Compositions comprising graphene-based materials as lubricant additives
The nanoparticle composition prepared by grinding contains multi-layer graphene, polymer and silane compound, which solves the problem of unstable dispersion of graphene nanoparticles in lubricating oil and achieves long-term stable dispersion and improvement of anti-friction performance. Suitable for industrial applications of lubricants.
Patent Information
- Application Number
- CN202180063793.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-08-11
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2041-08-11
AI Technical Summary
The dispersion of existing graphene nanoparticles in lubricating oil is unstable, causing frictional performance to decrease over a long period of time, and is incompatible with other packaging components, affecting the overall performance of the lubricant.
A nanoparticle composition prepared by a grinding method, including a multilayer graphene-based material, a polyalkyl (meth)acrylate polymer, a silane compound and a base fluid, and the dispersion and stability of the graphene nanoparticles are improved through a ball milling process properties to avoid agglomeration and settling.
It achieves long-term stable dispersion of graphene nanoparticles in lubricating oil, significantly improves anti-friction performance, and is well compatible with other components, improving the industrial application value of lubricants.
Smart Images

Figure BDA0004130585100000081 
Figure BDA0004130585100000082 
Figure BDA0004130585100000083
Abstract
Description
Technical Field
[0001] The present invention relates to nanoparticle compositions comprising graphene-based materials and methods for preparing the same. The present invention also relates to their use as lubricant additives for improving tribological properties, in particular for improving anti-friction properties on metal parts, and to lubricant compositions comprising these nanoparticle compositions. Background Art
[0002] The present invention relates to the field of lubrication. Lubricants are compositions that reduce friction between surfaces. In addition to allowing freedom of movement between two surfaces and reducing mechanical wear of the surfaces, lubricants can also inhibit corrosion of the surfaces and / or can inhibit damage to the surfaces due to heat or oxidation. Examples of lubricant compositions include, but are not limited to, engine oils, transmission fluids, gear oils, industrial lubricants, greases, and metalworking oils.
[0003] Lubricants typically contain a base fluid and variable amounts of additives. Some additives in lubricant formulations are used to reduce friction and wear between contacting parts, which is important for the energy efficiency and durability of the device being lubricated.
[0004] In recent years, there has been a growing interest in the use of graphene nanoparticles as self-lubricating solids or as additives in lubricant formulations. Studies have shown that the addition of graphene nanoparticles can greatly improve wear and friction performance, and this is attributed to their easy shearing ability on atomically smooth surfaces, extremely high strength and chemical inertness (Sumant et al., Mater. Today 17(1), pp. 31 et seq. (2014)).
[0005] However, constructing stable dispersions of graphene nanoparticles is problematic. Due to their hydrophilic nature, they form poor dispersions in oil or non-polar environments. Additionally, the poor dispersibility of the particles and the weak forces that attract the particles together lead to agglomeration and particle aggregates. These aggregates will lead to sedimentation, which is undesirable and ineffective for any lubricant formulation.
[0006] In order to prevent this sedimentation and enhance dispersibility, various techniques have been adopted, such as surface modification or the use of dispersants. The surface modification is completed by reacting some surface groups of the particles with small molecules or polymers suitable for non-polar fluids. However, compared with graphene, a large amount of small molecules are usually required, which is disadvantageous in terms of packaging compatibility. In addition, the dispersion is susceptible to environmental influences and is therefore unstable. This is because this method only covers a part of the particle surface, and there is still a considerable amount of hydrophilic properties, resulting in agglomeration.
[0007] For example, CN108102763A describes a two-step surface modification procedure for the preparation of serpentine / functionalized graphene lubricant additives. In the first step, they use an aminosilane coupling agent to obtain functionalized graphene oxide. In the second step, via a thermal reaction with magnesium silicate, a composite material as a lubricant additive is obtained. They claim excellent dispersibility, stability and processing performance. However, the final additive concentration in the lubricant is only 0.01 wt% to 0.5 wt% and there is no long-term data.
[0008] CN107758652A relates to the surface modification of graphene by polymers via imide, amide or ester groups to improve dispersion stability. These stabilizers mainly provide coordination bonding and also only provide one coordination site to the nanoparticles. This is still a disadvantage in terms of stability and process performance, as this method only covers a portion of the particle surface and there is still a considerable amount of hydrophilicity, which leads to agglomeration.
[0009] CN107384520A discloses a graphene-containing lubricating oil, which comprises a lubricating oil base oil, glyceryl tristearate, polymethacrylate, polyisobutylene, octylphenol, a fluorine surfactant, a silane coupling agent, a diisocyanate and graphene oxide powder.
[0010] US2013324447A1 uses block copolymers with alkenylbenzene blocks and linear alpha olefin blocks to stabilize carbon nanomaterials in lubricating oils. The resulting dispersion is obtained via shear mixing (ultra-turrax) and shows improved tribological properties compared to pure base oils. However, as shown by transmission measurements, the stability drops sharply within the first 28 days.
[0011] WO2020 / 172330A1 discloses graphene carbon nanoparticles dispersed in a solvent by using a dispersant resin. The authors describe that the exfoliated graphene carbon nanoparticles, which are used according to the method of WO2020172330A1 and are dispersed with a polymer containing a vinyl heterocyclic amide monomer as a functional group, show poor stability in oil over time. What is more, the application does not mention tribological performance and stability under severe conditions.
[0012] WO2019145307A1 discloses a polymer-inorganic nanoparticle composition comprising inorganic nanoparticles, i.e., boron nitride (hBN), and a functionalized comb polymer as an integrated lubricant additive, which has both low temperature performance and anti-weld and anti-friction properties. The nanoparticle composition not only maintains excellent stability in lubricating oil for a long time, but also avoids any incompatibility between different DI packaging components. Reference is also made to graphene nanoparticles, but no further details are given about the graphene type, and no analytical data are provided. Summary of the invention
[0013] Therefore, the object of the present invention is to provide a graphene dispersion as a lubricant additive, which not only shows improved anti-friction properties but also has excellent stability over a long period of time when used in a lubricating oil composition. In addition, the lubricant additive should show good compatibility with different packaging components, dispersants and other additives in the lubricant formulation to meet industrial needs. SUMMARY OF THE INVENTION
[0015] In the present invention, it has surprisingly been found that a nanoparticle composition prepared by a grinding process as defined in claim 1 can be used as a lubricant additive in a lubricating oil composition for significantly improving the anti-friction properties, said nanoparticle composition comprising a multilayer graphene-based material (A) having a carbon nanotube structure at 200 m / s according to ISO / TS 80004-13. 2 / g to 1,500m 2 / g, and a G / D ratio between 0.5 and 2; a polyalkyl (meth)acrylate polymer (B); a silane compound (C) and a base fluid (D). The challenge is to incorporate a large amount of graphene nanoparticles in the composition to improve the anti-friction performance, while these graphene nanoparticles remain well dispersed over a long period of time. In addition, the use of the claimed stabilized high-load graphene nanoparticle composition shows great advantages for the lubricant formulation industry. No additional stabilizing additives are required, and the dilution effect is negligible, which leads to good DI packaging compatibility.
[0016] According to a first aspect, the present invention relates to a nanoparticle composition as defined in claim 1 .
[0017] A second aspect of the invention is a method of preparing such a nanoparticle composition.
[0018] A third aspect of the present invention is the use of such a nanoparticle composition as an additive to a lubricating oil composition for reducing the friction of moving parts.
[0019] A fourth aspect of the present invention is a lubricating oil composition comprising one or more base oils and the nanoparticle composition of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] In order to better illustrate the advantages and properties of the claimed nanoparticle composition, object of the present invention, a figure is attached as a non-limiting example:
[0021] Figure 1 is a graph showing the change in light transmittance value at 800 nm of a lubricating oil composition comprising 0.05 wt. % of the nanoparticle composition IE1 as a function of storage time. DETAILED DESCRIPTION OF THE INVENTION
[0023] Nanoparticle composition according to the present invention
[0024] Thus, the present invention relates to a nanoparticle composition comprising one or more nanoparticles (A), one or more polymers (B), one or more silane compounds (C) and one or more base fluids (D), wherein
[0025] (A) The one or more nanoparticles (A) are multilayer graphene-based materials containing oxygen groups, which have a carbonyl group at 200 m 2 / g to 1,500m 2 / g, and a G / D ratio between 0.5 and 2, preferably with a surface area of 250 m 2 / g to 1,000m 2 / g, more preferably 350m 2 / g to 800m 2 / g surface area BET,
[0026] (B) The one or more polymers (B) may be obtained by polymerizing the following monomer composition, wherein the monomer composition comprises:
[0027] a) 1 to 30 wt % of one or more functional monomers, based on the total weight of the monomer composition, selected from:
[0028] a1) aminoalkyl (meth)acrylates and aminoalkyl (meth)acrylamides, preferably N-(3-dimethylaminopropyl)methacrylamide, 3-diethylaminopentyl (meth)acrylate, 3-dibutylaminohexadecyl (meth)acrylate;
[0029] a2) nitriles of alkyl(meth)acrylic acids and other nitrogen-containing alkyl(meth)acrylates, preferably N-(methacryloyloxyethyl)diisobutylketimine, N-(methacryloyloxyethyl)di(hexadecyl)ketimine, (meth)acrylamidoacetonitrile, 2-methacryloyloxyethylmethylcyanamide, cyanomethyl(meth)acrylate;
[0030] a3) (meth)acrylic esters of ether alcohols, preferably tetrahydrofurfuryl (meth)acrylate, methoxyethoxyethyl (meth)acrylate, 1-butoxypropyl (meth)acrylate, cyclohexyloxyethyl (meth)acrylate, propoxyethoxyethyl (meth)acrylate, benzyloxyethyl (meth)acrylate, furfuryl (meth)acrylate, 2-butoxyethyl (meth)acrylate, 2-ethoxy-2-ethoxyethyl (meth)acrylate, 2-methoxy-2-ethoxypropyl (meth)acrylate, ethoxylated (meth)acrylates, 1-ethoxybutyl (meth)acrylate, methoxyethyl (meth)acrylate, 2-ethoxy-2-ethoxy-2-ethoxyethyl (meth)acrylate, esters of (meth)acrylic acid and methoxypolyethylene glycol;
[0031] a4) (meth)acrylate epoxyalkyl alkyl esters, preferably 2,3-epoxybutyl (meth)acrylate, 3,4-epoxybutyl (meth)acrylate, 10,11-epoxyundecyl (meth)acrylate, 2,3-epoxycyclohexyl (meth)acrylate, epoxyalkyl (meth)acrylates, for example 10,11-epoxyhexadecyl (meth)acrylate, glycidyl (meth)acrylate;
[0032] a5) phosphorus-, boron- and / or silicon-containing alkyl (meth)acrylates, such as preferably 2-(dimethylphosphato)propyl (meth)acrylate, 2-(ethylphosphite)propyl (meth)acrylate, 2-dimethylphosphinomethyl (meth)acrylate, dimethylphosphonoethyl (meth)acrylate, diethyl methacryloylphosphonate, dipropyl methacryloylphosphate, 2-(dibutylphosphono)ethyl (meth)acrylate, 2,3-butylene methacryloylethylborate, methyldiethoxymethacryloylethoxysilane, diethylphosphatoethyl (meth)acrylate;
[0033] a6) Heterocyclic alkyl (meth)acrylate, preferably 2-(1-imidazolyl)ethyl (meth)acrylate, 2-(4-morpholinyl)ethyl (meth)acrylate, oxazolidinyl ethyl ester and N-methacryloyl morpholine;
[0034] a7) vinyl halides, preferably vinyl chloride, vinyl fluoride, vinylidene chloride and vinylidene fluoride;
[0035] a8) vinyl esters, preferably vinyl acetate;
[0036] a9) vinyl monomers containing aromatic groups, preferably styrene, substituted styrenes having alkyl substituents in the side chains, for example α-methylstyrene and α-ethylstyrene, substituted styrenes having alkyl substituents on the ring, for example vinyltoluene and p-methylstyrene, halogenated styrenes, for example monochlorostyrene, dichlorostyrene, tribromostyrene and tetrabromostyrene;
[0037] a10) heterocyclic vinyl compounds, preferably 2-vinylpyridine, 3-vinylpyridine, 2-methyl-5-vinylpyridine, 3-ethyl-4-vinylpyridine, 2,3-dimethyl-5-vinylpyridine, vinylpyrimidine, vinylpiperidine, 9-vinylcarbazole, 3-vinylcarbazole, 4-vinylcarbazole, 1-vinylimidazole, 2-methyl-1-vinylimidazole, N-vinylpyrrolidone, 2-vinylpyrrolidone, N-vinylpyrrolidine, 3-vinylpyrrolidine, N-vinylcaprolactam, N-vinylbutyrolactam, vinyloxolane, vinylfuran, vinylthiophene, vinylthiolane, vinylthiazole and hydrogenated vinylthiazole, vinyl Azoles and Hydrogenated Vinyl Azoles;
[0038] a11) vinyl and prenyl ethers;
[0039] a12) methacrylic acid and acrylic acid, and
[0040] b) 30 to 70 weight percent, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylate monomers, wherein each of the alkyl groups of the one or more alkyl (meth)acrylate monomers is independently linear, cyclic or branched and contains 1 to 40 carbon atoms, and
[0041] c) 20 to 60 wt % based on the total weight of the monomer composition of one or more monomers having a number average molecular weight (M) of 500 to 10,000 g / mol. n ) based on polybutadiene macromonomers,
[0042] (C) 0.02 to 5 wt. % of the one or more silane compounds (C), based on the total weight of the nanoparticle composition, having formula (IV)
[0043] Si(R)(M) h (X) 3-h (IV)
[0044] Where 0≤h≤2; preferably h is 0,
[0045] M is a branched or straight-chain C1 to C4 alkyl group,
[0046] R is a branched or straight chain aliphatic, aromatic or mixed aliphatic-aromatic C1 to C 30 A carbonyl group, or R is a branched or straight-chain aliphatic, aromatic or mixed aliphatic-aromatic C1 to C 30 The carbonyl group, wherein the functional group is selected from carboxyl, carbonyl, hydroperoxycarbonyl, cyano, formyl, oxo, thio, hydroxyl, amino, imino, hydrazine, epoxy; preferably R is selected from a linear aliphatic C8 carbonyl group, a linear aliphatic C 16 a carbonyl group, a straight-chain aliphatic 3-aminopropyl group or a 3-glycidyloxypropyl group,
[0047] X is selected from H, Cl or a group OY, wherein Y is H or a C1 to C8 branched or linear alkyl, alkenyl, aryl or aralkyl group, a branched or linear C2 to C8 alkyl ether group or a mixture thereof, preferably X is methoxy or ethoxy,
[0048] Wherein the nanoparticle composition can be obtained by grinding the nanoparticle composition, preferably via a ball milling process.
[0049] Preferably, the one or more polybutadiene-based macromonomers c) have a number average molecular weight (M) of 1,500 to 7,500 g / mol, more preferably 3,500 to 7,000 g / mol, even more preferably 4,000 to 6,000 g / mol, most preferably 4,500 to 5,500 g / mol. n ).
[0050] According to the present invention, preferably the one or more polymers (B) have a weight average molecular weight (MW) of 10,000 to 1,000,000 g / mol, more preferably 50,000 to 800,000 g / mol, even more preferably 100,000 to 500,000 g / mol, most preferably 150,000 to 350,000 g / mol. w ).
[0051] According to another preferred aspect of the present invention, the one or more polymers (B) can be obtained by polymerizing the following monomer composition, wherein the monomer composition comprises:
[0052] a) 1 to 30 wt %, more preferably 5 to 30 wt %, even more preferably 10 to 20 wt % of the one or more functional monomers as component a), based on the total weight of the monomer composition; and
[0053] b1) 30 to 60% by weight, more preferably 30 to 50% by weight, even more preferably 35 to 50% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (I) as first component b):
[0054]
[0055] Where R is hydrogen or methyl, R 1 refers to a straight chain, branched or cyclic alkyl group having 1 to 8 carbon atoms, preferably 1 to 5 carbon atoms, and more preferably 1 to 4 carbon atoms; and
[0056] b2) from 0 to 20% by weight, more preferably from 1 to 15% by weight, even more preferably from 1 to 10% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (II) as second component b):
[0057]
[0058] Where R is hydrogen or methyl, R 2 refers to a linear, branched or cyclic alkyl group having 9 to 15 carbon atoms, preferably 12 to 15 carbon atoms, and more preferably 12 to 14 carbon atoms; and
[0059] b3) 0 to 20% by weight, more preferably 0 to 15% by weight, even more preferably 0 to 10% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (III) as third component b):
[0060]
[0061] Where R is hydrogen or methyl, R 3 refers to a linear, branched or cyclic alkyl group having 16 to 40 carbon atoms, preferably 16 to 30 carbon atoms, and more preferably 6 to 20 carbon atoms; and
[0062] c) 20 to 60 wt %, more preferably 20 to 50 wt %, even more preferably 30 to 50 wt %, based on the total weight of the monomer composition, of one or more monomers having a number average molecular weight (M) of 500 to 10,000 g / mol. n ) based polybutadiene macromonomer.
[0063] Preferably, the weight contents of the monomers a), b) and c) of the monomer composition for preparing polymer (B) add up to 100% by weight, based on the total weight of the monomer composition.
[0064] Preferably, the one or more silane compounds (C) of formula (IV) are octyltrimethoxysilane, hexadecyltrimethoxysilane, 3-aminopropyltriethoxysilane or 3-glycidoxypropyltriethoxysilane.
[0065] Preferably, the nanoparticle composition comprises:
[0066] 1 to 20 wt. % of one or more nanoparticles (A), more preferably 5 to 20 wt. %, even more preferably 8 to 17 wt. % of one or more nanoparticles (A), and
[0067] 0.5 to 30 wt. % of one or more polymers (B), more preferably 3 to 30 wt. %, even more preferably 5 to 25 wt. % of one or more polymers (B), and
[0068] 0.02 to 5 wt. % of one or more silane compounds (C), more preferably 0.05 to 3 wt. %, even more preferably 0.1 to 2 wt. % of one or more silane compounds (C), and
[0069] 45 to 98.48 wt. % of one or more base fluids (D), more preferably 47 to 91.95 wt. %, even more preferably 56 to 86.9 wt. % of one or more base fluids (D),
[0070] All amounts are based on the total weight of the nanoparticle composition.
[0071] According to another preferred aspect of the present invention, the weight content of components A), B), C) and D) totals 100 weight %, based on the total weight of the composition.
[0072] According to another preferred aspect of the present invention, the one or more base fluids (D) are selected from API Group I base oil, API Group II base oil, API Group III base oil, API Group IV base oil, API Group V base oil or mixtures thereof.
[0073] Graphene nanoparticles (A)
[0074] According to the present invention, the one or more graphene nanoparticles (A) are multilayer graphene-based materials containing oxygen groups, which have a carbonyl group at 200 m / s according to ISO / TS 80004-13. 2 / g to 1,500m 2 / g, and a G / D ratio between 0.5 and 2, preferably with a surface area of 250 m 2 / g to 1,000m 2 / g, more preferably 350m 2 / g to 800m2 / g surface area BET.
[0075] The one or more graphene nanoparticles (A) are preferably selected from one to ten layers of graphene according to ISO / TS 80004-13, more preferably selected from the following one to ten layers of graphene, which are selected from exfoliated graphene, graphene nanoplatelets, graphene nanoplatelets, graphene nanosheets, graphene microplatelets, graphene nanoflakes, graphene oxide, graphene oxide nanoplatelets, multilayer graphene oxide, reduced graphene oxide or mixtures thereof.
[0076] Further details on graphene, its preparation, its properties and applications can also be found in the technical literature, for example in Angew. Chem. Int. Ed. 2014, 53, 7714-7718 or Mater. Today 2012, 15 (3) 86-97.
[0077] Preferably, the nanoparticle composition according to the present invention comprises 1 to 20 wt. % of one or more nanoparticles (A), more preferably 5 to 20 wt. %, even more preferably 8 to 17 wt. % of one or more nanoparticles (A), based on the total weight of the nanoparticle composition.
[0078] Polymer (B)
[0079] According to the present invention, the one or more polymer compounds (B) can be obtained by polymerizing the following monomer composition, the monomer composition comprising:
[0080] a) 1 to 30 wt %, preferably 5 to 30 wt %, more preferably 10 to 20 wt % of the one or more functional monomers as component a), based on the total weight of the monomer composition; and
[0081] b) 30 to 70 wt%, preferably 30 to 60 wt%, more preferably 35 to 60 wt%, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylate monomers, wherein each of the alkyl groups of the one or more alkyl (meth)acrylate monomers is independently linear, cyclic or branched and contains 1 to 40 carbon atoms, and
[0082] c) 20 to 60 wt %, more preferably 20 to 50 wt %, even more preferably 30 to 50 wt %, based on the total weight of the monomer composition, of one or more monomers having a number average molecular weight (M) of 500 to 10,000 g / mol. n ) based polybutadiene macromonomer.
[0083] In a preferred embodiment, the amounts of monomers a), b) and c) of the monomer composition for preparing polymer (B) add up to 100% by weight, based on the total weight of the monomer composition used for preparing polymer (B).
[0084] According to the present invention, it is preferred that the one or more polymers (B) have a weight average molecular weight (MW) of 10,000 to 1,000,000 g / mol, more preferably 50,000 to 1,000,000 g / mol, even more preferably 100,000 to 800,000 g / mol, most preferably 200,000 to 600,000 g / mol. w ).
[0085] Preferably, the nanoparticle composition according to the present invention comprises 0.5 to 30 wt.-% of one or more polymers (B), more preferably 3 to 30 wt.-%, even more preferably 5 to 25 wt.-% of one or more polymers (B), based on the total weight of the nanoparticle composition.
[0086] In the present invention, the weight average molecular weight (M w ) is determined by gel permeation chromatography (GPC) using polystyrene calibration standards according to DIN 55672-1 using the following measurement conditions:
[0087] Eluent: tetrahydrofuran (THF) containing 0.02 M 2-diethylaminoethylamine
[0088] Operating temperature: 35℃
[0089] The column set consisted of a precolumn (SDV 10μ; 8×50 mm) and the following four columns: SDV SDV and 2×SDV (PSS Standards Service GmbH, Mainz, Germany), all four columns had dimensions of 300×8 mm and an average particle size of 10 μm
[0090] Flow rate: 1mL / min
[0091] Injection volume: 100 μL
[0092] Instrument: Agilent 1100 series, which consists of an autosampler, pump and column oven
[0093] Detection equipment: Refractive index detector from Agilent 1260 series.
[0094] Functional monomer a)
[0095] As already defined above, the one or more functional monomers a) according to the invention are chosen from the list consisting of:
[0096] a1) Aminoalkyl (meth)acrylates and aminoalkyl (meth)acrylamides;
[0097] a2) alkyl(meth)acrylic nitriles and other nitrogen-containing alkyl(meth)acrylates;
[0098] a3) (meth)acrylates of ether alcohols;
[0099] a4) epoxyalkyl alkyl (meth)acrylate;
[0100] a5) phosphorus-, boron- and / or silicon-containing alkyl (meth)acrylates;
[0101] a6) Heterocycloalkyl (meth)acrylate;
[0102] a7) vinyl halides;
[0103] a8) vinyl esters;
[0104] a9) vinyl monomers containing aromatic groups;
[0105] a10) heterocyclic vinyl compounds;
[0106] a11) vinyl and prenyl ethers;
[0107] a12) Methacrylic acid and acrylic acid.
[0108] Preferably, the functional monomer a) is selected from aminoalkyl (meth)acrylate a1) or aminoalkyl (meth)acrylamide a1) or heterocycloalkyl (meth)acrylate a6) or vinyl monomer containing aromatic group a9) or mixtures thereof. More preferably, it is selected from aminoalkyl (meth)acrylamide a1) or vinyl monomer containing aromatic group a9) or mixtures thereof.
[0109] Even more preferably, the functional monomer a) is selected from aminoalkyl(meth)acrylamides, most preferably N-(3-dimethylaminopropyl)methacrylamide, as first component a), and vinyl monomers containing aromatic groups, most preferably styrene, as second component a).
[0110] (Meth) acrylate monomer b)
[0111] The term "(meth)acrylic acid C 1-40"Alkyl ester" refers to an ester formed from (meth)acrylic acid and a linear, cyclic or branched alcohol having 1 to 40 carbon atoms. The term includes a single (meth)acrylic acid ester formed with an alcohol of a specific length, and also includes a mixture of (meth)acrylic acid esters formed with alcohols of different lengths.
[0112] In one embodiment of the present invention, the monomer composition further comprises as component b) one or more alkyl (meth)acrylate monomers, wherein each alkyl group of the one or more alkyl (meth)acrylate monomers is independently linear, cyclic or branched and comprises 1 to 40 carbon atoms.
[0113] As already indicated above, according to the present invention, the one or more alkyl (meth)acrylate monomers b) comprise
[0114] b1) one or more alkyl (meth)acrylates of formula (I):
[0115]
[0116] Where R is hydrogen or methyl, R 1 refers to a straight-chain, branched or cyclic alkyl group having 1 to 8 carbon atoms, preferably 1 to 5 carbon atoms, and more preferably 1 to 4 carbon atoms,
[0117] b2) one or more alkyl (meth)acrylates of formula (II):
[0118]
[0119] Where R is hydrogen or methyl, R 2 refers to a linear, branched or cyclic alkyl group having 9 to 15 carbon atoms, preferably 12 to 15 carbon atoms, and more preferably 12 to 14 carbon atoms,
[0120] b3) one or more alkyl (meth)acrylates of formula (III):
[0121]
[0122] Where R is hydrogen or methyl, R 3 It refers to a linear, branched or cyclic alkyl group having 16 to 40 carbon atoms, preferably 16 to 30 carbon atoms, and more preferably 16 to 22 carbon atoms.
[0123] The term "(meth)acrylic acid C 1-8"Alkyl ester" refers to an ester formed from (meth)acrylic acid and a straight chain or branched alcohol having 1 to 8 carbon atoms. The term includes a single (meth)acrylic acid ester formed with an alcohol of a specific length, and also includes a mixture of (meth)acrylic acid esters formed with alcohols of different lengths.
[0124] According to the present invention, the one or more monomers according to formula (I) (ie (meth) acrylic acid C 1-8 Each of the (meth)acrylates and alkyl esters) may be independently selected from (meth)acrylates derived from saturated alcohols, preferably methyl (meth)acrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, tert-butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cycloalkyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, heptyl (meth)acrylate, 2-tert-butylheptyl (meth)acrylate, n-octyl (meth)acrylate and 3-isopropylheptyl (meth)acrylate, the most preferred monomer according to formula (II) is methyl methacrylate.
[0125] Particularly preferred (meth)acrylic acid C 1-8 The alkyl esters are methyl (meth)acrylate and n-butyl (meth)acrylate; methyl methacrylate and n-butyl methacrylate are particularly preferred.
[0126] The term "(meth)acrylic acid C 9-15 "Alkyl ester" refers to an ester formed from (meth)acrylic acid and a straight chain or branched alcohol having 9 to 15 carbon atoms. The term includes a single (meth)acrylic acid ester formed with an alcohol of a specific length, and also includes a mixture of (meth)acrylic acid esters formed with alcohols of different lengths.
[0127] According to the present invention, the one or more monomers according to formula (II) (ie (meth) acrylic acid C 9-15 Each of the alkyl esters) can also be independently selected from nonyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, undecyl (meth)acrylate, 5-methylundecyl (meth)acrylate, n-dodecyl (meth)acrylate, 2-methyldodecyl (meth)acrylate, tridecyl (meth)acrylate, 5-methyltridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, pentadecyl (meth)acrylate, oleyl (meth)acrylate, cycloalkyl (meth)acrylate, cyclohexyl (meth)acrylate having a ring substituent, tert-butylcyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, bornyl (meth)acrylate and isobornyl (meth)acrylate.
[0128] Particularly preferred (meth)acrylic acid C 9-15 Alkyl esters are straight chain C 12-14 (Meth)acrylate of alcohol mixture ((meth)acrylate C 12-14 alkyl esters).
[0129] The term "(meth)acrylic acid C 16-40 "Alkyl ester" refers to an ester formed from (meth)acrylic acid and a straight chain or branched alcohol having 16 to 40 carbon atoms. The term includes a single (meth)acrylic acid ester formed with an alcohol of a specific length, and also includes a mixture of (meth)acrylic acid esters formed with alcohols of different lengths.
[0130] According to the present invention, the one or more monomers according to formula (III) (ie (meth) acrylic acid C 16-40 Each of the alkyl esters) can also be independently selected from hexadecyl (meth)acrylate, 2-methylhexadecyl (meth)acrylate, heptadecyl (meth)acrylate, 5-isopropylheptadecyl (meth)acrylate, 4-tert-butyloctadecyl (meth)acrylate, 5-ethyloctadecyl (meth)acrylate, 3-isopropyloctadecyl (meth)acrylate, octadecyl (meth)acrylate, nonadecyl (meth)acrylate, eicosyl (meth)acrylate, cetyl eicosyl (meth)acrylate, stearyl eicosyl (meth)acrylate, behenyl (meth)acrylate, eicosyl tetratriadecyl (meth)acrylate, cycloalkyl (meth)acrylate, 2,4,5-tri-tert-butyl-3-vinylcyclohexyl (meth)acrylate and 2,3,4,5-tetra-tert-butylcyclohexyl (meth)acrylate.
[0131] Preferably, the (meth)acrylic acid C 1-40 Alkyl esters include (meth) acrylic acid C 1-8 Alkyl esters and (meth) acrylic acid C 9-15 A mixture of alkyl esters, more preferably (meth) acrylic acid C 12-14 Alkyl esters.
[0132] Macromonomer component (c)
[0133] According to the invention, the monomer composition defined above comprises as component c) one or more polybutadiene-based macromonomers having a number average molecular weight of 500 to 10,000 g / mol. The polybutadiene-based macromonomers c) of the invention are (meth)acrylic acid esters, which are either the reaction product of a (meth)acrylic acid ester with a hydroxylated hydrogenated polybutadiene (by transesterification) or the reaction product of a (meth)acrylic acid with a hydroxylated hydrogenated polybutadiene (by direct esterification).
[0134] In this respect, the polymer compound (B) of the invention comprises a first polymer, also referred to as the backbone or main chain, and a plurality of further polymers, referred to as side chains, covalently bonded to the main chain. In the case of the present invention, the main chain of the polymer is formed by the unsaturated groups of the (meth)acrylate mentioned linked to one another. The alkyl groups of the (meth)acrylate and the hydrogenated polybutadiene chains form the side chains of the polymer.
[0135] The reaction product of an ester of (meth)acrylic acid and a hydroxylated hydrogenated polybutadiene or the reaction product of a (meth)acrylic acid and a hydroxylated hydrogenated polybutadiene corresponds to monomer c) and is also referred to in the present invention as macromonomer or polybutadiene-based macromonomer c), having a number average molecular weight of 500 to 10,000 g / mol.
[0136] The number average molecular weight M of the macromonomer n is determined by gel permeation chromatography (GPC) using polybutadiene calibration standards according to DIN 55672-1 using the following measurement conditions:
[0137] Eluent: Tetrahydrofuran (THF)
[0138] Operating temperature: 35℃
[0139] In: The column set consisted of a precolumn (PSS-SDV; 10μ; 8×50 mm), four PSS-SDV columns with dimensions of 300×8 mm and an average particle size of 10 μm (SDV-LXL, SDV-LinL, 2 columns SDV (PSS Standards Service GmbH, Mainz, Germany) and a solvent peak separation column with a size of 8×100 mm (KF-800D from Shodex)
[0140] Flow rate: 1mL / min
[0141] Injection volume: 100 μL
[0142] Instrument: Agilent 1100 series, which consists of an autosampler, pump and column oven
[0143] Detection: Refractive index detector from Agilent 1100 series
[0144] The one or more polymer compounds (B) prepared from the monomer composition comprising components a), b) and c) can be characterized based on their molar branching degree ("f-branching"). The molar branching degree refers to the percentage expressed in mol % of the macromonomer (component (c)) used, based on the total molar amount of all monomers in the monomer composition. The molar amount of the macromonomer used is based on the number average molecular weight (M) of the macromonomer. n The calculation of the molar degree of branching is described in detail in WO 2007 / 003238 A1, in particular on pages 13 and 14, to which reference is expressly made here.
[0145] Preferably, the one or more polymer compounds (B) have a molar branching degree f of 0.1 to 6 mol %, more preferably 1 to 4 mol % and most preferably 1.5 to 3 mol %. 支化 .
[0146] The one or more polybutadiene-based macromonomers used as component c) according to the present invention have a number average molecular weight (M) of 500 g / mol to 10,000 g / mol. n Due to the high molecular weight of the hydroxylated hydrogenated polybutadienes, they can also be referred to as macroalcohols in the context of the present invention. In the context of the present invention, the corresponding (meth)acrylic acid esters can also be referred to as macromonomers.
[0147] Component c) may comprise a single type of macromonomer or may comprise a mixture of different macromonomers based on different macroalcohols.
[0148] The hydroxylated hydrogenated polybutadiene may be a polybutadiene having a single number average molecular weight (M n ) or it may be a single polybutadiene having different number average molecular weights (M n ) of a mixture of different polybutadienes.
[0149] According to the present invention, the monomer composition comprises as component c) 20 to 60 wt %, preferably 20 to 50 wt %, more preferably 30 to 50 wt %, based on the total weight of the monomer composition, of one or more monomers having a number average molecular weight (M) of 500 g / mol to 10,000 g / mol. n ) based polybutadiene macromonomer.
[0150] In a preferred embodiment, the one or more polybutadiene-based macromonomers used as component c) according to the invention have a number average molecular weight (Mn) of 1,500 to 7,500 g / mol, preferably 3,500 to 7,000 g / mol, more preferably 4,000 to 6,000 g / mol, even more preferably 4,500 to 5,500 g / mol.
[0151] In another preferred embodiment, component c) can be a macromonomer prepared using one or more macroalcohols having different molecular weights, the first macroalcohol having a number average molecular weight of 1,500 to 2,500 g / mol, more preferably 1,800 to 2,500 g / mol, most preferably 1,900 to 2,300 g / mol, and the second macroalcohol having a number average molecular weight of 3,500 to 7,000 g / mol, preferably 4,000 to 6,000 g / mol, more preferably 4,500 to 5,500 g / mol. Component c) may also comprise a mixture of two macromonomers, the first macromonomer being prepared with a macroalcohol having a number average molecular weight of 1,500 to 2,500 g / mol, more preferably 1,800 to 2,500 g / mol, most preferably 1,900 to 2,500 g / mol, and the second macromonomer being prepared with a macroalcohol having a number average molecular weight of 3,500 to 7,000 g / mol, preferably 4,000 to 6,000 g / mol, more preferably 4,500 to 5,500 g / mol.
[0152] According to a preferred embodiment of the present invention, by combining two macromonomers having different number average molecular weights, the weight ratio of the lower molecular weight macromonomer to the higher molecular weight macromonomer is preferably 1 or more, more preferably 1.5 to 15, even more preferably 2 to 7, most preferably 3 to 6.
[0153] In a preferred embodiment, the hydroxylated hydrogenated polybutadiene is a monohydroxylated hydrogenated polybutadiene, preferably a hydroxyethyl-terminated or hydroxypropyl-terminated hydrogenated polybutadiene.
[0154] In another preferred embodiment of the present invention, the one or more (meth)acrylic acid esters used to prepare component c) of the polymer compound (B) are methyl (meth)acrylate or ethyl (meth)acrylate.
[0155] Preferably, the one or more hydroxylated hydrogenated polybutadienes have a hydrogenation level of at least 99%. An alternative measure of the hydrogenation level that can be determined for the polymers of the present invention is the iodine value. The iodine value refers to the grams of iodine that can be added to 100 g of polymer. Preferably, the polymers of the present invention have an iodine value of not more than 5 g of iodine per 100 g of polymer. The iodine value is determined by the Wijs method according to DIN 53241-1: 1995-05.
[0156] Preferred hydroxylated hydrogenated polybutadienes are obtainable according to GB 2270317.
[0157] As used herein, the term "hydroxylated hydrogenated polybutadiene" refers to a hydrogenated polybutadiene comprising one or more hydroxyl groups. The hydroxylated hydrogenated polybutadiene may further comprise additional structural units, such as polyether groups derived from the addition of alkylene oxides to polybutadiene or maleic anhydride groups derived from the addition of maleic anhydride to polybutadiene. These additional structural units may be introduced into the polybutadiene when the polybutadiene is functionalized with hydroxyl groups.
[0158] Monohydroxylated hydrogenated polybutadiene is preferred. More preferably, the hydroxylated hydrogenated polybutadiene is hydroxyethyl or hydroxypropyl terminated hydrogenated polybutadiene. Hydroxypropyl terminated polybutadiene is preferred.
[0159] These monohydroxylated hydrogenated polybutadienes can be prepared by first converting butadiene monomers into polybutadiene by anionic polymerization. Subsequently, hydroxyl-functionalized polybutadiene can be prepared by reacting the polybutadiene monomers with an alkylene oxide such as ethylene oxide or propylene oxide. The polybutadiene can also be reacted with more than one alkylene oxide unit to result in a polyether-polybutadiene block copolymer having terminal hydroxyl groups. The hydroxylated polybutadiene can be hydrogenated in the presence of a suitable transition metal catalyst.
[0160] These monohydroxylated hydrogenated polybutadienes may also be selected from products obtained by hydroboration of (co)polymers having terminal double bonds (e.g., as described in U.S. Pat. No. 4,316,973); maleic anhydride-ene-amino alcohol adducts obtained by ene reaction between (co)polymers having terminal double bonds and maleic anhydride and amino alcohols; and products obtained by hydroformylation of (co)polymers having terminal double bonds and subsequent hydrogenation (e.g., as described in JP Publication S63-175096).
[0161] The macromonomers c) used according to the invention can be prepared by transesterification of alkyl (meth)acrylates. The reaction of the alkyl (meth)acrylates with the hydroxylated hydrogenated polybutadiene forms the esters according to the invention. Methyl (meth)acrylate or ethyl (meth)acrylate is preferably used as reactant.
[0162] Such transesterification is widely known. For example, heterogeneous catalyst systems, such as lithium hydroxide / calcium oxide mixtures (LiOH / CaO), pure lithium hydroxide (LiOH), lithium methoxide (LiOMe) or sodium methoxide (NaOMe), or homogeneous catalyst systems, such as isopropyl titanate (Ti(OiPr) 4) or dioctyltin oxide (Sn(OCt) 2O) can be used for this purpose. The reaction is an equilibrium reaction. Therefore, the released low molecular weight alcohol is usually removed, for example by distillation.
[0163] Furthermore, the macromonomers c) are obtainable by direct esterification, for example starting from (meth)acrylic acid or (meth)acrylic anhydride, preferably under acidic catalysis with p-toluenesulfonic acid or methanesulfonic acid, or by the DCC process (dicyclohexylcarbodiimide) starting from free methacrylic acid.
[0164] Additionally, the hydroxylated hydrogenated polybutadiene of the present invention can be converted into an ester by reaction with an acyl chloride (eg, (meth)acryloyl chloride).
[0165] Preferably, in the preparation of the esters of the invention as detailed above, a polymerization inhibitor is used, for example 4-hydroxy-2,2,6,6-tetramethylpiperidinyloxy free radical and / or hydroquinone monomethyl ether.
[0166] Preferred monomer compositions for preparing polymer (B)
[0167] According to a preferred aspect of the present invention, the one or more polymer compounds (B) can be obtained by polymerizing the following monomer composition, wherein the monomer composition comprises:
[0168] a1) 0.5 to 5 wt. % of aminoalkyl(meth)acrylamide, most preferably N-(3-dimethylaminopropyl)methacrylamide, as first component a), based on the total weight of the monomer composition;
[0169] a9) 5 to 15 wt. % of a vinyl monomer containing an aromatic group, most preferably styrene, as second component a), based on the total weight of the monomer composition;
[0170] b1) 35 to 50 wt. % of an alkyl (meth)acrylate monomer of formula (I), most preferably methyl methacrylate and / or butyl methacrylate, as first component b), based on the total weight of the monomer composition;
[0171] b2) 1 to 10 wt. % of an alkyl (meth)acrylate monomer of formula (II), most preferably lauryl methacrylate, as second component b), based on the total weight of the monomer composition;
[0172] c) 30 to 50 wt % of one or more monomers having a number average molecular weight (M) of 500 to 10,000 g / mol, based on the total weight of the monomer composition. n ), most preferably having a number average molecular weight (M) of 1,500 to 5,500 g / mol n ) as component c).
[0173] In an even preferred embodiment, the amount of all monomers a), b) and c) of the monomer composition adds up to 100% by weight, based on the total weight of the monomer composition.
[0174] Preparation of polymer compound (B)
[0175] According to the present invention, the above polymer can be prepared according to a method comprising the following steps:
[0176] (a) providing a monomer composition as described above; and
[0177] (b) initiating free radical polymerization in the monomer composition.
[0178] Standard free-radical polymerization is described in detail in particular in Ullmann's Encyclopedia of Industrial Chemistry, 6th edition. In general, polymerization initiators and optionally chain transfer agents are used for this purpose.
[0179] The polymerization can be carried out at standard pressure, reduced pressure or elevated pressure. The polymerization temperature is also not critical. However, in general, it is in the range of -20 to 200°C, preferably 50 to 150°C and more preferably 80 to 130°C.
[0180] The polymerization step (b) can be carried out with or without dilution in oil. If dilution is carried out, the amount of the monomer composition, i.e. the total amount of monomers, is preferably from 20 to 90% by weight, more preferably from 40 to 80% by weight, most preferably from 50 to 70% by weight relative to the total weight of the reaction mixture.
[0181] Preferably, the oil used to dilute the monomer mixture is an API Group I, II, III, IV or V oil or a mixture thereof. Preferably, a Group III oil or a mixture thereof is used to dilute the monomer mixture.
[0182] Preferably, step (b) comprises adding a free radical initiator.
[0183] Suitable free radical initiators are, for example, azo initiators, such as azobisisobutyronitrile (AIBN), 2,2′-azobis(2-methylbutyronitrile) (AMBN) and 1,1-azobiscyclohexanecarbonitrile, and peroxide compounds, such as methyl ethyl ketone peroxide, acetylacetone peroxide, dilauroyl peroxide, tert-butyl per-2-ethylhexanoate, ketone peroxide, tert-butyl peroctoate, methyl isobutyl ketone peroxide, cyclohexanone peroxide, dibenzoyl peroxide, tert-Butyl peroxybenzoate, tert-butyl peroxyisopropyl carbonate, 2,5-bis(2-ethylhexanoylperoxy)-2,5-dimethylhexane, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxy-3,5,5-trimethylhexanoate, dicumyl peroxide, 1,1-bis(tert-butylperoxy)cyclohexane, 1,1-bis(tert-butylperoxy)-3,3,5-trimethylcyclohexane, cumyl hydroperoxide, tert-butyl hydroperoxide and bis(4-tert-butylcyclohexyl)peroxydicarbonate.
[0184] Preferably, the free radical initiator is selected from 2,2'-azobis(2-methylbutyronitrile), 2,2-bis(tert-butylperoxy)butane, tert-butyl peroxy-2-ethylhexanoate, 1,1-di-tert-butylperoxy-3,3,5-trimethylcyclohexane, tert-butyl peroxybenzoate and tert-butyl peroxy-3,5,5-trimethylhexanoate. Particularly preferred initiators are tert-butyl peroxy-2-ethylhexanoate and 2,2-bis(tert-butylperoxy)butane.
[0185] Preferably, the total amount of free radical initiator is 0.01 to 5 wt%, more preferably 0.02 to 1 wt%, most preferably 0.05 to 0.6 wt%, relative to the total weight of the monomer mixture.
[0186] The total amount of free radical initiator can be added in a single step, or the free radical initiator can be added in multiple steps during the polymerization reaction. Preferably, the free radical initiator is added in multiple steps. For example, a portion of the free radical initiator can be added to initiate free radical polymerization and a second portion of the free radical initiator can be added 0.5 to 3.5 hours after the initial dose.
[0187] Preferably, step (b) further comprises adding a chain transfer agent. Suitable chain transfer agents are in particular oil-soluble mercaptans, such as n-dodecyl mercaptan or 2-mercaptoethanol, or chain transfer agents selected from terpenes, such as terpinolene. It is particularly preferred to add n-dodecyl mercaptan.
[0188] The monomer composition may also be divided into an initial portion and a second portion, and a portion of the free radical initiator may be added only to the initial portion to initiate a polymerization reaction therein. The second portion of the free radical initiator is then added to the second portion of the monomer composition, which is then added to the polymerization mixture over a period of 0.5 to 5 hours, preferably 1.5 to 4 hours, and more preferably 2 to 3.5 hours. After the addition of the second monomer mixture, a third portion of the free radical initiator may be added to the polymerization reaction as described above.
[0189] Preferably, the total reaction time of the free radical polymerization is 2 to 10 hours, more preferably 3 to 9 hours.
[0190] After the free radical polymerization is completed, the obtained polymer is preferably further diluted with the above mentioned oil to the desired viscosity. Preferably, the polymer is diluted to a concentration of 5 to 60 wt % polymer, more preferably 10 to 50 wt %, most preferably 20 to 40 wt %.
[0191] Silane compound (C)
[0192] According to the present invention, the one or more silane compounds (C) have the formula (IV)
[0193] Si(R)(M) h (X) 3-h (IV)
[0194] Where 0≤h≤2; preferably h is 0,
[0195] M is a branched or straight-chain C1 to C4 alkyl group,
[0196] R is a branched or straight chain aliphatic, aromatic or mixed aliphatic-aromatic C1 to C 30 A carbonyl group, or R is a branched or straight-chain aliphatic, aromatic or mixed aliphatic-aromatic C1 to C 30 The carbonyl group, wherein the functional group is selected from carboxyl, carbonyl, hydroperoxycarbonyl, cyano, formyl, oxo, thio, hydroxyl, amino, imino, hydrazine, epoxy; preferably R is selected from a linear aliphatic C8 carbonyl group, a linear aliphatic C 16 a carbonyl group, a straight-chain aliphatic 3-aminopropyl group or a 3-glycidyloxypropyl group,
[0197] X is selected from H, Cl or a group OY, wherein Y is H or a C1 to C8 branched or linear alkyl, alkenyl, aryl or aralkyl group, a branched or linear C2 to C8 alkyl ether group or a mixture thereof, preferably X is methoxy or ethoxy,
[0198] The nanoparticle composition according to the present invention comprises 0.02 to 5 wt %, preferably 0.05 to 3 wt %, more preferably 0.1 to 2 wt % of one or more silane compounds (C), based on the total weight of the nanoparticle composition.
[0199] Preferably, the one or more silane compounds (C) of formula (IV) are octyltrimethoxysilane, hexadecyltrimethoxysilane, 3-aminopropyltriethoxysilane or 3-glycidoxypropyltriethoxysilane.
[0200] Base fluid (D)
[0201] The base fluid (D) in the nanoparticle composition may be a base oil selected from API Group I base oil, API Group II base oil, API Group III, API Group IV base oil and API Group V base oil or a combination thereof.
[0202] The base fluid (D) may also be defined as specified by the American Petroleum Institute (API) (see "Appendix E—API Base Oil Interchangeability Guidelines for Passenger Car Motor Oils and Diesel Engine Oils," April 2008 edition, Section 1.3, Subheading 1.3, "Base Stock Categories").
[0203] The API currently defines five groups of lubricant base stocks (API 1509, Annex E - API Base Oil Interchangeability Guide for Passenger Car Motor Oils and Diesel Engine Oils, September 2011). Groups I, II and III are mineral oils, which are classified by the amount of saturates and sulfur they contain and by their viscosity index; Group IV is polyalphaolefins; and Group V is all other materials, including, for example, ester oils. The following table illustrates these API classifications.
[0204] Table 1: API Definition of Lubricant Base Oils.
[0205]
[0206] Further base oils which can be used as base fluid (D) according to the invention are Fischer-Tropsch derived base oils of Groups II-III.
[0207] Fischer-Tropsch derived base oils are known in the art. The term "Fischer-Tropsch derived" means that the base oil is or is derived from a synthetic product of a Fischer-Tropsch process. Fischer-Tropsch derived base oils may also be referred to as GTL (gas to liquid) base oils. Suitable Fischer-Tropsch derived base oils that may be conveniently used as base oils in the lubricating compositions of the present invention are those disclosed, for example, in EP 0776959, EP 0668342, WO 97 / 21788, WO 00 / 15736, WO 00 / 14188, WO 00 / 14187, WO 00 / 14183, WO 00 / 14179, WO 00 / 08115, WO 99 / 41332, EP 1029029, WO 01 / 18156, WO 01 / 57166 and WO 2013 / 189951.
[0208] Preferably, the base fluid (D) in the nanoparticle composition is an API Group III base oil.
[0209] Method for preparing the nanoparticle composition of the present invention
[0210] Another aspect of the present invention is a method for preparing a graphene nanoparticle composition according to the present invention, the method comprising the following steps:
[0211] (i) providing one or more nanoparticle compounds (A) as defined herein;
[0212] (ii) providing one or more polymer compounds (B) as defined herein;
[0213] (iii) providing one or more silane compounds (C) as defined herein;
[0214] (iv) providing one or more base fluids (D) as defined herein;
[0215] (v) combining (A) to (D) to obtain a mixture; and
[0216] (vi) grinding the mixture of step (v).
[0217] The grinding technique according to the invention described in step (vi) can be high pressure homogenization, high shear mixing, ball milling or ultra high pressure technology (jet milling) or a combination thereof. In practice, the use of these grinding techniques reduces the particle size of the agglomerates.
[0218] Preferably, in step (vi), the mixture of the one or more nanoparticles (A), the one or more polymer compounds (B), the one or more silane compounds (C) and the one or more base fluids (D) is ground via a ball milling process. More preferably, in step (v), either compounds (A) and (C) are first mixed together and then mixed with (B) and (D), or (B), (C) and (D) are first mixed and (A) is added to the mixture, followed by the ball milling step (vi).
[0219] Preferably, the ball milling process comprises introducing 0.1 to 10 kWh / kg, preferably 0.5 to 5 kWh / kg, more preferably 1 to 3 kWh / kg of energy into the mixture.
[0220] In another preferred embodiment, the mixture of graphene nanoparticles (A), the one or more polymer compounds (B), the one or more silane compounds (C) and the one or more base fluids (D) is ground using ultrahigh pressure technology (e.g., jet mill SuginoUltimaizer HJP-25050). With the aid of a pump, preferably a high-pressure pump, at least two streams of this mixture are each sprayed through a nozzle (0.10 or 0.25 mm diameter) into a grinding chamber enclosed by a reactor housing to the collision point, characterized in that the grinding chamber is filled with the mixture and the last ground mixture is removed from the grinding chamber by the overpressure of the continuous flow flowing into the grinding chamber. The pump pressure is between 100 and 4,000 bar, preferably between 400 and 3,000 bar, more preferably between 1,000 and 2,500 bar.
[0221] According to the present invention, the grinding step (vi) is defined by the change in the particle size distribution of the resulting graphene nanoparticle composition measured using the dynamic light scattering technique (DLS).
[0222] Preprocessing
[0223] Preferably, in step (v), the compounds (A) and (C) are first mixed together by jet milling or ball milling, and then mixed with (B) and (D).
[0224] For the pretreatment method of spraying, if necessary and appropriate, the graphene nanoparticles (A) are first sprayed with water, and then sprayed with the silane compound (C). Spraying can also be carried out in the opposite order. The water used may have been acidified with acid, preferably hydrochloric acid to a pH of 7 to 1. If two or more silane compounds (C) are used, they can be applied individually or as a mixture.
[0225] The one or more silane compounds (C) may be dissolved in a suitable solvent. Mixing may be performed for 5 to 30 minutes after spraying.
[0226] The mixture is subsequently heat treated at a temperature of 20 to 400° C. for a period of 0.1 to 6 hours. The heat treatment may be carried out under an inert gas, preferably nitrogen.
[0227] The pretreatment can be carried out continuously or intermittently in a heatable mixer and dryer with a spray device. Suitable apparatuses may be, for example, the following apparatuses: plowshare mixer, plate dryer, fluidized bed dryer or fluidized bed dryer.
[0228] By pre-treatment of ball milling, the graphene nanoparticles (A) are ground together with a silane compound (C) optionally dissolved in a solvent (preferably ethanol) using a ball mill at a rotation speed of 100 to 1,000 rpm, preferably 400 to 800 rpm for 1 to 120 minutes, preferably 5 to 25 minutes.
[0229] Use of the nanoparticle composition according to the invention
[0230] Another aspect of the present invention is the use of the nanoparticle composition according to the present invention as an additive in a lubricating oil composition. Preferably, the lubricant additive is advantageously used in drive system lubricating oils (e.g. manual transmission fluids, differential gear oils, automatic transmission fluids and belt-type continuously variable transmission fluids, axle fluid formulations, dual clutch transmission fluids and dedicated hybrid transmission fluids), hydraulic oils (e.g. hydraulic oils for mechanical devices, power steering oils, shock absorber oils), engine oils (for gasoline engines and for diesel engines) and industrial oil formulations (e.g. wind turbines).
[0231] In a preferred embodiment according to the present invention, the nanoparticle composition improves the anti-friction properties of moving metal parts of an engine, a gearbox or a pump, a wind turbine or a hydraulic system of an automobile.
[0232] Lubricating oil composition
[0233] Yet another aspect of the present invention is a lubricating oil composition comprising the nanoparticle composition as defined herein and at least one or more base oils (E).
[0234] In a preferred embodiment of the present invention, the base oil (E) is selected from API Group I base oils, API Group II base oils, API Group III, API Group IV base oils and API Group V base oils or a mixture of one or more of these base oils, as described above in the paragraph about base fluid (D).
[0235] The base oil (E) to be used in the lubricating oil composition preferably comprises an oil of lubricating viscosity. Such oils include natural and synthetic oils, oils derived from hydrocracking, hydrogenation and hydrofinishing, unrefined, refined, re-refined oils or mixtures thereof.
[0236] Especially for transmission oil formulations, base oils of API Group III and mixtures of different Group III oils are used. In another preferred embodiment, the base oil may also be a mixture of one or more API Group V base oils with one or more API Group III base oils.
[0237] According to the present invention, the lubricating oil composition comprising the nanoparticle composition according to the present invention and one or more base oils (E) may optionally further comprise an additive (F) as disclosed below. Preferably, the lubricating oil composition further comprises one or more additives (F) selected from antioxidants, anti-wear additives, pour point depressants, corrosion inhibitors, metal passivators or electrostatic discharge inhibitors, defoamers, seal fixatives or seal compatibility agents or mixtures thereof.
[0238] According to the present invention, the lubricating oil composition preferably comprises:
[0239] 0.01 to 50 wt. %, more preferably 0.01 to 35 wt. %, even more preferably 0.1 to 25 wt. % of the nanoparticle composition, based on the total weight of the lubricating oil composition,
[0240] - 50 to 99.99 wt. %, more preferably 65 to 99.99 wt. %, even more preferably 75 to 99.9 wt. % of a base fluid (E) and
[0241] - 0 to 20 wt. %, more preferably 0.05 to 15 wt. %, even more preferably 5 to 15 wt. %, of one or more additive components (F), based on the total weight of the lubricating oil composition.
[0242] Preferably, the amount of the nanoparticle composition, the base fluid (E), the one or more additive components (F) totals 98 wt%, more preferably totals 100 wt%, based on the total weight of the lubricating oil composition.
[0243] The lubricating oil composition according to the present invention may further contain as component (F) an additional additive selected from dispersants, defoamers, detergents, antioxidants, pour point depressants, antiwear additives, extreme pressure additives, anticorrosion additives, yellow metal deactivators, friction modifiers, dyes and mixtures thereof.
[0244] Suitable dispersants include poly(isobutylene) derivatives, such as poly(isobutylene) succinimide (PIBSI), including borated PIBSI; and ethylene-propylene oligomers having N / O functional groups.
[0245] Dispersants, including boronated dispersants, are preferably used in an amount of 0 to 20 wt %, more preferably 0 to 15 wt %, based on the total amount of the lubricant composition.
[0246] Suitable defoamers are silicone oils, fluorosilicone oils or fluoroalkyl ethers.
[0247] The defoaming agent is preferably used in an amount of 0.001 to 0.2 wt % based on the total amount of the lubricant composition.
[0248] Preferred detergents include metal-containing compounds, such as phenates; salicylates; thiophosphonates, especially thiopyrophosphonates, thiophosphonates and phosphonates; sulfonates and carbonates. As metals, these compounds may contain, inter alia, calcium, magnesium and barium. These compounds may preferably be used in neutral or overbased form.
[0249] The detergent is preferably used in an amount of 0.2 to 8 wt %, preferably 0.2 to 4 wt %, based on the total amount of the lubricant composition.
[0250] Suitable antioxidants include, for example, phenol-based antioxidants and amine-based antioxidants.
[0251] Phenol-based antioxidants include, for example, octadecyl 3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate; 4,4′-methylenebis(2,6-di-tert-butylphenol); 4,4′-bis(2,6-di-tert-butylphenol); 4,4′-bis(2-methyl-6-tert-butylphenol); 2,2′-methylenebis(4-ethyl-6-tert-butylphenol); 2,2′-methylenebis(4-methyl- 6-tert-butylphenol); 4,4′-butylidenebis(3-methyl-6-tert-butylphenol); 4,4′-isopropylidenebis(2,6-di-tert-butylphenol); 2,2′-methylenebis(4-methyl-6-nonylphenol); 2,2′-isobutylidenebis(4,6-dimethylphenol); 2,2′-methylenebis(4-methyl-6-cyclohexylphenol); 2,6-di-tert-butyl-4-methylphenol ; 2,6-di-tert-butyl-4-ethyl-phenol; 2,4-dimethyl-6-tert-butylphenol; 2,6-di-tert-amyl-p-cresol; 2,6-di-tert-butyl-4-(N,N′-dimethylaminomethylphenol); 4,4′-thiobis(2-methyl-6-tert-butylphenol); 4,4′-thiobis(3-methyl-6-tert-butylphenol); 2,2′-thiobis(4-methyl-6-tert-butylphenol); phenol); bis(3-methyl-4-hydroxy-5-tert-butylbenzyl) sulfide; bis(3,5-di-tert-butyl-4-hydroxybenzyl) sulfide; 3-(4-hydroxy-3,5-di-tert-butylphenyl) propionate n-octyl; 3-(4-hydroxy-3,5-di-tert-butylphenyl) propionate n-octadecyl; 2,2′-thio[diethyl-bis-3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate], etc. Among them, particularly preferred are bisphenol-based antioxidants and phenol-based antioxidants containing ester groups.
[0252] The amine-based antioxidants include, for example, monoalkyldiphenylamines, such as monooctyldiphenylamine, monononyldiphenylamine, and the like; dialkyldiphenylamines, such as 4,4′-dibutyldiphenylamine, 4,4′-dipentyldiphenylamine, 4,4′-dihexyldiphenylamine, 4,4′-diheptyldiphenylamine, 4,4′-dioctyldiphenylamine, 4,4′-dinonyldiphenylamine, and the like; polyalkyldiphenylamines, such as tetrabutyldiphenylamine, tetrahexyldiphenylamine, tetraoctyldiphenylamine, tetranonyldiphenylamine, and the like; naphthylamines, specifically, α-naphthylamine, phenyl-α-naphthylamine and additional alkyl-substituted phenyl-α-naphthylamines, such as butylphenyl-α-naphthylamine, pentylphenyl-α-naphthylamine, hexylphenyl-α-naphthylamine, heptylphenyl-α-naphthylamine, octylphenyl-α-naphthylamine, nonylphenyl-α-naphthylamine, and the like. Among them, diphenylamines are superior to naphthylamines from the viewpoint of their antioxidant effects.
[0253] Suitable antioxidants may further be selected from compounds containing sulfur and phosphorus, for example metal dithiophosphates, such as zinc dithiophosphate (ZnDTP), "OOS triesters" = reaction products of dithiophosphoric acids with activated double bonds from olefins, cyclopentadiene, norbornadiene, α-pinene, polybutene, acrylates, maleates (ashless on combustion); organic sulfur compounds, such as dialkyl sulfides, diaryl sulfides, polysulfides, modified mercaptans, thiophene derivatives, xanthates, thioglycols, thioaldehydes, sulfur-containing carboxylic acids; heterocyclic sulfur / nitrogen compounds, especially dialkyldimercaptothiadiazoles, 2-mercaptobenzimidazoles; zinc bis(dialkyldithiocarbamates) and methylenebis(dialkyldithiocarbamates); organic phosphorus compounds, such as triaryl and trialkyl phosphites; organic copper compounds and overbased calcium- and magnesium-based phenates and salicylates.
[0254] The antioxidant is used in an amount of 0 to 15 wt %, preferably 0.01 to 10 wt %, more preferably 0.01 to 5 wt %, based on the total amount of the lubricant composition.
[0255] Suitable anti-corrosion additives are partial succinates, amine salts of partial succinates, organic carboxylic acids, sulfonates, and suitable yellow metal passivators are thiadiazoles, triazoles and high molecular weight phenolic antioxidants.
[0256] The anti-corrosion additive is used in an amount of 0 to 5 weight percent, and the yellow metal passivator is used in an amount of 0 to 1 weight percent, all amounts being based on the total weight of the lubricant composition.
[0257] Pour point depressants include ethylene-vinyl acetate copolymers, chlorinated paraffin-naphthalene condensates, chlorinated paraffin-phenol condensates, polymethacrylates, polyalkylstyrenes, etc. Preferred are those having a weight average molecular weight (M) of 5,000 to 200,000 g / mol. w ) of polymethacrylate.
[0258] The amount of the pour point depressant is preferably 0.1 to 5 wt % based on the total amount of the lubricant composition.
[0259] Preferred antiwear and extreme pressure additives include sulfur-containing compounds such as zinc dithiophosphate, di-C 3-12Zinc alkyl dithiophosphate (ZnDTP), zinc phosphate, zinc dithiocarbamate, molybdenum dithiocarbamate, molybdenum dithiophosphate, alkyl dithiophosphate, disulfide, sulfurized olefins, sulfurized oils and fats, sulfurized esters, thiocarbonates (salts), thiocarbamates (salts), polysulfides, etc.; phosphorus-containing compounds, such as phosphites (salts), phosphates (salts), such as trialkyl phosphates, triaryl phosphates, such as tricresyl phosphate, amine-neutralized mono- and dialkyl phosphates, ethoxylated mono- and dialkyl phosphates, phosphonates, phosphines, amine salts or metal salts of these compounds, etc.; sulfur- and phosphorus-containing antiwear agents, such as thiophosphites (salts), thiophosphates (salts), thiophosphonates (salts), amine salts or metal salts of these compounds.
[0260] The antiwear agent may be present in an amount of 0 to 3 wt%, preferably 0.1 to 1.5 wt%, more preferably 0.5 to 0.9 wt%, based on the total amount of the lubricant composition.
[0261] Preferred friction modifiers may include mechanically active compounds such as molybdenum disulfide, graphite (including graphite fluoride), poly(trifluoroethylene), polyamide, polyimide; compounds that form adsorption layers, such as long-chain carboxylic acids, fatty acid esters, ethers, alcohols, amines, amides, imides, phosphonates, phosphites; compounds that form layers by tribochemical reactions, such as saturated fatty acids, phosphoric acid, borate esters and thiophosphates, xanthogenates, sulphurized fatty acids; compounds that form polymeric layers, such as ethoxylated dicarboxylic acid partial esters, dialkyl phthalates, methacrylates, unsaturated fatty acids, sulphurized olefins and organometallic compounds, such as molybdenum compounds (molybdenum dithiophosphates and molybdenum dithiocarbamates MoDTC) and their combinations with ZnDTP, copper-containing organic compounds.
[0262] Some of the compounds listed above can fulfill multiple functions. For example, ZnDTP is primarily an antiwear additive and an extreme pressure additive, but also has the characteristics of an antioxidant and a corrosion inhibitor (here: metal passivator / deactivator).
[0263] The additives specified above are described in detail in particular in T. Mang, W. Dresel (eds.): “Lubricants and Lubrication”, Wiley-VCH, Weinheim 2001; RM Mortier, ST Orszulik (eds.): “Chemistry and Technology of Lubricants”.
[0264] An all-in-one lubricant formulation comprising the nanoparticle composition of the present invention combines long-term stability with improved anti-friction properties, as demonstrated below in the experimental section. This approach can thus avoid any incompatibilities between different packaging components, dispersants and other additives in the lubricant formulation, since a single additive combines all properties. DETAILED DESCRIPTION
[0265] Experimental Section
[0266] The present invention is hereinafter further illustrated in detail with reference to Examples and Comparative Examples, without any intention of limiting the scope of the present invention.
[0267] abbreviation
[0268] 9116 Hexadecyltrimethoxysilane
[0269] AMEO 3-Aminopropyltriethoxysilane
[0270] C1 AMA C1-alkyl methacrylate (methyl methacrylate; MMA)
[0271] C4 AMA C4-alkyl methacrylate (n-butyl methacrylate)
[0272] C 12-14 AMA Methacrylic Acid C 12-14 -Alkyl ester
[0273] DMAPMAA N-3-Dimethylaminopropyl methacrylamide
[0274] f 支化 Degree of branching expressed in mol%
[0275] GLYEO 3-Glycidyloxypropyltriethoxysilane
[0276] MMA Methyl (meth)acrylate
[0277] MA-1 macroalcohol (hydroxylated hydrogenated polybutadiene, M n =4,900 g / mol)
[0278] MM-1 Macromonomer of hydrogenated polybutadiene MA-1 with methacrylate functional groups (M n =4,900 g / mol)
[0279] M n Number average molecular weight
[0280] MTM Mini Traction Machine Equipment
[0281] M w Weight average molecular weight
[0282] NB3020 3020; Group III base oil from Neste with a KV of 2.2 cSt 100
[0283] NB3043 3043; Group III base oil from Neste with a KV of 4.3 cSt 100
[0284] OCTMO Octyltrimethoxysilane
[0285] PDI polydispersity index, via M w / M n Calculated molecular weight distribution
[0286] PS Standard Polystyrene Calibration Standard
[0287] Si69 Bis[3-(triethoxysilyl)propyl]polysulfide
[0288] Synthesis of Hydroxylated Hydrogenated Polybutadiene (Macroalcohol) MA-1
[0289] The macroalcohol is synthesized by anionic polymerization of 1,3-butadiene with butyl lithium at 20-45° C. When the desired degree of polymerization is reached, the reaction is terminated by addition of propylene oxide and the lithium is removed by precipitation with methanol. Subsequently, the polymer is hydrogenated in a hydrogen atmosphere in the presence of a noble metal catalyst at up to 140° C. and 200 bar pressure. After the hydrogenation has ended, the noble metal catalyst is removed and the organic solvent is drawn off under reduced pressure to obtain 100% macroalcohol MA-1. Table 2 summarizes the characterization data of MA-1:
[0290] Table 2: Characterization data of the macroalcohols used.
[0291] <![CDATA[M n [g / mol]]]> Hydrogenation level [%] OH functionality [%] MA-1 4,900 >99 >98
[0292] Synthesis of Macromonomer MM-1
[0293] In a 2-liter stirred apparatus equipped with a saber stirrer, air inlet tube, thermocouple with controller, heating jacket, randomly packed column with 3 mm wire spiral, steam distributor, top thermometer, reflux condenser and bottom cooler, 1000 g of the above macroalcohol was dissolved in methyl methacrylate (MMA) by stirring at 60° C. 20 ppm of 2,2,6,6-tetramethylpiperidin-1-oxyl radical and 200 ppm of hydroquinone monomethyl ether were added to the solution. After heating to MMA reflux (bottom temperature of about 110° C.) while passing air through for stabilization, about 20 mL of MMA was distilled out for azeotropic drying. After cooling to 95° C., LiOCH3 was added, and the mixture was heated back to reflux. After a reaction time of about 1 hour, the top temperature dropped to about 64° C. due to the formation of methanol. The methanol / MMA azeotrope formed was continuously distilled out until a constant top temperature of about 100° C. was established again. At this temperature, the mixture was reacted for another 1 hour. For further post-processing, most of the MMA was extracted under reduced pressure. Insoluble catalyst residues were removed by pressure filtration (Seitz T1000 depth filter). Table 3 summarizes the amount of MMA and LiOCH3 used to synthesize the macromonomer MM-1.
[0294] Table 3: Amounts of macroalcohol, MMA and catalyst for transesterification of macromonomers
[0295] Macromonomer Macroalcohol Amount of MMA [g] <![CDATA[Amount of LiOCH3 [g]]]> MM-1 MA-1 500 1.5
[0296] As described above, the polymer weight average molecular weight (M) of all inventive polymers and comparative polymers was measured by gel permeation chromatography (GPC) using polystyrene calibration standards according to DIN 55672-1. w ).
[0297] Example of the present invention - Preparation of polymer (P1) containing amine and macromonomer:
[0298] 85 grams of Nexbase 3020, 85 grams of Berylane 230SPP, 98 grams of macromonomers, 107 grams of butyl methacrylate, 28 grams of styrene, 12.5 grams of lauryl methacrylate, 8.6 grams of dimethylaminopropyl methacrylamide, 0.5 grams of methyl methacrylate and 0.1 grams of n-dodecyl mercaptan are fed into 2 liters of 4-necked round-bottomed flasks. The reaction mixture is stirred using a C stirring rod, protected by nitrogen inertia, and heated to 115 ° C. Once the reaction mixture reaches the set point temperature, 0.9 grams of 2-ethylperoxyhexanoic acid tert-butyl esters are fed into the reactor in 3 hours. In 30 minutes and 3 hours after the previous feeding, 0.5 grams of 2,2-bis--(tert-butyl peroxy) butane are added. Allow the reaction to stir for 1 hour, and then add other 175 grams of Nexbase3020 into the reactor and mix it for 1 hour. The obtained polymer had a weight average molecular weight (Mw) of 238,000 g / mol (PS standard).
[0299] Preparation of Comparative Example Polymer (P2):
[0300] 200 g Nexbase 3043, 28.36 g benzyl methacrylate, 255.2 g lauryl methacrylate (C 12-14 AMA), 5.53 g of n-dodecyl mercaptan (n-DDM), 5.53 g of 2-ethylhexyl thioglycolate (TGEH) were added to a 2-liter 4-necked round bottom flask. The reaction mixture was stirred using a C stirring rod, inertly protected with nitrogen, and heated to 90°C. Once the reaction mixture reached the set point temperature, 2.83 g of tert-butyl per-2-ethylhexanoate was fed into the reactor within 2 hours. After 2 hours, the mixture was heated to a maximum of 100°C, and after reaching the set point, 1.42 g of tert-butyl per-2-ethylhexanoate and 1.13 g of tert-butyl perpivalate were fed within one hour. The residual monomers were measured by gas chromatography to ensure good monomer conversion. The polymer obtained had a weight average molecular weight (M) of 9,470 g / mol. w )(PS standard).
[0301] For Examples P1 and P2, the monomer components total 100%. The amounts of initiator and chain transfer agent are given relative to the total amount of monomers. Table 4 below shows the monomer compositions and reactants used to prepare polymers P1 and P2, as well as their final characterization.
[0302]
[0303] Preparation of the nanoparticle composition according to the present invention
[0304] Dispersion IE1 of the present invention:
[0305] The ball mill apparatus (Netzsch laboratory mill micro series) was pre-loaded with 230.85 g NB3043 oil and 82.4 g P1 and 1.75 g silane (Dynasylan OCTMO), while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 35 g of graphene nanoparticles (surface area 700 m 2 / g and G / D ratio of 1.1) were added to the solution. The peristaltic pump was adjusted to 130 rpm, and the ball mill was set to a rotation speed of 3900 rpm. The dispersion was treated for 120 minutes (1.0 kWh of energy was introduced). The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in TegosoftDEC oil) showed a d90 value of 85 nm.
[0306] Dispersion IE2 of the present invention:
[0307] A ball mill apparatus (Netzsch laboratory mill micro series) was pre-loaded with 230.85 g NB3043 oil and 82.4 g P1 and 1.75 g silane (Dynasylan 9116), while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 35 g of graphene nanoparticles (surface area 700 m 2 / g and G / D ratio of 1.1) were added to the solution. The peristaltic pump was adjusted to 130 rpm, and the ball mill was set to a rotation speed of 3900 rpm. The dispersion was treated for 120 minutes (1.0 kWh of energy was introduced). The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in TegosoftDEC oil) showed a d90 value of 76 nm.
[0308] Dispersion IE3 of the present invention:
[0309] The ball mill apparatus (Netzsch laboratory mill micro series) was pre-loaded with 229.1 g NB3043 oil and 82.4 g P1 and 3.5 g silane (Dynasylan OCTMO), while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 35 g of graphene nanoparticles (surface area 700 m 2 / g and G / D ratio of 1.1) were added to the solution. The peristaltic pump was adjusted to 130 rpm, and the ball mill was set to a rotation speed of 3900 rpm. The dispersion was treated for 120 minutes (1.0 kWh of energy was introduced). The particle size distribution (measured using a dynamic light scattering device, LA-950, from Horiba Ltd., Japan, in TegosoftDEC oil) showed a d90 value of 75 nm.
[0310] Dispersion IE4 of the present invention:
[0311] The ball mill apparatus (Netzsch laboratory mill micro series) was pre-loaded with 231.9 g NB3043 oil and 82.4 g P1 and 0.7 g silane (Dynasylan OCTMO), while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 35 g of graphene nanoparticles (surface area 700 m 2 / g and G / D ratio of 1.1) were added to the solution. The peristaltic pump was adjusted to 130 rpm, and the ball mill was set to a rotation speed of 3900 rpm. The dispersion was treated for 120 minutes (1.0 kWh of energy was introduced). The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in TegosoftDEC oil) showed a d90 value of 73 nm.
[0312] Dispersion IE5 of the present invention:
[0313] The ball mill apparatus (Netzsch laboratory mill micro series) was pre-loaded with 230.85 g NB3043 oil and 82.4 g P1 and 1.75 g silane (Dynasylan OCTMO), while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 35 g of graphene nanoparticles (surface area 500 m 2 / g and G / D ratio of 1.0) were added to the solution. The peristaltic pump was adjusted to 130 rpm, and the ball mill was set to a rotation speed of 3900 rpm. The dispersion was treated for 120 minutes (1.0 kWh of energy was introduced). The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in TegosoftDEC oil) showed a d90 value of 96 nm.
[0314] Dispersion IE6 of the present invention:
[0315] The ball mill apparatus (Netzsch laboratory mill micro series) was pre-loaded with 230.85 g NB3043 oil and 82.4 g P1 and 1.75 g silane (Dynasylan OCTMO), while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 35 g of graphene nanoparticles (surface area 250 m 2 / g and G / D ratio of 1.5) were added to the solution. The peristaltic pump was adjusted to 130 rpm, and the ball mill was set to a rotation speed of 3900 rpm. The dispersion was treated for 120 minutes (1.0 kWh of energy was introduced). The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in TegosoftDEC oil) showed a d90 value of 194 nm.
[0316] Dispersion IE7 of the present invention:
[0317] The pre-treated graphene-based material was prepared as follows:
[0318] Ethanol was provided in an amount of 3 ppw (pa). 1 ppw of silane (Dynasylan OCTMO) was carefully added using a syringe and stirred at room temperature for about 10 minutes. A clear phase was obtained. 10 ppw of graphene nanoparticles (surface area 700 m 2 / g and G / D ratio of 1.1) are filled into the grinding container of a ball mill, and 4 ppw of the clarified phase is added. In addition, 4 ppw of grinding balls with a diameter of 2 to 10 mm are added. The reaction is carried out in a ball mill at a rotation speed of 600 rpm for 15 minutes. The functionalized graphene-based material obtained is then washed with ethanol (pa) by means of a Soxhlet extractor, pre-dried overnight in a fume hood, and then dried in a rotary evaporator at 100 ° C and at a pressure of 30 hPa for 3 hours.
[0319] Grinding process:
[0320] The ball mill equipment (Netzsch laboratory mill micro series) is preloaded with 221.85gNB3043 oil and 82.4gP1, and the peristaltic pump is set to 90rpm, and the ball mill is set to 1000rpm. Then, 35g of pretreated graphene nanoparticles are added to the solution. The peristaltic pump is adjusted to 130rpm, and the ball mill is set to a rotating speed of 3900rpm. The dispersion is processed for 120 minutes (introducing 1.0kWh of energy). Particle size distribution (using the dynamic light scattering equipment of Japan Horiba Ltd., LB-500, measured in Tegosoft DEC oil) shows a d90 value of 100nm.
[0321] Dispersion IE8 of the present invention:
[0322] The pre-treated graphene-based material was prepared as follows:
[0323] Ethanol was provided in an amount of 3 ppw (pa). 1 ppw of silane (Dynasylan 9116) was carefully added with a syringe and stirred at room temperature for about 10 minutes. A clear phase was obtained. 10 ppw of graphene nanoparticles (surface area 700 m 2 / g and G / D ratio of 1.1) are filled into the grinding container of a ball mill, and 4 ppw of the clarified phase is added. In addition, 4 ppw of grinding balls with a diameter of 2 to 10 mm are added. The reaction is carried out in a ball mill at a rotation speed of 600 rpm for 15 minutes. The functionalized graphene-based material obtained is then washed with ethanol (pa) by means of a Soxhlet extractor, pre-dried overnight in a fume hood, and then dried in a rotary evaporator at 100 ° C and at a pressure of 30 hPa for 3 hours.
[0324] Grinding process:
[0325] Ball mill equipment (Netzsch laboratory mill micro series) is preloaded with 221.85gNB3043 oil and 82.4gP1, peristaltic pump is set to 90rpm, and ball mill is set to 1000rpm. Then, 35g of pretreated graphene nanoparticles are added to the solution. The peristaltic pump is adjusted to 130rpm, and the ball mill is set to a rotating speed of 3900rpm. The dispersion is processed for 120 minutes (introducing 1.0kWh of energy). Particle size distribution (using the dynamic light scattering equipment of Japan Horiba Ltd., LB-500, measured in Tegosoft DEC oil) shows a d90 value of 75nm.
[0326] Dispersion IE9 of the present invention:
[0327] Preparation of pre-treated graphene-based materials:
[0328] The pre-treated graphene-based material was prepared as follows:
[0329] Ethanol was provided in an amount of 3 ppw (pa). 1 ppw of silane (Dynasylan AMEO) was carefully added using a syringe and stirred at room temperature for about 10 minutes. A clear phase was obtained. 10 ppw of graphene nanoparticles (surface area 700 m 2 / g and G / D ratio of 1.1) are filled into the grinding container of a ball mill, and 4 ppw of the clarified phase is added. In addition, 4 ppw of grinding balls with a diameter of 2 to 10 mm are added. The reaction is carried out in a ball mill at a rotation speed of 600 rpm for 15 minutes. The functionalized graphene-based material obtained is then washed with ethanol (pa) by means of a Soxhlet extractor, pre-dried overnight in a fume hood, and then dried in a rotary evaporator at 100 ° C and at a pressure of 30 hPa for 3 hours.
[0330] Grinding process:
[0331] The ball mill equipment (Netzsch laboratory mill micro series) is preloaded with 221.85gNB3043 oil and 82.4gP1, and the peristaltic pump is set to 90rpm, and the ball mill is set to 1000rpm. Then, 35g of pretreated graphene nanoparticles are added to the solution. The peristaltic pump is adjusted to 130rpm, and the ball mill is set to a rotating speed of 3900rpm. The dispersion is processed for 120 minutes (introducing 1.0kWh of energy). Particle size distribution (using the dynamic light scattering equipment of Japan Horiba Ltd., LB-500, measured in Tegosoft DEC oil) shows a d90 value of 79nm.
[0332] Dispersion IE10 of the present invention:
[0333] The pre-treated graphene-based material was prepared as follows:
[0334] Ethanol was provided in an amount of 3 ppw (pa). 1 ppw of silane (Dynasylan GLYEO) was carefully added using a syringe and stirred at room temperature for about 10 minutes. A clear phase was obtained. 10 ppw of graphene nanoparticles (surface area 700 m 2 / g and G / D ratio of 1.1) are filled into the grinding container of a ball mill, and 4 ppw of the clarified phase is added. In addition, 4 ppw of grinding balls with a diameter of 2 to 10 mm are added. The reaction is carried out in a ball mill at a rotation speed of 600 rpm for 15 minutes. The functionalized graphene-based material obtained is then washed with ethanol (pa) by means of a Soxhlet extractor, pre-dried overnight in a fume hood, and then dried in a rotary evaporator at 100 ° C and at a pressure of 30 hPa for 3 hours.
[0335] Grinding process:
[0336] The ball mill equipment (Netzsch laboratory mill micro series) is preloaded with 221.85gNB3043 oil and 82.4gP1, and the peristaltic pump is set to 90rpm, and the ball mill is set to 1000rpm. Then, 35g of pretreated graphene nanoparticles are added to the solution. The peristaltic pump is adjusted to 130rpm, and the ball mill is set to a rotating speed of 3900rpm. The dispersion is processed for 120 minutes (introducing 1.0kWh of energy). Particle size distribution (using the dynamic light scattering equipment of Japan Horiba Ltd., LB-500, measured in Tegosoft DEC oil) shows a d90 value of 81nm.
[0337] Dispersion IE11 of the present invention:
[0338] The ball mill apparatus (Netzsch laboratory mill micro series) was pre-loaded with 171.37 g NB3020 oil and 123.5 g P1 and 2.63 g silane (Dynasylan OCTMO), while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 52.5 g of graphene nanoparticles (surface area 500 m 2 / g and G / D ratio of 1.0) were added to the solution. The peristaltic pump was adjusted to 130 rpm, and the ball mill was set to a rotation speed of 3900 rpm. The dispersion was treated for 120 minutes (1.0 kWh of energy was introduced). The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d90 value of 83 nm.
[0339] Dispersion IE12 of the present invention:
[0340] The ball mill apparatus (Netzsch laboratory mill micro series) was pre-loaded with 232.42 g NB3043 oil and 82.4 g P1 and 0.18 g silane (Dynasylan OCTMO), while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 35 g of graphene nanoparticles (surface area 500 m 2 / g and G / D ratio of 1.0) were added to the solution. The peristaltic pump was adjusted to 130 rpm, and the ball mill was set to a rotation speed of 3900 rpm. The dispersion was treated for 120 minutes (1.0 kWh of energy was introduced). The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d90 value of 86 nm.
[0341] Preparation of nanoparticle composition as a comparative example
[0342] Comparative Example Dispersion CE1:
[0343] A ball mill apparatus (Netzsch laboratory mill micro series) was preloaded with 230.85 g NB3043 oil and 82.4 g P1, while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 35 g of graphene nanoparticles (surface area 700 m 2 / g and G / D ratio of 1.1) were added to the solution. The peristaltic pump was adjusted to 130 rpm, and the ball mill was set to a rotation speed of 3900 rpm. The dispersion was treated for 120 minutes (1.0 kWh of energy was introduced). The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d90 value of 98 nm.
[0344] Comparative Example Dispersion CE2:
[0345] 2g of graphene nanoparticles (surface area 700m 2 / g and G / D ratio of 1.1) was added to a solution of 16g NB3043 and 2g silane (Dynasylan OCTMO), while the mixture was treated with ultrasound (ultrasonic processor UP400S, using 400 watts, 24kHz, using Ti-ultrasonic generator). After 4 minutes of treatment, the mixture became noticeably thicker. The ultrasonic treatment had to be stopped. The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d90 value of 552nm.
[0346] Comparative Example Dispersion CE3:
[0347] 1g of graphene nanoparticles (surface area 700m 2 / g and G / D ratio of 1.1) was added to a solution of 18 g NB3043 and 1 g silane (Dynasylan OCTMO) while the mixture was treated with ultrasound (ultrasonic processor UP400S, using 400 watts, 24 kHz, using a Ti-ultrasonic generator). The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d90 value of 494 nm.
[0348] Comparative Example Dispersion CE4:
[0349] 2g of graphene nanoparticles (surface area 700m2 / g and G / D ratio of 1.1) was added to a solution of 13.3 g NB3043 and 4.7 g P1, while the mixture was treated with ultrasound (ultrasonic processor UP400S, using 400 watts, 24 kHz, using a Ti-ultrasonic generator) for 60 minutes. The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d90 value of 93 nm.
[0350] Comparative Example Dispersion CE5:
[0351] 2g of graphene nanoparticles (surface area 700m 2 / g and G / D ratio of 1.1) was added to a solution of 14.6 g NB3043, 3.3 g P1 and 0.1 g silane (Dynasylan OCTMO), while the mixture was treated with ultrasound (ultrasonic processor UP400S, using 400 watts, 24 kHz, using a Ti-ultrasonic generator) for 60 minutes. The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d90 value of 93 nm.
[0352] Comparative Example Dispersion CE6:
[0353] A ball mill apparatus (Netzsch laboratory mill micro series) was preloaded with 280 g NB3043 oil and 35 g P2, while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 35 g of graphene nanoparticles (surface area 700 m 2 / g and G / D ratio of 1.1) were added to the solution. The peristaltic pump was adjusted to 130 rpm, and the ball mill was set to a rotation speed of 3900 rpm. (1.0 kWh of energy was introduced). The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d90 value of 573 nm.
[0354] Comparative Example Dispersion CE7:
[0355] A ball mill apparatus (Netzsch laboratory mill micro series) was preloaded with 230.85 g NB3043 oil and 82.4 g P1 and 1.75 g silane (Dynasylan Si 69), while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 35 g of graphene nanoparticles (surface area 700 m 2 / g and G / D ratio of 1.1) were added to the solution. The peristaltic pump was adjusted to 130 rpm, and the ball mill was set to a rotation speed of 3900 rpm. The dispersion was treated for 120 minutes (1.0 kWh of energy was introduced). The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d90 value of 76 nm.
[0356] Comparative Example Dispersion CE8:
[0357] The ball mill apparatus (Netzsch laboratory mill micro series) was pre-loaded with 230.85 g NB3043 oil and 82.4 g P1 and 1.75 g silane (Dynasylan OCTMO), while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 35 g of graphene nanoparticles (surface area 170 m 2 / g and G / D ratio of 2.8) were added to the solution. The peristaltic pump was adjusted to 130 rpm, and the ball mill was set to a rotation speed of 3900 rpm. After 120 minutes of treatment, the mixture showed extreme thickening. (1.0 kWh of energy was introduced). The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d90 value of 1267 nm.
[0358] Comparative dispersion CE9:
[0359] The ball mill apparatus (Netzsch laboratory mill micro series) was pre-loaded with 230.85 g NB3043 oil and 82.4 g P1 and 1.75 g silane (Dynasylan OCTMO), while the peristaltic pump was set to 90 rpm and the ball mill was set to 1000 rpm. Then, 35 g of graphene nanoparticles (surface area 110 m 2 / g and G / D ratio of 2.6) were added to the solution. The peristaltic pump was adjusted to 130 rpm, and the ball mill was set to a rotation speed of 3900 rpm. After 120 minutes of treatment, the mixture showed extreme thickening. (1.0 kWh of energy was introduced). The particle size distribution (measured using a dynamic light scattering device, LB-500, from Horiba Ltd., Japan, in Tegosoft DEC oil) showed a d90 value of 1807 nm.
[0360] Table 5 below summarizes inventive nanoparticle compositions according to the invention (inventive dispersions IE1 to IE11) and comparative nanoparticle compositions (comparative dispersions C1 to C9). The weight percentages listed are based on the total weight of the respective nanoparticle composition.
[0361]
[0362] Dynamic Light Scattering (DLS)
[0363] The particle size distribution was measured using a dynamic light scattering apparatus LB-500 manufactured by Horiba Ltd. in TegosoftDEC oil.
[0364] Dynamic light scattering (DLS) is a technique in physics that can be used to determine the size distribution curve of small particles in suspension or polymers in solution. This equipment can be used to measure the particle size of dispersed materials in the range of 3nm to 6μm. The measurement is based on the Brownian motion of particles in the medium and the scattering of incident laser light due to the difference in refractive index of liquid and solid materials.
[0365] The value obtained is the hydrodynamic diameter of the corresponding sphere of the particle. v 50, d v 90 and d v 99 are commonly used standards for discussion because they describe the hydrodynamic diameter of the particles below which 50%, 90% or 99% of the particles within the particle size distribution are below this diameter. The lower these values, the better the particle dispersion. Monitoring these values can give clues about the stability of the particle dispersion. If the values increase significantly, the particles are not sufficiently stabilized and may tend to agglomerate and settle over time, resulting in a lack of stability. Depending on the viscosity of the medium, it can be stated that a d90 value of <200 nm (e.g., for Nexbase base oil) is an indication of a stable dispersion when the particles remain suspended over time.
[0366] Stability testing was performed on Example IE1, Example IE7 and Example IE9 of Table 5, where these were characterized by measuring particle size distribution using the DLS method described previously. This was done after preparation, one week later and four weeks later, respectively, as shown in Table 6 below.
[0367] Table 6: DLS values over time for selected examples.
[0368]
[0369] The results of Table 6 demonstrate the excellent stability of the nanoparticle compositions according to the invention and show that little agglomeration occurs over long periods of time in these dispersions. The particle size values do not increase significantly.
[0370] Over a 4-week time frame, the d v 50, d v 90 and d v The values of 99 are comparable and can be considered to correspond to stable dispersions. In fact, the values remain below the above-mentioned d v 90, and taking into account the accuracy of the measurement method (about 10 relative %), the d90 values of the examples in Table 6 are close to the initial measured values after preparation. As a comparison, it can be mentioned that the dispersion using graphene particles according to the invention but without using polymer compound (B) (Example CE2) leads to DLS values of 484, 552, 581 nm (d90, ... v 50, d v 90,d v 99). These are much higher than the particles dispersed in the dispersion system of the present invention.
[0371] Dispersion stability testing by visual appearance
[0372] According to the present invention, the processing performance of the nanoparticle composition of the present invention is judged by two additional stability tests. Therefore, each sample is diluted to a 0.1 wt % solution of the nanoparticle composition based on the total weight of the different compositions. The dilution is prepared by blending a concentrate selected from the examples of the present invention or the comparative examples in a 10 mL glass vial at room temperature. For example, 0.05 g of the example of the present invention IE1 is mixed with 4.95 g of NB3043 to obtain a 0.1 wt % solution of graphene nanoparticles IE1-1.
[0373] The corresponding dilutions were stored at room temperature. The vials were checked after 1 week and 4 weeks for signs of sedimentation or other instability (e.g., becoming clear). The stability of the dispersion was judged visually by the amount of sedimentation after slowly tilting the vial. Sedimentation is the tendency of particles in suspension to settle out of the fluid in which they are entrained and to rest against obstacles. The adverse effects caused by particle sedimentation are usually dealt with by using a dispersant. The sedimentation behavior is divided into 4 categories: o : no sedimentation (no particles settled at the bottom of the vial); Δ: slight sedimentation (some particles began to settle at the bottom of the vial); +: moderate sedimentation (a thin layer at the bottom of the vial), and +++: almost complete sedimentation (a large number of particles have settled).
[0374] The results obtained are shown in the following Table 7 (Examples of the present invention) and Table 8 (Comparative Examples).
[0375] Dynamic viscosity
[0376] The dynamic viscosity is measured with a Physica MCR 301 from Anton Paar using the rotational viscosity method and a measuring plate PP25, with the distance set to 0.5 mm.
[0377] The motor of the viscometer drives a rotating unit (bob) inside a fixed cup. The rotation speed of the rotating unit is preset, and it generates a specific motor torque required to rotate the measuring rotating unit. This torque must overcome the viscous forces of the measured material and is therefore a measure of its viscosity.
[0378] The data is in 100s -1 The shear rate was measured at 22 °C.
[0379] Dispersion stability testing by monitoring viscosity changes
[0380] The key of the present invention is to prepare a stable, high-filling graphene nanoparticle dispersion. Over time, dispersed particles tend to interact with each other, especially when their surfaces show different polarities compared to the surrounding medium. Additives are used in the dispersion to prevent this interaction. On the one hand, this interaction may lead to agglomeration and sedimentation, which has been evaluated in the previous section. On the other hand, this interaction may lead to the formation of a network in the fluid, which causes the dispersion viscosity to increase significantly.
[0381] In order to investigate the latter behavior, the inventors of the present invention measured the viscosity of the dispersions after 1 and 4 weeks and calculated the change in viscosity. This is the most important test for the present invention. In the comparative example, only the dispersions showing (1) d v Those with a 90 value of less than 200 nm and (2) without strong sedimentation were subjected to this test.
[0382] Viscosity measurements were always carried out with concentrated inventive and comparative examples (10 or 15 wt %) in order to correctly judge the change in viscosity.
[0383] As shown in Table 7 below, the inventors were able to prepare nanoparticle dispersions that showed no significant increase in viscosity after 4 weeks.
[0384] In contrast, the comparative nanoparticle dispersions in Table 8 showed a significant viscosity increase after 4 weeks. Comparative Example CE1 even showed a viscosity increase of more than 50% after only one week.
[0385]
[0386]
[0387] As shown in Tables 7 and 8, the nanoparticle compositions that do not contain any silane compounds do not show good stability over time (see Comparative Examples CE1, CE4 and CE6). This is either because they show strong sedimentation, or because viscosity increases significantly. The nanoparticle dispersions prepared only by ultrasonic treatment do not show good stability either (see Comparative Examples CE2, CE3 and CE4). Although the particle size distribution may be low, strong sedimentation can be seen after 4 weeks. Need to obtain stable nanoparticle compositions according to the present invention by grinding treatment according to the present invention.
[0388] Only the inventive examples according to the invention show the following combination of effects: Particle size (d v 90), good visual stability without any significant amount of sedimentation and no significant increase in viscosity after 4 weeks. Formulations prepared with nanoparticle compositions containing a small amount of silane compound (C) also showed very good dispersion stability without any observed particle sedimentation and no increase in viscosity after 4 weeks (see inventive example IE12, which was prepared with a nanoparticle composition containing 0.05 wt. % of silane compound (C) based on the total weight of the nanoparticle composition). In the case of using other polymers (see comparative example CE6) or graphene nanoparticles that do not meet the definition according to the present invention (see comparative examples CE8 and CE9), excessively high particle sizes (d v 90), or strong sedimentation.
[0389] Light transmittance measurement using a spectrophotometer
[0390] Inventive Example 1 was diluted to 0.005 wt% particle content in NB3043 base oil to allow the light transmittance to be measured using spectroscopy (resulting in a lubricant composition containing 0.05 wt% of IE1). The sample was subjected to light absorption and transmittance measurements using a Perkin Elmer Lambda 950S UV / Vis / NIR spectrophotometer using a 1 cm wide cuvette. The light transmittance at 800 am was recorded after storage for different days.
[0391] Figure 1 These results in show that the composition according to the invention is very stable to dilution and sedimentation over time. In fact, the light transmittance of the sample increased by only about 1% after 28 days of storage (see Figure 1). Compared to the prior art results as disclosed in US Pat. No. 8,703,666 B2, in which the light transmittance increased by about 45% after 28 days of storage, much better processing properties can be achieved with the dispersion according to the invention. This significant improvement in stability enables good and reproducible use in industrial applications.
[0392] Friction reduction rate measured by microtraction tester (MTM)
[0393] The coefficient of friction was measured using a microtraction tester named MTM2 from PCS Instruments according to the test method described in Table 9 below. SRR refers to the slide-to-roll ratio. This parameter was kept constant during the 2 hour test and is defined as (U 球 -U 盘 ) / U, where (U 球 -U 盘 ) represents the sliding velocity and U represents the entrainment velocity, which is given by U = (U 球 +U 盘 The Stribeck curve of each sample was measured according to the scheme in Table 9.
[0394] Table 9 : Scheme for measuring the Stribeck curve.
[0395]
[0396] According to MTM method 1, the friction coefficient of each blend was recorded over the entire speed range and the Stribeck curve was obtained. According to these conditions, the lubricating oil formulations containing the nanoparticle composition IE1 of the present invention listed in Table 10 were subjected to friction testing. The results of the friction testing are disclosed in the following Tables 11 to 13. The weight percentages listed are based on the total weight of the different formulations.
[0397] The fully formulated industrial gear oil (IGO) composition according to ISO VG 68 used in Table 10 comprises
[0398] 79.5% by weight 3060(base oil)
[0399] 18.0 wt% 5-220(base oil)
[0400] 0.7 wt% PPD
[0401] 1.8 wt% RC9420(DI package)
[0402] 0.2 wt% 14-520(defoaming agent).
[0403] Table 10 : Lubricating oil formulation according to the present invention.
[0404]
[0405] In order to express the friction reduction in %, a quantifiable result can be expressed as a number and is obtained by integrating the friction value curve using the corresponding Stribeck curve obtained in the sliding speed range of 5 mm / s-60 mm / s using the trapezoidal rule. The area corresponds to the "total friction" in the selected speed range. The smaller the area, the greater the friction reduction effect of the product being examined. By using a reference oil 3043 value to calculate the friction reduction percentage, the reference oil 3043 produced a friction area of 6.32 mm / s. A positive value indicates a reduction in the coefficient of friction. The values for the reference oils are summarized in Tables 11-13 below.
[0406] Table 11 : Friction reduction of the formulation according to the invention in the boundary state compared to the base oil.
[0407]
[0408] Table 12 : Friction reduction at the borderline state of the formulation according to the invention (topped up with original engine oil 0W-16) compared to original engine oil 0W-16 alone.
[0409] Example Friction area of 5-60mm / s Friction reduction rate, expressed in % Reference 0W-16 engine oil 3.80 0 Formulation 2 2.57 32.3
[0410] Table 13 : Friction reduction at the borderline state for the formulation according to the invention (topped up on the fully formulated industrial gear oil ISO VG 68) compared to a fully formulated industrial gear oil ISO VG 68.
[0411]
[0412] The experimental results show good friction reduction performance compared to the base oil reference. In fact, the results of the total friction calculated in the sliding speed range of 5 mm / s-60 mm / s clearly show that the lubricating oil formulation comprising the nanoparticle composition according to the present invention significantly improves the friction reduction rate.
[0413] Determination of wear reduction in the 4-ball wear test according to DIN 51315-2
[0414] The same lubricant formulation 1 used for the friction test showed a diameter of 0.496 mm for the callotes on the state ball. Compared to 3043 oil, the graphene dispersion reduced wear by 41.2%.
[0415] The tribological results show that the graphene composition of the present invention not only has good anti-friction process properties, but also has very good anti-wear properties due to the high stability of the dispersion over a long period of time.
[0416] It has been found that the nanoparticle compositions of the present invention can contain high concentrations of graphene particles (even at 10 wt. % concentration) without any stability problems (agglomeration or viscosity increase in oil) while maintaining good friction and wear reduction properties. Graphene nanoparticles having BET and G / D ratios both within the ranges defined in claim 1 outperform any other tested graphene nanoparticles that do not meet the BET and G / D ratio requirements of the present invention in terms of dispersion stability. In fact, graphene nanoparticles that do not meet the BET and G / D ratio requirements of the present invention lead to viscosity increase and sedimentation when dispersed in oil (Comparative Dispersion Examples C8 and C9).
Claims
1. A nanoparticle composition comprising one or more graphene nanoparticles (A), one or more polymers (B), one or more silane compounds (C) and one or more base fluids (D), wherein (A) The one or more nanoparticles (A) are multilayer graphene-based materials containing oxygen groups, which have a carbonyl group at 200 m 2 / g to 1,500m 2 / g and a G / D ratio between 0.5 and 2, (B) The one or more polymers (B) are obtained by polymerizing the following monomer composition, wherein the monomer composition comprises: a) 1 to 30 wt % of one or more functional monomers, based on the total weight of the monomer composition, selected from: a1) Aminoalkyl (meth)acrylates and aminoalkyl (meth)acrylamides; a2) alkyl(meth)acrylic nitriles and other nitrogen-containing alkyl(meth)acrylates; a3) (meth)acrylates of ether alcohols; a4) epoxyalkyl alkyl (meth)acrylate; a5) phosphorus-, boron- and / or silicon-containing alkyl (meth)acrylates; a6) Heterocycloalkyl (meth)acrylate; a7) vinyl halides; a8) vinyl esters; a9) vinyl monomers containing aromatic groups; a10) heterocyclic vinyl compounds; a11) vinyl and prenyl ethers; a12) methacrylic acid and acrylic acid, and b) 30 to 70 wt % of one or more alkyl (meth)acrylate monomers, based on the total weight of the monomer composition, wherein each of the alkyl groups of the one or more alkyl (meth)acrylate monomers is independently linear, cyclic or branched, and contains from 1 to 40 carbon atoms, and c) 20 to 60 wt % based on the total weight of the monomer composition of one or more monomers having a number average molecular weight (M) of 500 to 10,000 g / mol. n ) based on polybutadiene macromonomers, (C) 0.02 to 5 wt. % of one or more silane compounds (C) having formula (IV) based on the total weight of the nanoparticle composition Si(R)(M) h(X) 3-h (IV) Where 0≤h≤2; M is a branched or straight-chain C1 to C4 alkyl group, R is a branched or straight chain aliphatic, aromatic or mixed aliphatic-aromatic C1 to C 30 A carbonyl group, or R is a branched or straight-chain aliphatic, aromatic or mixed aliphatic-aromatic C1 to C 30 A carbonyl group, wherein the functional group is selected from carboxyl, carbonyl, hydroperoxycarbonyl, cyano, formyl, oxo, thio, hydroxyl, amino, imino, hydrazine, and epoxy; X is selected from H, Cl or a group OY, wherein Y is H or a C1 to C8 branched or linear alkyl, alkenyl, aryl or aralkyl group, a branched or linear C2 to C8 alkyl ether group or a mixture thereof, The nanoparticle composition is obtained by grinding the nanoparticle composition.
2. The nanoparticle composition according to claim 1, wherein the nanoparticle composition is obtained by a ball milling process.
3. The nanoparticle composition according to claim 1, wherein R in formula (IV) is selected from a linear aliphatic C8 carbonyl group, a linear aliphatic C 16 A carbonyl group, a straight-chain aliphatic 3-aminopropyl group or a 3-glycidyloxypropyl group.
4. The nanoparticle composition according to claim 1, wherein X in formula (IV) is methoxy or ethoxy.
5. The nanoparticle composition of claim 1, wherein the one or more polybutadiene-based macromonomers c) have a number average molecular weight (M) of 1,500 to 7,500 g / mol. n ).
6. The nanoparticle composition of claim 1, wherein the one or more polymers (B) have a weight average molecular weight (MW) of 10,000 to 1,000,000 g / mol. w ).
7. The nanoparticle composition according to any one of claims 1 to 6, wherein the one or more polymers (B) are obtained by polymerizing the following monomer composition, the monomer composition comprising: a) 1 to 30 wt. % of the one or more functional monomers as component a), based on the total weight of the monomer composition; and b1) as first component b) 30 to 60% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (I); Where R is hydrogen or methyl, R 1 refers to a straight-chain, branched or cyclic alkyl group having 1 to 8 carbon atoms; and b2) from 0 to 20% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (II) as second component b): Where R is hydrogen or methyl, R 2 refers to a straight-chain, branched or cyclic alkyl group having 9 to 15 carbon atoms; and b3) from 0 to 20% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (III) as third component b): Where R is hydrogen or methyl, R 3 refers to a straight-chain, branched or cyclic alkyl group having 16 to 40 carbon atoms; and c) 20 to 60 wt % based on the total weight of the monomer composition of one or more monomers having a number average molecular weight (M) of 500 to 10,000 g / mol. n ) based polybutadiene macromonomer.
8. The nanoparticle composition according to claim 7, wherein the one or more polymers (B) are obtained by polymerizing the following monomer composition, the monomer composition comprising: a) 10 to 20 wt % of the one or more functional monomers as component a), based on the total weight of the monomer composition; and b1) as first component b) 35 to 50% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (I); Where R is hydrogen or methyl, R 1 refers to a straight-chain, branched or cyclic alkyl group having 1 to 8 carbon atoms; and b2) from 1 to 10% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (II) as second component b): Where R is hydrogen or methyl, R 2 refers to a straight-chain, branched or cyclic alkyl group having 9 to 15 carbon atoms; and b3) 0 to 10% by weight, based on the total weight of the monomer composition, of one or more alkyl (meth)acrylates of the formula (III) as third component b): Where R is hydrogen or methyl, R 3 refers to a straight-chain, branched or cyclic alkyl group having 16 to 40 carbon atoms; and c) 30 to 50 wt % of one or more monomers having a number average molecular weight (M) of 500 to 10,000 g / mol, based on the total weight of the monomer composition. n ) based polybutadiene macromonomer.
9. The nanoparticle composition according to any one of claims 1 to 6, wherein the one or more polymer compounds (B) are obtained by polymerizing the following monomer composition, the monomer composition comprising: a1) as first component a) 0.5 to 5% by weight of aminoalkyl(meth)acrylamide, based on the total weight of the monomer composition; a9) 5 to 15% by weight, based on the total weight of the monomer composition, of a vinyl monomer containing an aromatic group as the second component a); b1) 35 to 50 wt. % of an alkyl (meth)acrylate monomer of formula (I), based on the total weight of the monomer composition, as a first component b); b2) 1 to 10% by weight, based on the total weight of the monomer composition, of an alkyl (meth)acrylate monomer of the formula (II) as a second component b); c) 30 to 50 wt % of the following, based on the total weight of the monomer composition, as component c): one or more monomers having a number average molecular weight (M) of 500 to 10,000 g / mol; n ) based polybutadiene macromonomer.
10. The nanoparticle composition of claim 9, wherein the monomer composition comprises: a1) 0.5 to 5% by weight, based on the total weight of the monomer composition, of N-(3-dimethylaminopropyl)methacrylamide as first component a); a9) 5 to 15% by weight of styrene, based on the total weight of the monomer composition, as second component a); b1) 35 to 50% by weight, based on the total weight of the monomer composition, of methyl methacrylate and / or butyl methacrylate as first component b); b2) 1 to 10% by weight, based on the total weight of the monomer composition, of lauryl methacrylate as second component b); c) 30 to 50 wt. % of the following as component c), based on the total weight of the monomer composition: one or more polybutadiene-based macromonomers derived from esters of (meth)acrylic acid and having a number average molecular weight (M) of 1,500 to 5,500 g / mol; n ) of the hydroxylated hydrogenated polybutadiene.
11. The nanoparticle composition according to any one of claims 1 to 6, wherein the weight contents of the monomers a), b) and c) of the monomer composition total 100 wt%, based on the total weight of the monomer composition.
12. The nanoparticle composition according to any one of claims 1 to 6, wherein the one or more silane compounds (C) of formula (IV) are octyltrimethoxysilane, hexadecyltrimethoxysilane, 3-aminopropyltriethoxysilane or 3-glycidoxypropyltriethoxysilane.
13. The nanoparticle composition of any one of claims 1 to 6, wherein the nanoparticle composition comprises, based on the total weight of the nanoparticle composition: 1 to 20% by weight of one or more nanoparticles (A), 0.5 to 30% by weight of one or more polymers (B), 0.02 to 5% by weight of one or more silane compounds (C), 45 to 98.48 wt. % of one or more base fluids (D).
14. The nanoparticle composition according to claim 13, wherein the weight contents of components A), B), C) and D) total 100 weight % based on the total weight of the nanoparticle composition.
15. A method for preparing a nanoparticle composition as defined in any one of claims 1 to 14, wherein the method comprises the following steps: (i) providing one or more nanoparticle compounds (A) as defined herein; (ii) providing one or more polymer compounds (B) as defined herein; (iii) providing one or more silane compounds (C) as defined herein; (iv) providing one or more base fluids (D) as defined herein; (v) combining (A) to (D) to obtain a mixture; and (vi) grinding the mixture of step (v).
16. The method according to claim 15, wherein in step (v), the compounds (A) and (C) are first mixed together by jet or ball milling and then mixed with (B) and (D).
17. A lubricating oil composition comprising the nanoparticle composition defined in any one of claims 1 to 14 and one or more base fluids (E).
18. The lubricating oil composition according to claim 17, wherein the lubricating oil composition further comprises one or more additive components (F) selected from antioxidants, antiwear additives, pour point depressants, corrosion inhibitors, metal deactivators or electrostatic discharge inhibitors, defoamers, seal fixatives or seal compatibility agents or mixtures thereof.
19. The lubricating oil composition according to claim 17 or 18, wherein the lubricating oil composition comprises 50 to 99.99 wt. % of a base oil (E), 0.01 to 50 wt. % of a nanoparticle composition, and 0 to 20 wt. % of one or more additive components (F), based on the total weight of the lubricating oil composition.
20. Use of the nanoparticle composition defined in any one of claims 1 to 14 as a lubricant additive in a lubricating oil composition, or use as a lubricant additive in a lubricating grease.
21. The use according to claim 20, wherein the nanoparticle composition is used as a lubricant additive in a gear oil composition, a transmission oil composition, a hydraulic oil composition, an engine oil composition or a marine oil composition.
22. The use according to claim 20, wherein the nanoparticle composition is used as a lubricant additive in an industrial lubricating oil composition.
Citation Information
Patent Citations
Lubricating oil with graphene
CN107384520A
Polymer functional graphene and preparation method and application thereof
CN107758652A
Serpentine / functionalized graphene lubricating oil additive as well as preparation method and application thereof
CN108102763A
Lubricating base oil preparation process
EP0668342A1
Process for producing lubricating base oils
EP0776959A2