentioned above. The InGaN layer can also be divided into three regions according to specific application needs, so as to subsequently emit three wavelengths of light.
[0075] As an example of this specific embodiment, the material of the substrate includes sapphire, silicon carbide or silicon, etc.; the thickness of the substrate is 350-750μm, for example, it can be 350μm, 360μm, 400μm, 450μm, 500μm, 600μm, 650μm, 700μm or 750μm, etc.
[0076] As an example of this specific embodiment, the buffer layer includes a nitride nucleation layer and an unintentionally doped nitride layer arranged in sequence, and the material of the nitride nucleation layer is Al a Ga b In 1-a-b N, 1≥a≥0, for example, it can be 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1 or 0; 1≥b≥0, for example, it can be 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1 or 0; 1≥1-ab≥0, for example, it can be 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1 or 0; for example, Al a Ga b In 1-a-b N includes any one of GaN, AlN, AlGaN, InN, InGaN, AlInGaN or AlInN or a combination of at least two thereof, wherein a typical but non-limiting combination is a combination of GaN and AlN, a combination of InGaN and AlN, a combination of GaN and AlInN, etc.; the thickness of the nitride nucleation layer is 80 to 120 nm, for example, 80 nm, 90 nm, 100 nm, 110 nm, 120 nm, etc. The nitride in the unintentionally doped nitride layer is Al c Ga d In 1-c-d N, 1≥c≥0, for example, it can be 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1 or 0; 1≥d≥0, for example, it can be 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1 or 0; 1≥1-cd≥0, for example, it can be 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1 or 0; for example, nitrogen The nitride layer includes any one of GaN, AlN, AlGaN, InN, InGaN, AlInGaN or AlInN, or a combination of at least two of them, wherein typical but non-limiting combinations are a combination of GaN and AlN, a combination of InGaN and AlN, a combination of GaN and AlInN, etc.; the thickness of the unintentionally doped nitride layer is 300 to 700 nm, for example, 300 nm, 400 nm, 500 nm, 600 nm or 700 nm, etc.
[0077] As an example of this specific embodiment, the metal nanoparticles are nickel nanoparticles; it can be understood that in other embodiments, other metals that can form nanoparticles after annealing treatment can also be used, and this embodiment is not limited to this.
[0078] As an example of this specific embodiment, the thickness of the n-type GaN layer is 2000-4000 nm. It can be understood that the thickness of the n-type GaN layer refers to the overall thickness.
[0079] As an example of this specific embodiment, the thickness of the InGaN layer in a single period in the multi-quantum well layer is 2 to 5 nm, for example, it can be 2 nm, 2.5 nm, 3 nm, 3.5 nm, 4 nm, 4.5 nm or 5 nm, etc. By controlling the thickness of a single InGaN layer within the above range, while ensuring the area of the non-polar InGaN surface grown on the side, it has the advantage of higher device luminescence efficiency, and avoids the space separation of the wave functions of electrons and holes in the quantum well caused by excessive thickness, the probability of radiation recombination is reduced, and the luminescence efficiency of the device is finally reduced; when the thickness of the InGaN layer is too thin, it will cause the quantum well to be unable to fully contain electrons and holes, and the electrons and holes overflow and recombine outside the quantum well, which reduces the luminescence intensity of the corresponding wavelength in the quantum well, and finally reduces the luminescence efficiency of the device.
[0080] As an example of this specific implementation, when the thickness of the GaN layer is too thick, it will cause electrons to concentrate on the n-type GaN side and holes to concentrate on the p-type GaN side, the recombination probability of electrons and holes will be reduced, and the luminous efficiency of the device will be reduced; when the thickness of the GaN layer is too thin, it will cause the electrons and holes to not be fully confined inside the InGaN quantum well, causing the electrons and holes to overflow and recombine outside the quantum well, reducing the luminous intensity of the corresponding wavelength in the quantum well, and finally reducing the luminous efficiency of the device. Based on this, this implementation sets the thickness of the GaN layer in a single period in the multi-quantum well layer to 1 to 3nm, for example, it can be 1nm, 1.5nm, 2nm, 2.5nm or 3nm, etc.; by controlling the thickness of the GaN layer in a single period within the above range, the luminous efficiency of the device is improved.
[0081] As an example of this specific implementation, when the thickness of the multi-quantum well layer is too thick or the number of periods is too many, it will cause electrons to concentrate on the n-type GaN side and holes to concentrate on the p-type GaN side, the recombination probability of electrons and holes will decrease, and the luminous efficiency of the device will decrease; when the thickness of the multi-quantum well layer is too thin or the number of periods is too small, the quantum well will not be able to fully contain electrons and holes, and the electrons and holes will overflow and recombine outside the quantum well, reducing the luminous intensity of the corresponding wavelength in the quantum well, and finally the luminous efficiency of the device will decrease. Based on this, the thickness of the multi-quantum well layer is 9 to 40nm, for example, it can be 9nm, 10nm, 12nm, 15nm, 20nm, 22nm, 25nm, 30nm, 35nm or 40nm. The number of alternating periods of InGaN layer and GaN layer in the multi-quantum well layer is 3 to 5; the number of periods and the total thickness in the multi-quantum well layer are controlled within the above range, which has the advantage of improving the luminous efficiency of the device.
[0082] As an example of this specific embodiment, the depth of the InGaN pit is 300 to 800 nm.
[0083] As an example of this specific embodiment, the ratio of the area of the first region to the area of the second region is (1:2) to (2:1).
[0084] As an example of this specific embodiment, the electron blocking layer includes a nitride electron blocking layer, and the material of the nitride electron blocking layer includes a group III nitride, for example, Al e Ga f In 1-e-f N, 1≥e≥0, for example, it can be 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1 or 0, etc.; 1≥f≥0, for example, it can be 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1 or 0, etc.; 1≥1-ef≥0, for example, it can be 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1 or 0, etc. For example, Al e Ga f In 1-e-f N includes any one of GaN, AlN, AlGaN, InN, InGaN, AlInGaN or AlInN, or a combination of at least two of them, wherein a typical but non-limiting combination is a combination of GaN and AlN, a combination of InGaN and AlN, a combination of GaN and AlInN, etc.; the thickness of the electron blocking layer is 5 to 15 nm, for example, 5 nm, 6 nm, 8 nm, 9 nm, 10 nm, 12 nm or 15 nm, etc. Similarly, the electron blocking layer includes pits corresponding to the pits of the n-type GaN layer.
[0085] As a specific example of this embodiment, the material of the p-type nitride layer includes group III nitride, for example, Al g Ga h In 1-g-h N, 1≥g≥0, for example, it can be 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1 or 0, etc.; 1≥h≥0, for example, it can be 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1 or 0, etc.; 1≥1-gh≥0, for example, it can be 1, 0.9, 0.8, 0.7, 0.6, 0.5, 0.4, 0.3, 0.2, 0.1 or 0, etc. For example, Al g Ga h In 1-g-h N includes any one of GaN, AlN, AlGaN, InN, InGaN, AlInGaN or AlInN, or a combination of at least two thereof, wherein a typical but non-limiting combination is a combination of GaN and AlN, a combination of InGaN and AlN, a combination of GaN and AlInN, etc. The thickness of the p-type nitride layer is 200 to 300 nm, for example, 200 nm, 210 nm, 220 nm, 230 nm, 250 nm, 280 nm or 300 nm, etc. Similarly, the p-type nitride layer includes pits corresponding to the pits of the n-type GaN layer.
[0086] The present invention provides a method for preparing an epitaxial structure of an LED device, the method comprising:
[0087] Step S1, providing a substrate.
[0088] Step S2, growing a buffer layer on the substrate.
[0089] The buffer layer includes a nitride nucleation layer and an unintentionally doped nitride layer stacked in sequence.
[0090] As an example of this specific embodiment, the nitride nucleation layer is an AlN layer, and its growth temperature is 1000-1200°C and the pressure is 100-150 mbar. During the growth of the nitride nucleation layer, the flow ratio of the aluminum source to the nitrogen source is (1-2): (10-30), for example, it can be 1:10, 1.5:10, 2:10, 1:15, 1:20, 1.5:18, 1:30, 1.2:30, 1.3:30 or 1.8:30, etc. The aluminum source can be TMAl, and the nitrogen source can be nitrogen.
[0091] As an example of this specific embodiment, the growth temperature of the unintentionally doped nitride layer is 950-1150°C, for example, it can be 950°C, 960°C, 970°C, 980°C, 1000°C, 1050°C, 1100°C or 1150°C; the growth pressure of the unintentionally doped nitride layer is 200-300 mbar, for example, it can be 200 mbar, 210 mbar, 220 mbar, 230 mbar, 240 mbar, 250 mbar, 260 mbar, 270 mbar, 280 mbar or 300 mbar. For example, when the material of the unintentionally doped nitride layer is GaN, during the growth of the GaN buffer layer, the flow ratio of the gallium source to the nitrogen source is (2-3):(300-400), for example, it can be 2:300, 2.5:300, 3:300, 2:400, 2.2:400, 2.5:400, 2.8:400, 3:375 or 3:400, etc.
[0092] Step S3, forming an n-type GaN layer containing pits on the buffer layer.
[0093] GaN is grown on the buffer layer to form a basic n-type GaN layer; a metal layer is grown on the basic n-type GaN layer, and after annealing, a device containing metal nanoparticles is obtained; the basic n-type GaN layer is etched using the metal nanoparticles as a mask, and the residual metal nanoparticles are removed to form an n-type GaN layer containing pits.
[0094] As an example of this specific embodiment, the growth temperature of the basic n-type GaN layer is 950-1150°C, for example, it can be 950°C, 960°C, 970°C, 980°C, 1000°C, 1050°C, 1100°C or 1150°C; the growth pressure of the basic n-type GaN layer is 200-300 mbar, for example, it can be 200 mbar, 210 mbar, 220 mbar, 230 mbar, 240 mbar, 250 mbar, 260 mbar, 270 mbar, 280 mbar or 300 mbar. Furthermore, the growth of the basic n-type GaN layer itself in the preparation method provided by the present invention is also very critical. It is preferred to control the temperature to 950-1150°C and the pressure to 200-300 mbar. At this time, the crystal quality of the n-type GaN layer is better. If the above process conditions are not adopted, when the temperature is too high, the decomposition rate of the n-type GaN layer increases, the growth rate decreases, and the growth cost increases; when the temperature is too low, the C impurity content inside the n-type GaN layer is high, which reduces the conductivity of the n-type GaN layer and affects the current distribution in the device and the luminescence characteristics of the device.
[0095] As a specific example of this embodiment, during the growth of the basic n-type GaN layer, a nitrogen source, a gallium source and a silicon source are introduced, and the flow rate of the nitrogen source can be 30000-40000sccm, for example, 30000sccm, 31000sccm, 32000sccm, 33000sccm, 34000sccm, 35000sccm, 36000sccm, 38000sccm or 40000sccm, etc.; the nitrogen source can be ammonia (NH3). The flow rate of the gallium source is 200-300sccm, for example, 200sccm, 210sccm, 230sccm, 250sccm, 280sccm or 300sccm, etc.; the gallium source can be TMGa. The flow rate of the silicon source is 10 to 30 sccm, for example, it can be 10 sccm, 11 sccm, 12 sccm, 13 sccm, 14 sccm, 15 sccm, 18 sccm, 19 sccm or 20 sccm, etc.; the silicon source can be SiH4 and / or Si2H6.
[0096] Furthermore, in step S3, the thickness of the metal layer is 20 to 80 nm. In this example or another example, the growth temperature of the metal layer is 80 to 120° C., and the vacuum degree is 10 -5 ~10 -6 Pa or less; the annealing temperature is 700 to 900°C, the annealing time is 5 to 40 min, and the flow rate of ammonia gas introduced during the annealing is 1000 to 2000 sccm.
[0097] Furthermore, the etching depth in step S3 is 300-800 nm.
[0098] Furthermore, the temperature for removing the residual metal nanoparticles is 40 to 60° C. and the time is 20 to 40 minutes.
[0099] As an example of this specific embodiment, since metals can be slowly dissolved in dilute nitric acid, dilute nitric acid can be used to remove metal nanoparticles, and the concentration of dilute nitric acid is 5-8wt%, for example, 5wt%, 6wt%, 7wt%, 7.5wt% or 8wt%, etc. There is no special restriction on the removal temperature, preferably 40-60°C, for example, 40°C, 42°C, 45°C, 50°C or 60°C, etc. There is no special restriction on the removal time, which is based on the complete removal of metal nanoparticles, for example, it can be 20-40min, for example, it can be 20min, 22min, 25min, 30min, 35min or 40min, etc.
[0100] As an example of this specific implementation, the process of etching the basic n-type GaN layer in step S3 includes inductively coupled plasma etching (ICP) or reactive ion etching (RIE), for example, the gas used by ICP can be chlorine and / or hydrogen chloride. The power of ICP is 800-1000W, the pressure is 2-5Pa, the self-bias voltage is 150-200V, and the etching depth is guaranteed to be 300-800nm.
[0101] Step S4, periodically growing an InGaN layer and a GaN layer on the n-type GaN layer to form a multi-quantum well layer.
[0102] The number of cycles of periodic alternating growth is 3 to 5; the temperature of multi-quantum well layer growth is 850 to 950° C., and the pressure is 300 to 500 mbar; the flow ratio of NH3:TMGa:TMIn for InGaN layer growth during multi-quantum well layer growth is (20000 to 40000):(200 to 300):(50 to 150).
[0103] Step S5, growing an electron blocking layer on the n-type GaN layer.
[0104] When the electron blocking layer (EBL) is made of AlGaN, its growth temperature may be 1000-1100° C., for example, 1000° C., 1020° C., 1050° C. or 1100° C.; the pressure may be 200-300 mbar, for example, 200 mbar, 210 mbar, 220 mbar, 230 mbar, 240 mbar, 250 mbar, 280 mbar, 290 mbar or 300 mbar.
[0105] Furthermore, during the growth of the electron blocking layer, the flow ratio of the aluminum source, the gallium source and the nitrogen source is (3-5):(10-20):(2000-3000), for example, it can be 3:10:2000, 3:15:2000, 3:20:2000, 4:10:2000, 5:10:2000, 3:10:3000, 3:15:3000, 3:15:2500, 4:10:2500 or 5:20:3000, etc., wherein the aluminum source can be TMAl, the gallium source can be TMGa, and the nitrogen source can be ammonia.
[0106] Step S6, growing a p-type nitride layer on the electron blocking layer.
[0107] When the material of the p-type nitride layer is GaN, its growth pressure can be 200-300 mbar, for example, it can be 200 mbar, 210 mbar, 220 mbar, 230 mbar, 240 mbar, 250 mbar, 280 mbar, 290 mbar or 300 mbar, etc.; the temperature can be 900-1100°C, for example, it can be 900°C, 920°C, 950°C, 1000°C, 1050°C or 1100°C, etc. In the growth process of the p-type nitride layer, the flow ratio of the magnesium source, the gallium source and the nitrogen source is (1-2): (20-30): (3000-4000), for example, it can be 1:20:3000, 1:25:3000, 1:30:3000, 1:24:3000, 1.5:20:3000, 1.5:25:3000, 1.5:30:3000, 2:25:3000, 2:20:4000, 2:30:3500, 2:20:4000 or 2:25:3500, etc., wherein the magnesium source can be bismuth magnesium, the gallium source can be TMGa, and the nitrogen source can be ammonia. As this specific example or another specific example, the growth carrier gas of the p-type nitride layer includes nitrogen.
[0108] Further, step S6 also includes activating the p-type nitride layer, the activation process includes maintaining the N2 and NH3 flow rates of the p-type nitride layer originally grown in the metal-organic chemical vapor deposition (MOCVD) equipment, lowering the temperature to room temperature, and activating the p-type GaN layer. Further, the pressure is maintained at 200-300 mbar during the activation process, for example, 200 mbar, 210 mbar, 220 mbar, 230 mbar, 240 mbar, 250 mbar, 280 mbar, 290 mbar or 300 mbar, etc.
[0109] See below Figures 1 to 10 , Figures 1 to 10 1 is a schematic diagram of the structure corresponding to each step in the method for preparing the epitaxial structure of the LED device provided by the present invention, and the preparation method comprises:
[0110] Step S1, providing a substrate 1.
[0111] Step S2, such as Figure 1 As shown, a substrate 1 is placed in a MOCVD device, the temperature is set to 1000-1200° C., the pressure is set to 100-150 mbar, and a nitride nucleation layer 2 with a thickness of 80-120 nm is grown on the substrate 1 .
[0112] Step S3, such as Figure 2As shown, the temperature in the MOCVD device is lowered to 950-1150° C., the pressure is adjusted to 200-300 mbar, and the unintentionally doped nitride layer 3 with a thickness of 300-700 nm is grown.
[0113] Step S4, such as Figure 3 As shown, hydrogen is introduced as a carrier gas, the temperature is adjusted to 950-1150° C., the pressure is adjusted to 200-300 mbar, and a basic n-type GaN layer 4 with a thickness of 2000-4000 nm is grown to obtain a device having a basic n-type GaN layer 4 grown thereon.
[0114] Step S5, such as Figure 4 As shown, the device with the basic n-type GaN layer 4 grown in step S4 is taken out from the MOCVD device and placed in an electron beam evaporation device, the temperature is set to 80-120°C, and the vacuum degree of the device is 10 -5 ~10 -6 Below Pa, the growth rate of the nickel metal layer 5 is 0.1-0.3 nm / s, and the nickel metal layer 5 with a thickness of 20-80 nm is grown.
[0115] Step S6, as Figure 5 As shown, the device obtained in step S5 is taken out from the electron beam evaporation equipment, put into an annealing furnace, 1000-2000sccm of NH3 is introduced as a carrier gas, the temperature is raised to 700-900°C, and an annealing treatment is performed for 5-40 minutes to obtain a device containing nickel nanoparticles 51.
[0116] Step S7, Figure 6 As shown, the device containing nickel nanoparticles 51 obtained in step S6 is taken out of the annealing furnace and placed in an ICP device. The power is set to 800-1000 W, the pressure is 2-5 Pa, the self-bias is 150-200 V, 30-50 sccm chlorine gas and 5-20 sccm argon gas are introduced, and the basic n-type GaN layer 4 is etched to a depth of 300-800 nm.
[0117] Step S8, Figure 7 As shown, the device obtained in step S7 is taken out from the ICP equipment, placed in 5-8wt% dilute nitric acid, and reacted at 40-60°C for 20-40 minutes to remove the residual nickel nanoparticles 51, thereby forming an n-type GaN layer 4 containing pits, wherein the side walls of the pits are non-polar surfaces 42, and the bottom plane of the pits and the peripheral plane of the pits are polar surfaces 41.
[0118] Step S9, as Figure 8As shown, the epitaxial wafer obtained in step S8 is put back into the MOCVD equipment, H2 is introduced as a carrier gas, the temperature is raised to 850-950°C, the pressure is adjusted to 300-500 mbar, TMGa, TMIn and NH3 are introduced, and 2-5 nm InGaN layers and 1-3 nm GaN layers are periodically grown to form a multi-quantum well layer 6.
[0119] The growth cycle of the multi-quantum well layer 6 is 3 to 5; when growing the InGaN layer, the gas flow rates are NH3 = 20000 to 40000 sccm, TMGa = 200 to 300 sccm, and TMIn = 50 to 150 sccm; when growing the GaN layer, the gas flow rates are NH3 = 20000 to 40000 sccm, and TMGa = 200 to 300 sccm.
[0120] Furthermore, the InGaN layer contains InGaN pits corresponding to the n-type GaN layer; the InGaN layer includes a first region 61 and a second region 62, the first region 61 is the side wall of the InGaN pit; the second region 62 is the bottom plane of the InGaN pit and the peripheral plane of the InGaN pit; the In content in the first region 61 and the second region 62 is different.
[0121] Step S10, as Fig. 9 As shown, H2 is introduced as a carrier gas, the temperature is raised to 1000-1100°C, the pressure is adjusted to 200-300 mbar, and an electron blocking layer 7 of 5-15 nm is grown.
[0122] Step S11, as Fig.10 As shown, N2 is introduced as a carrier gas, the temperature is adjusted to 900-1100°C, the pressure is 200-300 mbar, and a p-type nitride layer 8 with a thickness of 100-300 nm is grown; the flow rates of N2 carrier gas and NH3 in the MOCVD equipment are maintained, the pressure is adjusted to 260 mbar, the temperature is lowered to room temperature, and the p-type nitride layer 8 is activated.
[0123] The present invention also provides a semiconductor device, which includes the epitaxial structure in the above solution. The semiconductor device may be an LED lamp, and the first region and the second region in the InGaN layer of the epitaxial structure can emit light of two different wavelengths.
[0124] The technical solution of the present application will be described in more detail below in conjunction with the accompanying drawings and several embodiments, but it should be understood that the following embodiments are only for the purpose of explaining and illustrating the technical solution, but do not limit the scope of the present application. In addition, unless otherwise specified, the various raw materials, reaction equipment, detection equipment and methods used in the following embodiments are all known in the art.
[0125] Example 1
[0126] This embodiment provides an epitaxial structure of an LED device, such as Fig.10 As shown, the epitaxial structure includes: a substrate 1, a buffer layer (not marked in the figure) located on the substrate 1, an n-type GaN layer 4 located on the buffer layer, a multi-quantum well layer 6 located on the n-type GaN layer, an electron blocking layer 7 located on the multi-quantum well layer 6, and a p-type nitride layer 8 located on the electron blocking layer 7.
[0127] Further, the buffer layer includes a nitride nucleation layer 2 and an unintentionally doped nitride layer 3 stacked in sequence. The n-type GaN layer has a pit, the sidewall of the pit is a non-polar plane 42, and the bottom plane of the pit and the peripheral plane of the pit are polar planes 41. The multi-quantum well layer 6 includes an InGaN layer and a GaN layer that are periodically alternately arranged; the InGaN layer contains InGaN pits corresponding to the pits of the n-type GaN layer; the InGaN layer includes a first region 61 and a second region 62, the first region is the sidewall of the InGaN pit, the second region 62 is the bottom plane of the InGaN pit and the peripheral plane of the InGaN pit, and the In content in the first region 61 and the second region 62 is different.
[0128] The method for preparing the epitaxial structure of the LED device in this embodiment comprises the following steps:
[0129] Step S1, providing a sapphire substrate.
[0130] Step S2, placing the sapphire substrate into the MOCVD equipment, setting the temperature to 1100°C, the pressure to 130 mbar, introducing hydrogen as a carrier gas, introducing 100 sccm of TMAl and 1000 sccm of NH3, and growing a nitride nucleation layer with a thickness of 100 nm and made of AlN on the sapphire substrate.
[0131] Step S3, introducing hydrogen as a carrier gas, cooling to 1050°C, adjusting the pressure to 260 mbar, introducing 240 sccm of TMGa and 30,000 sccm of NH3, growing a GaN layer with a thickness of 500 nm, and forming an unintentionally doped nitride layer.
[0132] Step S4, introducing hydrogen as a carrier gas, adjusting the temperature to 1050°C and the pressure to 260 mbar, introducing 30000 sccm of NH3, 240 sccm of TMGa and 10 sccm of SiH4, growing a basic n-type GaN layer with a thickness of 2500 nm, and obtaining a device having a basic n-type GaN layer grown thereon.
[0133] Step S5, taking out the device with the basic n-type GaN layer grown in step S4 from the MOCVD device, placing it in an electron beam evaporation device, setting the temperature to 100°C and the vacuum degree of the device to 10 -5Below Pa, the growth rate of the nickel metal layer is 0.05 nm / s, and a nickel metal layer with a thickness of 40 nm is grown.
[0134] Step S6, taking the device obtained in step S5 out of the electron beam evaporation equipment, putting it into an annealing furnace, introducing 1000 sccm of NH3 as a carrier gas, raising the temperature to 800°C, and performing annealing treatment for 30 minutes to obtain a device containing nickel nanoparticles.
[0135] Step S7, take out the nickel nanoparticle-containing device obtained in step S6 from the annealing furnace, put it into the ICP equipment, set the power to 900 W, the pressure to 2 Pa, the self-bias to 200 V, pass 40 sccm chlorine gas and 10 sccm argon gas, and etch the basic n-type GaN layer to a depth of 500 nm.
[0136] Step S8, taking out the device obtained in step S7 from the ICP equipment, placing it in 5wt% dilute nitric acid, and reacting it at 50°C for 30 minutes to remove the residual nickel nanoparticles and generate an n-type GaN layer containing pits, wherein the side walls of the pits are non-polar surfaces, and the bottom plane of the pits and the surrounding plane of the pits are polar surfaces.
[0137] Step S9, placing the device obtained in step S8 into the MOCVD equipment, introducing H2 as the carrier gas, raising the temperature to 820°C, adjusting the pressure to 400mbar, introducing TMGa, TMIn and NH3, periodically growing a 3nm InGaN layer and a 2nm GaN layer to form a multi-quantum well layer.
[0138] The growth cycle of the multi-quantum well layer can be 3; when growing the InGaN layer, the gas flow rates are NH3=30000sccm, TMGa=240sccm, TMIn=100sccm; when growing the GaN layer, the gas flow rates are NH3=30000sccm, TMGa=240sccm.
[0139] Furthermore, the InGaN layer contains InGaN pits corresponding to the pits of the n-type GaN layer; the InGaN layer includes a first region and a second region, the first region is the side wall of the InGaN pit; the second region is the bottom plane of the InGaN pit and the peripheral plane of the InGaN pit; the In content in the first region and the second region is different.
[0140] Step S10, introduce H2 as a carrier gas, raise the temperature to 1050°C, adjust the pressure to 260mbar, introduce 30sccm of TMAl, 100sccm of TMGa and 30000sccm of NH3, and grow 10nm AlGaN as an electron blocking layer.
[0141] Step S11, introduce N2 as a carrier gas, adjust the temperature to 1000°C and the pressure to 260 mbar, introduce 240 sccm of TMGa, 30000 sccm of NH3 and 10 sccm of Cp2Mg, and grow a GaN layer with a thickness of 200 nm as a p-type nitride layer; maintain the flow rate of N2 carrier gas and NH3 in the MOCVD equipment, adjust the pressure to 260 mbar, and reduce the temperature to room temperature to activate the p-type GaN layer.
[0142] The luminescence spectrum of the epitaxial structure of the LED device prepared by the solution provided in this embodiment is as follows: Fig.11 As shown, from Fig.11 It can be seen that the epitaxial structure of the present embodiment can simultaneously emit light of about 440nm and 510nm, thereby being able to emit white light in a superimposed manner; and when the epitaxial structure of the present embodiment extracts light, there is no problem of short-wavelength light passing through the long-wavelength active layer and being absorbed, which can improve the light extraction efficiency of the device. As shown in Table 2, the brightness can reach 210mW, and the wavelength uniformity is good, the uniformity of the 440nm wavelength is 1.0nm, the uniformity of the 510nm wavelength is 2.0nm, and the light extraction efficiency is 22.1%.
[0143] The preparation method of the epitaxial structure provided in this embodiment can adjust the difference in In component content between the first region and the second region in the InGaN layer in the multi-quantum well, so as to better adjust the wavelength difference between the emission wavelengths and emit light of the desired wavelength; and the growth of different In components can be achieved under the same growth conditions, avoiding the problem of degradation of the quantum well structure corresponding to the long-wavelength light due to different growth conditions in the existing scheme, which helps to improve the performance of the device.
[0144] Example 2
[0145] This embodiment provides an epitaxial structure of an LED device, and a preparation method thereof includes the following steps:
[0146] Step S1, providing a sapphire substrate.
[0147] Step S2, placing the sapphire substrate into the MOCVD equipment, setting the temperature to 1000°C, the pressure to 100 mbar, introducing hydrogen as a carrier gas, introducing 80 sccm of TMAl and 800 sccm of NH3, and growing a nitride nucleation layer with a thickness of 80 nm and made of AlN on the sapphire substrate.
[0148] Step S3, introducing hydrogen as a carrier gas, cooling to 950°C, adjusting the pressure to 200 mbar, introducing 200 sccm of TMGa and 20,000 sccm of NH3, growing a GaN layer with a thickness of 700 nm, and forming an unintentionally doped nitride layer.
[0149] Step S4, introducing hydrogen as a carrier gas, adjusting the temperature to 950°C and the pressure to 300 mbar, introducing 20000 sccm of NH3, 200 sccm of TMGa and 30 sccm of SiH4, growing a basic n-type GaN layer with a thickness of 4000 nm, and obtaining a device having a basic n-type GaN layer grown thereon.
[0150] Step S5, taking out the device with the basic n-type GaN layer grown in step S4 from the MOCVD device, placing it in an electron beam evaporation device, setting the temperature to 120°C and the vacuum degree of the device to 10 -5 Below Pa, the growth rate of the nickel metal layer is 0.3 nm / s, and a nickel metal layer with a thickness of 20 nm is grown.
[0151] Step S6, taking the device obtained in step S5 out of the electron beam evaporation equipment, putting it into an annealing furnace, introducing 1000 sccm of NH3 as a carrier gas, raising the temperature to 900°C, and performing annealing treatment for 5 minutes to obtain a device containing nickel nanoparticles.
[0152] Step S7, take out the nickel nanoparticle-containing device obtained in step S6 from the annealing furnace, put it into the ICP equipment, set the power to 1000 W, the pressure to 2 Pa, the self-bias to 200 V, pass 30 sccm HCl and 20 sccm argon, and etch the basic n-type GaN layer to a depth of 300 nm.
[0153] Step S8, taking out the device obtained in step S7 from the ICP equipment, placing it in 8wt% dilute nitric acid, reacting it at 40°C for 40 minutes, removing the residual nickel nanoparticles, and generating an n-type GaN layer containing pits, wherein the side walls of the pits are non-polar surfaces, and the bottom plane of the pits and the surrounding plane of the pits are polar surfaces.
[0154] Step S9, placing the device obtained in step S8 into the MOCVD equipment, introducing H2 as the carrier gas, raising the temperature to 850°C, adjusting the pressure to 500mbar, introducing TMGa, TMIn and NH3, periodically growing a 5nm InGaN layer and a 1nm GaN layer to form a multi-quantum well layer.
[0155] The growth cycle of the multi-quantum well layer can be 3; when growing the InGaN layer, the gas flow rates are NH3=20000sccm, TMGa=300sccm, TMIn=50sccm; when growing the GaN layer, the gas flow rates are NH3=40000sccm, TMGa=200sccm.
[0156] Furthermore, the InGaN layer contains InGaN pits corresponding to the pits of the n-type GaN layer; the InGaN layer includes a first region and a second region, the first region is the side wall of the InGaN pit; the second region is the bottom plane of the InGaN pit and the peripheral plane of the InGaN pit; the In content in the first region and the second region is different.
[0157] Step S10, introducing H2 as a carrier gas, raising the temperature to 1100°C, adjusting the pressure to 200 mbar, introducing 40 sccm of TMAl, 50 sccm of TMGa and 40000 sccm of NH3, and growing 15 nm of AlGaN as an electron blocking layer.
[0158] Step S11, introduce N2 as a carrier gas, adjust the temperature to 900°C and the pressure to 300 mbar, introduce 200 sccm of TMGa, 40000 sccm of NH3 and 20 sccm of Cp2Mg, and grow a GaN layer with a thickness of 300 nm as a p-type nitride layer; maintain the flow rate of N2 carrier gas and NH3 in the MOCVD equipment, adjust the pressure to 260 mbar, and reduce the temperature to room temperature to activate the p-type GaN layer.
[0159] The epitaxial structure prepared by the scheme provided in this embodiment can simultaneously emit light of about 430nm and 500nm, thereby being able to emit white light in a superimposed manner; and when the epitaxial structure in this embodiment extracts light, there is no problem of short-wavelength light passing through the long-wavelength active layer and being absorbed, which can improve the light extraction efficiency of the device. As shown in Table 2, the brightness can reach 205mW, and the wavelength uniformity is good, the uniformity of the 430nm wavelength is 1.1nm, the uniformity of the 500nm wavelength is 2.1nm, and the light extraction efficiency is 20.7%.
[0160] The preparation method of the epitaxial structure provided in this embodiment can adjust the difference in In component content between the first region and the second region in the InGaN layer in the multi-quantum well, so as to better adjust the wavelength difference between the emission wavelengths and emit light of the desired wavelength; and the growth of different In components can be achieved under the same growth conditions, avoiding the problem of degradation of the quantum well structure corresponding to the long-wavelength light due to different growth conditions in the existing scheme, which helps to improve the performance of the device.
[0161] Example 3
[0162] This embodiment provides an epitaxial structure of an LED device, and a preparation method thereof includes the following steps:
[0163] Step S1, providing a sapphire substrate.
[0164] Step S2, placing the sapphire substrate into the MOCVD equipment, setting the temperature to 1200°C, the pressure to 150 mbar, introducing hydrogen as a carrier gas, introducing 120 sccm of TMAl and 1200 sccm of NH3, and growing a nitride nucleation layer with a thickness of 120 nm and made of AlN on the substrate.
[0165] Step S3, introducing hydrogen as a carrier gas, cooling to 1150°C, adjusting the pressure to 300 mbar, introducing 300 sccm of TMGa and 40000 sccm of NH3, growing a GaN layer with a thickness of 300 nm, and forming an unintentionally doped nitride layer.
[0166] Step S4, introducing hydrogen as a carrier gas, adjusting the temperature to 1150°C, the pressure to 200 mbar, introducing 40000 sccm of NH3, 300 sccm of TMGa and 10 sccm of SiH4, growing a basic n-type GaN layer with a thickness of 2000 nm, and obtaining a device having a basic n-type GaN layer grown thereon.
[0167] Step S5, taking out the device with the basic n-type GaN layer grown in step S4 from the MOCVD device, placing it in an electron beam evaporation device, setting the temperature to 80°C and the vacuum degree of the device to 10 -6 Below Pa, the growth rate of the nickel metal layer is 0.1 nm / s, and a nickel metal layer with a thickness of 80 nm is grown.
[0168] Step S6, taking the device obtained in step S5 out of the electron beam evaporation equipment, putting it into an annealing furnace, introducing 2000 sccm of NH3 as a carrier gas, raising the temperature to 700°C, and performing annealing treatment for 40 minutes to obtain a device containing nickel nanoparticles.
[0169] Step S7, take out the nickel nanoparticle-containing device obtained in step S6 from the annealing furnace, put it into the ICP equipment, set the power to 800 W, the pressure to 5 Pa, the self-bias to 150 V, pass 50 sccm chlorine gas and 5 sccm argon gas, and etch the basic n-type GaN layer to a depth of 800 nm.
[0170] Step S8, taking out the device obtained in step S7 from the ICP equipment, placing it in 5wt% dilute nitric acid, and reacting it at 60°C for 20 minutes to remove the residual nickel nanoparticles and generate an n-type GaN layer containing pits, wherein the side walls of the pits are non-polar surfaces, and the bottom plane of the pits and the surrounding plane of the pits are polar surfaces.
[0171] Step S9, placing the device obtained in step S8 into the MOCVD equipment, introducing H2 as the carrier gas, raising the temperature to 800°C, adjusting the pressure to 300 mbar, introducing TMGa, TMIn and NH3, periodically growing a 2nm InGaN layer and a 3nm GaN layer to form a multi-quantum well layer.
[0172] The growth cycle of the multi-quantum well layer can be 5; when growing the InGaN layer, the gas flow rates are NH3=40000sccm, TMGa=200sccm, TMIn=150sccm; when growing the GaN layer, the gas flow rates are NH3=20000sccm, TMGa=300sccm.
[0173] Furthermore, the InGaN layer contains InGaN pits corresponding to the pits in the n-type GaN layer; the InGaN layer includes a first region and a second region, the first region is the side wall of the InGaN pit; the second region is the bottom plane of the InGaN pit and the peripheral plane of the InGaN pit; the In content in the first region and the second region is different.
[0174] Step S10, introducing H2 as a carrier gas, raising the temperature to 1000°C, adjusting the pressure to 300 mbar, introducing 20 sccm of TMAl, 200 sccm of TMGa and 20000 sccm of NH3, and growing 5 nm of AlGaN as an electron blocking layer.
[0175] Step S11, introduce N2 as a carrier gas, adjust the temperature to 1100°C and the pressure to 200 mbar, introduce 300 sccm of TMGa, 20000 sccm of NH3 and 5 sccm of Cp2Mg, and grow a GaN layer with a thickness of 100 nm as a p-type nitride layer; maintain the flow rate of N2 carrier gas and NH3 in the MOCVD equipment, adjust the pressure to 270 mbar, and reduce the temperature to room temperature to activate the p-type GaN layer.
[0176] The epitaxial structure prepared by the solution provided in this embodiment can simultaneously emit light of about 445nm and 520nm, so that white light can be emitted in a superimposed manner; and when the epitaxial structure in this embodiment extracts light, there is no problem of short-wavelength light passing through the long-wavelength active layer and being absorbed, which can improve the light extraction efficiency of the device. As shown in Table 2, the brightness can reach 200mW, and the wavelength uniformity is good, the uniformity of the 445nm wavelength is 1.2nm, the uniformity of the 520nm wavelength is 2.0nm, and the light extraction efficiency is 19.5%.
[0177] The preparation method of the epitaxial structure provided in this embodiment can adjust the difference in In component content between the first region and the second region in the InGaN layer in the multi-quantum well, so as to better adjust the wavelength difference between the emission wavelengths and emit light of the desired wavelength; and the growth of different In components can be achieved under the same growth conditions, avoiding the problem of degradation of the quantum well structure corresponding to the long-wavelength light due to different growth conditions in the existing scheme, which helps to improve the performance of the device.
[0178] Example 4
[0179] This embodiment provides an epitaxial structure of an LED device. In the preparation method of the epitaxial structure, except that the growth thickness of the nickel metal layer in step S5 is 100 nm, the rest is the same as that of embodiment 1, and will not be repeated here.
[0180] In this embodiment, the growth thickness of the nickel metal layer is too thick, resulting in the subsequent nickel nanoparticles having a diameter that is too large and the particle size distribution of the nickel nanoparticles is uneven. As shown in Table 1, the D10 of the nickel nanoparticles is 460nm and the D90 is 835nm, the uniformity of the particle size distribution decreases, and the surface roughness reaches 1.6nm, which leads to a decrease in the uniformity of the subsequent emitted light. The uniformity of the 440nm wavelength is 2.2nm, the uniformity of the 510nm wavelength is 3.0nm, and the brightness is reduced to 170mW compared to Example 1.
[0181] Example 5
[0182] This embodiment provides an epitaxial structure of an LED device. In the preparation method of the epitaxial structure, except that the growth thickness of the nickel metal layer in step S5 is 10 nm, the rest is the same as that of embodiment 1, and will not be repeated here.
[0183] In this embodiment, the growth thickness of the nickel metal layer is relatively thin, resulting in the subsequent nickel nanoparticles having a diameter that is too small. As shown in Table 1, the particle size distribution of the nickel nanoparticles is D10=290nm and D90=425nm, and the masking effect is relatively poor, resulting in uneven intensity distribution of the subsequent two wavelengths of light. The intensity ratio of the light with a wavelength of 440nm to that of the light with a wavelength of 510nm is 1.4:1, resulting in the final brightness being reduced to 174mW compared to Example 1.
[0184] It can be seen from Example 1 and Examples 4 to 5 that the present invention, by controlling the thickness of the nickel metal layer within a specific range, is more conducive to the subsequent acquisition of nickel nanoparticles with uniform particle size distribution and sizes within the expected range, and is more conducive to the subsequent use of mask selective etching to produce uniformly distributed two different wavelengths of light.
[0185] Example 6
[0186] This embodiment provides an epitaxial structure of an LED device. In the preparation method of the epitaxial structure, except that the temperature in step S5 is set to 150° C. and the growth rate of the nickel metal layer is set to 0.5 nm / s, the rest is the same as that in embodiment 1 and will not be repeated here.
[0187] In this embodiment, the growth rate of the nickel metal layer is too fast, resulting in uneven thickness distribution of the nickel metal layer during growth. The surface roughness of the nickel metal layer is as high as 2.5nm, resulting in the uniformity of the two different wavelengths of light being as high as 2.5nm and 3.2nm respectively, and the brightness is reduced to 165mW compared to Example 1. This shows that the present invention is more conducive to obtaining a nickel metal layer with lower surface roughness by controlling the growth rate of the nickel-gold layer within a specific range, and is more conducive to improving the light extraction efficiency of the device and adjusting the uniformity of the two different wavelengths of light.
[0188] Example 7
[0189] This embodiment provides an epitaxial structure of an LED device. In the preparation method of the epitaxial structure, except that the annealing temperature in step S6 is 1000° C., the rest is the same as that of embodiment 1 and will not be described again.
[0190] Compared with Example 1, the annealing temperature in this example is higher, resulting in a larger number of nickel nanoparticles formed in the first stage with smaller particle size. The final nickel nanoparticles have a relatively small particle size, and it is more difficult to control the light intensity of two different wavelengths, and the final brightness drops to 165mW.
[0191] Example 8
[0192] This embodiment provides an epitaxial structure of an LED device. In the preparation method of the epitaxial structure, except that the annealing temperature in step S6 is 500° C., the rest is the same as that of embodiment 1 and will not be described again.
[0193] Compared with Example 1, the annealing temperature in this example is lower, resulting in a smaller number of nickel nanoparticles formed in the first stage and a larger particle size. The final nickel nanoparticles have a particle size of up to 1500nm, an increased span of particle size distribution, and it is more difficult to control the light intensity of two different wavelengths and the emission is uneven, and the final brightness drops to 155mW.
[0194] It can be seen from Example 1 and Examples 7 to 8 that the present invention can better control the particle size of nickel nanoparticles by controlling the annealing temperature, thereby making the light intensity and uniformity of two different wavelengths more controllable.
[0195] Example 9
[0196] This embodiment provides an epitaxial structure of an LED device. In the preparation method of the epitaxial structure, except that the flow rate of ammonia gas in the annealing treatment in step S6 is 3500 sccm, the rest is the same as that of embodiment 1, which will not be repeated here.
[0197] It can be seen from Example 1 and Example 9 that the flow rate of ammonia in Example 9 is too large, and the formation rate of nickel nanoparticles increases, resulting in an increase in the particle size span of the formed nickel nanoparticles compared to Example 1, and a decrease in the uniformity of the two different wavelengths of light. As shown in Table 2, the brightness of the final device drops to 158mW.
[0198] Example 10
[0199] This embodiment provides an epitaxial structure of an LED device. In the preparation method of the epitaxial structure, except that the etching depth in step S6 is 200 nm, the rest is the same as that of embodiment 1, and will not be described again.
[0200] In this embodiment, the etching depth is relatively shallow, resulting in an area ratio of the first region to the second region of 1.7:1, which ultimately results in an intensity ratio of two different wavelengths of light of 1.5:1, and the final brightness drops to 170 mW.
[0201] Embodiment 11
[0202] This embodiment provides an epitaxial structure of an LED device. In the preparation method of the epitaxial structure, except that the etching depth in step S7 is 1000 nm, the rest is the same as that of embodiment 1, and will not be described again.
[0203] In this embodiment, the etching depth is deep, resulting in an area ratio of the first region to the second region of 1:1.5, and ultimately resulting in an intensity ratio of two different wavelengths of light of 1:1.8, which reduces the controllability of light intensity at different wavelengths.
[0204] Example 12
[0205] This embodiment provides an epitaxial structure of an LED device. In the preparation method of the epitaxial structure, except that the flow ratio of NH3:TMGa:TMIn for growing the InGaN layer in step S9 is 30000:240:20, the rest is the same as that in embodiment 1 and will not be repeated here.
[0206] Compared with Example 1, the TMIn flow rate in this embodiment is only 20 sccm, resulting in a small difference in the content of the In component in the first region and the second region. The absolute value of the difference in the content of the In component between the first region and the second region is only 6%, and the wavelength difference between the two different wavelengths of light finally emitted is small. It is difficult to emit white light after the two are superimposed and combined.
[0207] Example 13
[0208] This embodiment provides an epitaxial structure of an LED device. In the preparation method of the epitaxial structure, except that the flow ratio of NH3:TMGa:TMIn for growing the InGaN layer in step S9 is 30000:240:200, the rest is the same as that in embodiment 1 and will not be repeated here.
[0209] Compared with Example 1, the TMIn flow rate in this embodiment is as high as 200 sccm, but the difference in the content of the In component in the first region and the second region is not much different from that in Example 1, and the absolute value of the difference in the indium component content is 11%. However, the excessive TMIn flow rate leads to waste of raw materials.
[0210] Comparative Example 1
[0211] This comparative example provides an epitaxial structure. In the preparation method of the epitaxial structure, except that steps S5 to S8 are not performed, the rest are the same as those in Example 1, and will not be described again.
[0212] In this comparative example, since steps S5 to S8 are not performed, no pits are generated in the final epitaxial structure, and it is impossible to emit light of two different wavelengths, and the brightness is only 150 mW.
[0213] In one embodiment, the above-mentioned embodiments and comparative examples can be tested to prove the effectiveness and rationality of the scheme provided by the present invention. Specifically, the test method is: the roughness of the surface of the nickel metal layer is tested by an atomic force microscope method; the particle size distribution of the nanoparticles is tested by a scanning electron microscope; the In component content in the single-layer InGaN in the first region and the second region is tested by a photoluminescence method; the luminous wavelength WLD and the wavelength uniformity std are tested on the epitaxial wafer by photoluminescence, and a 150μm*150μm chip is prepared on the epitaxial wafer by a chip preparation process, and the brightness of the chip is tested. The generated test data are shown in Tables 1 to 2.
[0214] Table 1
[0215]
[0216]
[0217] Table 2
[0218]
[0219] “ / ” in Tables 1 and 2 indicates no relevant data.
[0220] It can be seen from Examples 1 to 3 that the epitaxial structure and preparation method thereof provided by the present invention can realize a design with different In component contents in a single InGaN layer, and can simultaneously emit light of two wavelengths, wherein the luminous intensity ratio of the non-polar plane to the polar plane can be effectively regulated between 0.5 and 2.1, and there is no problem of short-wavelength light passing through the long-wavelength active layer and being absorbed, and the light extraction efficiency of the device can be improved, with the light extraction efficiency being above 19.0%, and the brightness of a chip of 150μm*150μm reaching above 200mW.
[0221] The present invention illustrates the detailed structural features of the present invention through the above embodiments, but the present invention is not limited to the above detailed structural features, that is, it does not mean that the present invention must rely on the above detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing an epitaxial structure of an LED device, characterized in that: The preparation method comprises: providing a substrate; Setting the temperature to 1000-1200° C. and the pressure to 100-150 mbar, growing a nitride nucleation layer with a thickness of 80-120 nm on the substrate; The temperature is lowered to 950-1150° C., the pressure is adjusted to 200-300 mbar, and an unintentionally doped nitride layer having a thickness of 300-700 nm is grown on the nitride nucleation layer; Hydrogen is introduced as a carrier gas, the temperature is adjusted to 950-1150° C., the pressure is adjusted to 200-300 mbar, a nitrogen source with a flow rate of 30000-40000 sccm, a gallium source with a flow rate of 200-300 sccm, and a silicon source with a flow rate of 10-30 sccm are introduced, and GaN is grown on the unintentionally doped nitride layer to form a basic n-type GaN layer with a thickness of 2000-4000 nm; Set the temperature to 80~120℃ and the vacuum degree to 10 -5 ~10 -6 Below Pa, growing a metal layer with a thickness of 20-80 nm and a surface roughness of ≤2 nm on the basic n-type GaN layer; NH3 with a flow rate of 1000-2000 sccm is introduced as a carrier gas, the temperature is raised to 700-900° C., and the metal layer is annealed for 5-40 minutes to obtain metal nanoparticles with a particle size range of 300-800 nm; The power of the inductively coupled plasma etching is set to 800-1000 W, the pressure is set to 2-5 Pa, the self-bias voltage is set to 150-200 V, the chlorine gas with a flow rate of 30-50 sccm and the argon gas with a flow rate of 5-20 sccm are introduced, the metal nanoparticles are used as a mask, the basic n-type GaN layer is etched, and the residual metal nanoparticles are removed to form an n-type GaN layer containing pits with a depth of 300-800 nm; An InGaN layer and a GaN layer are periodically grown on the n-type GaN layer to form a multi-quantum well layer; the InGaN layer contains an InGaN pit corresponding to the pit of the n-type GaN layer; the InGaN layer includes a first region and a second region, the first region is a side wall of the InGaN pit; the second region is a bottom plane of the InGaN pit and a peripheral plane of the InGaN pit; the absolute value of the difference in In content between the first region and the second region is 5% to 10%; An electron blocking layer and a p-type nitride layer are sequentially grown on the n-type GaN layer.
2. The preparation method according to claim 1, characterized in that: The sidewall of the pit is a non-polar surface, and the bottom plane of the pit and the peripheral plane of the pit are polar surfaces.
3. The preparation method according to claim 1, characterized in that: The metal layer is a nickel metal layer.
4. The preparation method according to claim 1, characterized in that: The growth temperature of the multi-quantum well layer is 850-950° C. and the pressure is 300-500 mbar.
5. The preparation method according to claim 1, characterized in that: During the growth of the InGaN layer of the multi-quantum well layer, the flow ratio of NH3:TMGa:TMIn is (20000-40000):(200-300):(50-150).
6. An epitaxial structure of an LED device, characterized in that: The epitaxial structure is prepared by the preparation method according to any one of claims 1 to 5, comprising: substrate; a buffer layer located on the substrate; an n-type GaN layer located on the buffer layer and containing pits; A multi-quantum well layer located on the n-type GaN layer; the multi-quantum well layer comprises an InGaN layer and a GaN layer that are periodically and alternately arranged; the InGaN layer comprises an InGaN pit corresponding to the pit of the n-type GaN layer; the InGaN layer comprises a first region and a second region, the first region being a side wall of the InGaN pit; the second region being a bottom plane of the InGaN pit and a peripheral plane of the InGaN pit; the In content in the first region and the second region is different; an electron blocking layer located on the multi-quantum well layer; A p-type nitride layer is located on the electron blocking layer.
7. The epitaxial structure according to claim 6, characterized in that: The depth of the InGaN pit is 300-800nm.
8. The epitaxial structure according to claim 6, characterized in that: The area ratio of the first region to the second region is (1:2) to (2:1).
9. A semiconductor device, characterized in that: An epitaxial structure comprising the LED device according to any one of claims 6 to 8.