A preparation method of graphene toughening agent and its application in nylon material
Through the preparation method of graphene toughening agent, combined with nylon materials for melt blending, the problem of insufficient notch impact toughness of nylon materials is solved, and its toughness and mechanical properties are significantly improved.
Patent Information
- Application Number
- CN202310223747.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-09
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-03-09
AI Technical Summary
The notch impact toughness of nylon materials is low, and it is difficult for the prior art to effectively improve its toughness, tensile strength and bending strength.
Using the preparation method of graphene toughening agent, the preparation of grafted graphene oxide toughening agent by epoxidizing polyolefin thermoplastic elastomer, polyhydroxy polyolefin thermoplastic elastomer and polyolefin thermoplastic elastomer is combined with nylon material for melting and consolidation. Mixed granulation to enhance the toughness and mechanical properties of the material.
The elongation of break, tensile strength, bending strength and notch impact strength of nylon materials are significantly improved, and the toughness and mechanical properties of the material are enhanced.
Smart Images

Figure CN116199900B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nylon materials, and in particular to a preparation method of a graphene toughening agent and application of the same in nylon materials. Background Art
[0002] Polyamide, commonly known as nylon material, is a general term for thermoplastic resins containing repeated amide groups on the main chain of the molecule. Nylon has good mechanical properties, electrical insulation, heat resistance, wear resistance, corrosion resistance, and good processing properties. Therefore, it is widely used in the automotive, home appliance, clothing, packaging and other industries. However, as a pseudo-tough plastic, nylon itself has good toughness, but has low notch impact toughness. For example, the patent "A Graphene-modified Nylon 66 / Nylon 6 Fiber and Its Preparation and Application" with the authorization announcement number CN110093679B discloses a graphene-modified nylon 66 / nylon 6 fiber and its preparation and application. In-situ reduction polymerization is used to prepare a high-concentration nylon 6 / graphene low molecular weight composite material, which is then added to the PA66 polymerization system. Graphene-modified nylon 66 and nylon 6 slices are prepared by in-situ polymerization and copolymerization, and melt spinning is performed to prepare PA66 / PA6 fibers with uniform dispersion and good mechanical properties.
[0003] Polyolefin thermoplastic elastomer (POE) is a high-performance polyolefin product with excellent properties such as large bending degree, high low-temperature impact resistance, easy processing, and reusability. It is often used in the automotive industry, wire and cable fields, hoses, etc. to make products with environmental resistance, high heat resistance, and good impact resistance. Graphene has excellent optical, electrical, and mechanical properties, and has important application prospects in the fields of materials science, energy, biomedicine, and drug delivery. For example, the document "The Effect of Graphene Dispersibility on Graphene / Nylon 6 Properties" discloses that graphene / PA6 composites with different degrees of dispersion were prepared by water-assisted melt twin-screw extrusion. The results show that the good dispersion of graphene in the matrix makes the composite material have higher thermal stability and mechanical properties. A new type of graphene toughening agent prepared by the present invention improves the properties of nylon materials such as elongation at break, tensile strength, and flexural strength. Summary of the invention
[0004] 1. Technical issues to be resolved
[0005] In view of the deficiencies in the prior art, the present invention provides a method for preparing a graphene toughening agent and its application in nylon materials, and proposes a method for preparing a new toughening agent, which enhances the toughness, tensile strength, flexural strength and other properties of nylon.
[0006] (II) Technical solution
[0007] A method for preparing a graphene toughening agent:
[0008] (1) Preparation of epoxidized polyolefin thermoplastic elastomer
[0009] At 130-180° C., polyolefin thermoplastic elastomer (POE), glycidyl methacrylate, and dicumyl peroxide are sequentially added into a torque rheometer for melt grafting reaction for 6-10 minutes, and then the obtained product is placed in a flask filled with xylene solution, condensed and refluxed at 130-140° C. for 2-4 hours, filtered, washed with acetone, and vacuum dried to obtain an epoxidized polyolefin thermoplastic elastomer;
[0010] (2) Preparation of polyhydroxy polyolefin thermoplastic elastomer
[0011] At 20-35° C., adding epoxidized polyolefin thermoplastic elastomer, tetrahydrofuran, and sulfuric acid with a concentration of 60-80% into a flask for reaction for 2-4 hours, washing and separating with deionized water to obtain a polyhydroxy polyolefin thermoplastic elastomer;
[0012] (3) Preparation of polyolefin thermoplastic elastomer grafted with graphene oxide toughening agent
[0013] At 50-60° C., a polyhydroxy polyolefin thermoplastic elastomer is placed in a flask containing dimethyl sulfoxide, and graphene oxide, dicyclohexylcarbodiimide and dimethylaminopyridine are added thereto, and the mixture is stirred for reaction for 3-5 hours, and then washed with deionized water and separated to obtain a polyolefin thermoplastic elastomer grafted with graphene toughening agent;
[0014] Preferably, in step (1), the mass ratio of polyolefin thermoplastic elastomer, glycidyl methacrylate and dicumyl peroxide is 1:0.04-0.06:0.07-0.09.
[0015] Preferably, in step (3), the mass ratio of graphene oxide, polyhydroxy polyolefin thermoplastic elastomer, dicyclohexylcarbodiimide and dimethylaminopyridine is 5-20:1:2-10:0.3-1.5.
[0016] Preferably, the nylon material is placed in a drying oven at 100-110° C. and dried for 8-12 hours, and then a polyolefin thermoplastic elastomer grafted graphene toughening agent and an antioxidant are added thereto, stirred and mixed, and melt-blended and granulated through a twin-screw extruder to obtain a nylon material with a new toughening agent.
[0017] Preferably, in the step, the mass ratio of nylon material, polyolefin thermoplastic elastomer grafted graphene toughening agent, and antioxidant is 1:0.05-0.3:0.002-0.005.
[0018] Preferably, the extrusion process parameters in the step are: processing temperature is 200-260°C, screw speed is 100-150r / min, material temperature is 250-260°C, and main feed speed is 10-20r / min.
[0019] (III) Beneficial technical effects
[0020] The polyolefin thermoplastic elastomer is melt-grafted with glycidyl methacrylate to obtain an epoxidized polyolefin thermoplastic elastomer, which is then subjected to a sulfuric acid oxidation ring-opening reaction to obtain a polyhydroxyl polyolefin thermoplastic elastomer, thereby introducing abundant hydroxyl groups into the side chains of the polyolefin thermoplastic elastomer, which is then subjected to an esterification reaction with the carboxyl group of graphene oxide to obtain a novel polyolefin thermoplastic elastomer grafted graphene toughening agent. The polyolefin thermoplastic elastomer grafted graphene toughening agent is melt-blended and granulated with nylon material. After the graphene is grafted with the polyolefin thermoplastic elastomer, the compatibility and interaction between the graphene and the nylon interface are stronger, and the graphene is evenly dispersed in the nylon material. When the material is strained or impacted, many fine cracks will be generated inside the nylon material. The polyolefin thermoplastic elastomer grafted graphene toughening agent absorbs a large amount of energy, avoids stress concentration and cracks, and prevents the cracks from further expanding, thereby enhancing the toughness, tensile strength, bending strength and other properties of the nylon material. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a route for the preparation of polyhydroxy polyolefin thermoplastic elastomers DETAILED DESCRIPTION
[0022] Example 1
[0023] (1) Preparation of epoxidized polyolefin thermoplastic elastomer
[0024] At 150°C, 100 g of polyolefin thermoplastic elastomer, 5 g of glycidyl methacrylate and 8 g of diisopropylbenzene peroxide were sequentially added into a torque rheometer for melt grafting reaction for 8 minutes. The obtained product was then placed in a flask filled with xylene solution, condensed and refluxed at 135°C for 3 hours, filtered, washed with acetone, and vacuum dried to obtain an epoxidized polyolefin thermoplastic elastomer.
[0025] (2) Preparation of polyhydroxy polyolefin thermoplastic elastomer
[0026] At 20° C., 5 g of epoxidized polyolefin thermoplastic elastomer, 200 mL of tetrahydrofuran, and 5 mL of 60% sulfuric acid were added into a flask and reacted for 2 h. The mixture was washed and separated with deionized water to obtain a polyhydroxy polyolefin thermoplastic elastomer.
[0027] (3) Preparation of polyolefin thermoplastic elastomer grafted with graphene oxide toughening agent
[0028] At 50°C, 10 g of a polyhydroxy polyolefin thermoplastic elastomer was placed in a flask filled with dimethyl sulfoxide, and then 2 g of graphene oxide, 4 g of dicyclohexylcarbodiimide, and 0.6 g of dimethylaminopyridine were added thereto. The mixture was stirred for reaction for 3 h, washed with deionized water, and separated to obtain a polyolefin thermoplastic elastomer grafted with graphene toughening agent.
[0029] (4) Preparation of toughened nylon materials
[0030] At 105°C, 20g of nylon material was placed in a drying oven and dried for 10 hours. Then, 1g of polyolefin thermoplastic elastomer grafted graphene toughening agent and 0.04g of antioxidant were added thereto, stirred and mixed, and melt-blended and granulated by a twin-screw extruder at a processing temperature of 230°C, wherein the screw speed was 150r / min, the material temperature was 250°C, and the main feed speed was 15r / min, to obtain the toughened nylon material.
[0031] Example 2
[0032] (1) Preparation of epoxidized polyolefin thermoplastic elastomer
[0033] At 130°C, 100 g of polyolefin thermoplastic elastomer, 5 g of glycidyl methacrylate and 8 g of diisopropylbenzene peroxide were sequentially added into a torque rheometer for melt grafting reaction for 8 minutes. The obtained product was then placed in a flask filled with xylene solution, condensed and refluxed at 130°C for 4 hours, filtered, washed with acetone, and vacuum dried to obtain an epoxidized polyolefin thermoplastic elastomer.
[0034] (2) Preparation of polyhydroxy polyolefin thermoplastic elastomer
[0035] At 20° C., 5 g of epoxidized polyolefin thermoplastic elastomer, 150 mL of tetrahydrofuran, and 5 mL of 75% sulfuric acid were added into a flask and reacted for 2 h. The mixture was washed and separated with deionized water to obtain a polyhydroxy polyolefin thermoplastic elastomer.
[0036] (3) Preparation of polyolefin thermoplastic elastomer grafted with graphene oxide toughening agent
[0037] At 55°C, 15 g of a polyhydroxy polyolefin thermoplastic elastomer was placed in a flask filled with dimethyl sulfoxide, and then 2 g of graphene oxide, 20 g of dicyclohexylcarbodiimide, and 3 g of dimethylaminopyridine were added thereto. The mixture was stirred for reaction for 4 hours, washed with deionized water, and separated to obtain a polyolefin thermoplastic elastomer grafted with graphene toughening agent.
[0038] (4) Preparation of toughened nylon materials
[0039] At 100°C, 20g of nylon material was placed in a drying oven and dried for 8h, and then 2g of polyolefin thermoplastic elastomer grafted graphene toughening agent and 0.04g of antioxidant were added thereto, stirred and mixed, and melt blended and granulated at a processing temperature of 200°C through a twin-screw extruder, wherein the screw speed was 100r / min, the material temperature was 250°C, and the main feed speed was 10r / min, to obtain the toughened nylon material.
[0040] Example 3
[0041] (1) Preparation of epoxidized polyolefin thermoplastic elastomer
[0042] At 130°C, 100 g of polyolefin thermoplastic elastomer, 4 g of glycidyl methacrylate and 7 g of diisopropylbenzene peroxide were sequentially added into a torque rheometer for melt grafting reaction for 6 minutes. The obtained product was then placed in a flask filled with xylene solution, condensed and refluxed at 130°C for 2 hours, filtered, washed with acetone, and vacuum dried to obtain an epoxidized polyolefin thermoplastic elastomer.
[0043] (2) Preparation of polyhydroxy polyolefin thermoplastic elastomer
[0044] At 20° C., 5 g of epoxidized polyolefin thermoplastic elastomer, 200 mL of tetrahydrofuran, and 10 mL of 80% sulfuric acid were added into a flask and reacted for 2 h. The mixture was washed and separated with deionized water to obtain a polyhydroxy polyolefin thermoplastic elastomer.
[0045] (3) Preparation of polyolefin thermoplastic elastomer grafted with graphene oxide toughening agent
[0046] At 50°C, 15 g of a polyhydroxy polyolefin thermoplastic elastomer was placed in a flask filled with dimethyl sulfoxide, and then 2 g of graphene oxide, 20 g of dicyclohexylcarbodiimide, and 0.6 g of dimethylaminopyridine were added thereto. The mixture was stirred for reaction for 4 hours, washed with deionized water, and separated to obtain a polyolefin thermoplastic elastomer grafted with graphene toughening agent.
[0047] (4) Preparation of toughened nylon materials
[0048] At 110°C, 20g of nylon material was placed in a drying oven and dried for 10 hours. Then, 3g of polyolefin thermoplastic elastomer grafted graphene toughening agent and 0.04g of antioxidant were added thereto, and the mixture was stirred and mixed. At a processing temperature of 230°C, the mixture was melt-blended and granulated through a twin-screw extruder, wherein the screw speed was 120r / min, the material temperature was 255°C, and the main feed speed was 15r / min, to obtain the toughened nylon material.
[0049] Example 4
[0050] (1) Preparation of epoxidized polyolefin thermoplastic elastomer
[0051] At 180°C, 100 g of polyolefin thermoplastic elastomer, 5 g of glycidyl methacrylate and 9 g of diisopropylbenzene peroxide were sequentially added into a torque rheometer for melt grafting reaction for 6 minutes. The obtained product was then placed in a flask filled with xylene solution, condensed and refluxed at 130°C for 3 hours, filtered, washed with acetone, and vacuum dried to obtain an epoxidized polyolefin thermoplastic elastomer.
[0052] (2) Preparation of polyhydroxy polyolefin thermoplastic elastomer
[0053] At 20° C., 5 g of epoxidized polyolefin thermoplastic elastomer, 100 mL of tetrahydrofuran, and 5 mL of 80% sulfuric acid were added into a flask and reacted for 2 h. The mixture was washed and separated with deionized water to obtain a polyhydroxy polyolefin thermoplastic elastomer.
[0054] (3) Preparation of polyolefin thermoplastic elastomer grafted with graphene oxide toughening agent
[0055] At 60°C, 20 g of a polyhydroxy polyolefin thermoplastic elastomer was placed in a flask filled with dimethyl sulfoxide, and then 2 g of graphene oxide, 20 g of dicyclohexylcarbodiimide, and 3 g of dimethylaminopyridine were added thereto. The mixture was stirred for reaction for 5 h, washed with deionized water, and separated to obtain a polyolefin thermoplastic elastomer grafted with graphene toughening agent.
[0056] (4) Preparation of toughened nylon materials
[0057] At 110°C, 20g of nylon material was placed in a drying oven and dried for 12h, and then 4g of polyolefin thermoplastic elastomer grafted graphene toughening agent and 0.1g of antioxidant were added thereto, stirred and mixed, and melt blended and granulated by a twin-screw extruder at a processing temperature of 260°C, wherein the screw speed was 150r / min, the material temperature was 260°C, and the main feed speed was 20r / min, to obtain the preparation of toughened nylon material.
[0058] Example 5
[0059] (1) Preparation of epoxidized polyolefin thermoplastic elastomer
[0060] At 180°C, 100 g of polyolefin thermoplastic elastomer, 6 g of glycidyl methacrylate and 9 g of diisopropylbenzene peroxide were sequentially added into a torque rheometer for melt grafting reaction. The reaction time was 10 min. The obtained product was placed in a flask filled with xylene solution, condensed and refluxed at 140°C for 4 h, filtered, washed with acetone and dried in vacuo to obtain an epoxidized polyolefin thermoplastic elastomer.
[0061] (2) Preparation of polyhydroxy polyolefin thermoplastic elastomer
[0062] At 20° C., 5 g of epoxidized polyolefin thermoplastic elastomer, 200 mL of tetrahydrofuran, and 10 mL of 80% sulfuric acid were added into a flask and reacted for 2 h. The mixture was washed and separated with deionized water to obtain a polyhydroxy polyolefin thermoplastic elastomer.
[0063] (3) Preparation of polyolefin thermoplastic elastomer grafted with graphene oxide toughening agent
[0064] At 50°C, 20 g of a polyhydroxy polyolefin thermoplastic elastomer was placed in a flask filled with dimethyl sulfoxide, and then 2 g of graphene oxide, 4 g of dicyclohexylcarbodiimide, and 3 g of dimethylaminopyridine were added thereto. The mixture was stirred for reaction for 4 hours, washed with deionized water, and separated to obtain a polyolefin thermoplastic elastomer grafted with graphene toughening agent.
[0065] (4) Preparation of toughened nylon materials
[0066] At 105°C, 20g of nylon material was placed in a drying oven and dried for 10 hours. Then, 6g of polyolefin thermoplastic elastomer grafted graphene toughening agent and 0.04g of antioxidant were added thereto, stirred and mixed, and melt-blended and granulated by a twin-screw extruder at a processing temperature of 230°C, wherein the screw speed was 100r / min, the material temperature was 260°C, and the main feed speed was 10r / min to obtain the toughened nylon material.
[0067] The elongation at break was tested according to GB / T14344-2008.
[0068] The tensile strength was tested according to GB / T1040-2006.
[0069] The bending strength is tested according to GB / T9341-2008.
[0070] The notched impact strength is tested according to GB / T1043.1-2008.
[0071]
[0072] The elongation at break of Example 1 is the largest, reaching 23.1%. The tensile strength of Example 2 is the largest, reaching 75.6 MPa. The bending strength of Example 1 is the largest, reaching 90.6 MPa. The notched impact strength of Example 4 is the largest, reaching 38.2 kJ / m 2 .
Claims
1. The application of graphene toughening agent in improving the notched impact strength of nylon material is characterized by: The application steps are: drying 20g of nylon material at 110°C for 12h, adding 4g of graphene toughening agent and 0.1g of antioxidant thereto, stirring and mixing, and melt blending and granulating through a twin-screw extruder at a processing temperature of 260°C, wherein the screw speed is 150r / min, the material temperature is 260°C, and the main feed speed is 20r / min; The preparation method of the graphene toughening agent is: (1) Preparation of epoxidized polyolefin thermoplastic elastomer: At 180° C., 100 g of polyolefin thermoplastic elastomer, 5 g of glycidyl methacrylate, and 9 g of dicumyl peroxide were sequentially added into a torque rheometer for melt grafting reaction, and the reaction lasted for 6 min. The obtained product was then placed in a flask filled with a xylene solution, condensed and refluxed at 130° C. for 3 h, filtered, washed with acetone, and vacuum dried to obtain an epoxidized polyolefin thermoplastic elastomer. (2) Preparation of polyhydroxy polyolefin thermoplastic elastomer: At 20° C., 5 g of epoxidized polyolefin thermoplastic elastomer, 100 mL of tetrahydrofuran, and 5 mL of 80% sulfuric acid were added into a flask and reacted for 2 h, and then washed and separated with deionized water to obtain a polyhydroxy polyolefin thermoplastic elastomer; (3) Preparation of graphene toughening agent: At 60°C, 20 g of polyhydroxy polyolefin thermoplastic elastomer was placed in a flask filled with dimethyl sulfoxide, and then 2 g of graphene oxide, 20 g of dicyclohexylcarbodiimide and 3 g of dimethylaminopyridine were added thereto. The mixture was stirred for reaction for 5 h, washed with deionized water, and separated to obtain a graphene toughening agent.