A PET composition and its preparation method and application

By adding a specially formulated composition to the PET material, including oxidized polyethylene wax, isopropoxy distearoyloxyaluminate and modified glass fiber, the color difference changes and mechanical property degradation of the PET material at high temperatures are solved. solve the problem and achieve the maintenance of color stability and mechanical properties after continuous baking for 1000 hours at 210°C.

CN116200013BActive Publication Date: 2024-10-18KINGFA SCI & TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310160559.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-02-24
Publication Date
2024-10-18
Estimated Expiration
2043-02-24

AI Technical Summary

Technical Problem

The color difference change of existing PET materials cannot meet the stringent requirements of △E ≤ 1 after continuous baking for 1000 hours at 210°C, and cannot meet the high-temperature stability and color change performance required by end users.

Method used

Using a PET composition formula, including polyethylene terephthalate, brominated flame retardant, glass fiber, hydrotalcite and isopropoxy distearoyloxyaluminate, through the oxidation of specific molecular weight Polyethylene wax and controlled sodium antimonate content, combined with the use of modified glass fiber, prepare a PET composition with minimal color change at high temperatures.

Benefits of technology

After continuous baking at 210°C for 1000 hours, the color difference of the PET composition changed to ΔE ≤ 1, which significantly improved the degree of discoloration and retention of mechanical properties under long-term high temperatures, meeting the industry's stringent requirements for plastic materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention discloses a PET composition. The PET composition comprises the following components by weight: 28 to 76 parts of polyethylene terephthalate, 10 to 20 parts of brominated flame retardants, 2 to 6 parts of synergistic flame retardants, 10 to 40 parts of glass fibers, 1 to 3 parts of hydrotalcite, 0.5 to 2 parts of lubricants, and 0.2 to 1 parts of isopropoxy distearyloxyaluminate; the lubricant is an oxidized polyethylene wax with a weight average molecular weight of 3000 to 4000; the synergistic flame retardant is sodium antimonate with a Sb2O3 content of ≤0.05%; the particle size D of the hydrotalcite is 0.1 to 0.2 mm ... 50 ≤0.70μm. After the PET composition is continuously baked at 210°C for 1000h, the color difference change △E≤1, and the color difference change is very small under long-term high-temperature baking, which solves the core demands of customers and related industries and has extremely high economic value and application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of engineering plastics, and more specifically, relates to a PET composition and a preparation method and application thereof. Background Art

[0002] Polyethylene terephthalate (PET) is a thermoplastic polyester that is first commercialized and has the widest application field. Polyethylene terephthalate is an important polymer material that is widely used in the fields of engineering plastics and textiles. Its modified products are widely used in household appliances, connectors, coil skeletons, electrical housings and other electronic and electrical components.

[0003] The Chinese patent "Polybutylene terephthalate composite material and its preparation method" discloses a polybutylene terephthalate composite material with good anti-yellowing performance and good mechanical strength. The composite material formula system is a non-flame retardant glass fiber reinforced PBT / PET alloy (PBT is the main component). By adding 0.5-1% anti-yellowing additive (a mixture of anti-ultraviolet stabilizer and light stabilizer), it achieves an anti-yellowing effect of a color difference value △E≤3 when baked at 210 degrees Celsius for 48 hours under xenon lamp conditions.

[0004] Modified PET materials have been increasingly used in the small appliance industry in recent years due to their outstanding mechanical properties, heat resistance, electrical properties and processing properties. With the continuous increase in terminal demand, customers often require plastic materials to be able to work continuously under high temperature conditions of 200℃ to 210℃. Many customers have put forward strict requirements for the color difference change of the parts after baking at 210℃ for 1000h, △E≤1, but there are almost no materials on the market that can meet this test requirement. Summary of the invention

[0005] In response to the above-mentioned existing technical problems, the present invention provides a PET composition. After the PET composition is continuously baked for 1000 hours at 210°C, the color difference change △E≤1, and the color difference change is extremely small under long-term high-temperature baking, which solves the core demands of customers and related industries and has extremely high economic value and application prospects.

[0006] The second object of the present invention is to provide a method for preparing a PET composition.

[0007] The third object of the present invention is to provide an application of a PET composition in the electronic and electrical fields.

[0008] In order to achieve the above object, the present invention is implemented by the following technical solutions:

[0009] A PET composition comprises the following components by weight: 28 to 76 parts of polyethylene terephthalate, 10 to 20 parts of a brominated flame retardant, 2 to 6 parts of a synergistic flame retardant, 10 to 40 parts of glass fiber, 1 to 3 parts of hydrotalcite, 0.5 to 2 parts of a lubricant, and 0.2 to 1 part of isopropoxy distearyloxyaluminate; the lubricant is an oxidized polyethylene wax having a weight average molecular weight of 3000 to 4000; the synergistic flame retardant is Sb 2 O 3 The content of sodium antimonate is ≤0.05%, and the particle size of the hydrotalcite is D 50 ≤0.70μm.

[0010] In the present application, the weight average molecular weight of the oxidized polyethylene wax can be 3000, 3200, 3400, 3600, 3800, 4000, etc., but the present application is not limited thereto.

[0011] In this application, Sb of sodium antimonate 2 O 3 The content may be 0%, 0.01%, 0.02%, 0.03%, 0.04%, 0.05%, etc., but the present application is not limited thereto.

[0012] In the present application, the particle size of the hydrotalcite may be 0.55 μm, 0.5 μm, 0.45 μm, 0.4 μm, 0.35 μm, 0.3 μm, 0.25 μm, 0.2 μm, 0.15 μm, 0.1 μm, 0.05 μm, 0.01 μm, etc., but the present application is not limited thereto.

[0013] The inventors have found through research that isopropoxy distearyloxyaluminate has the best dispersing effect on hydrotalcite in the formula compared to coupling agents such as silane coupling agents and titanate coupling agents, so as to maximize the effect of hydrotalcite on improving the heat resistance stability of the body. The oxidized polyethylene wax can gradually precipitate to the surface of the product during high-temperature aging to form a protective film, which plays a role in partially isolating oxygen, thereby achieving the effect of reducing high-temperature baking discoloration; on this basis, the inventors further found that the oxidized polyethylene wax of a specific molecular weight has a greater impact on the compatibility of the PET system. The oxidized polyethylene wax with too high a molecular weight has poor compatibility in the system and is easy to precipitate during the molding process, thereby affecting the final lubrication and dispersion effect, thereby significantly reducing the implementation effect of the present invention. The oxidized polyethylene wax with too low a molecular weight has a poor lubrication and dispersion effect on the system, so that the implementation effect of the present invention will also be significantly reduced. In addition, the inventors found that when sodium antimonate is used as a synergistic flame retardant, it will cause a certain degree of degradation of the PET resin, thereby affecting the performance of the PET composition. It is speculated that this is caused by the antimony trioxide contained in the sodium antimonate. Finally, the hydrotalcite with a specific particle size in the PET system can not only greatly improve the heat resistance stability of the polymer, but also effectively reduce the discoloration degree of the PET system under long-term high-temperature baking, inhibit the decline of mechanical properties, and other effects. The inventor speculated through research that when the hydrotalcite is heated, the hydroxyl groups and interlayer ions of its structure are hydrated with water and CO 2 In addition, the inventors found that in the actual aging environment, there may be uncertain acidic components / environments. + The presence of can greatly catalyze and intensify the degradation of the PET system during the thermal oxidative aging process, thereby leading to the deterioration of polyester performance, intensified discoloration, etc., and hydrotalcite can be used as an acid absorber. From the perspective of acid absorption, the addition of hydrotalcite can also greatly improve the stability of the PET system under high temperature aging.

[0014] The inventors have found through research that the PET composition prepared by adding isopropoxy distearyloxyaluminate, a specific lubricant and hydrotalcite of a specific particle size to the PET system and controlling the content of sodium antimonate, combined with the comprehensive effect of other components in the system, can have a color difference change of △E≤1 after continuous baking at 210°C for 1000h, and the color difference change is extremely small under long-term high-temperature baking. A large amount of experimental data shows that only adding or controlling one or two of these, or the addition amount is not within the range specified by the present invention, is not enough to achieve the performance effect described in the present invention.

[0015] Preferably, the particle size D of the hydrotalcite is 50≤0.6 μm. Within this preferred range, the color difference of the PET composition under long-term high-temperature baking changes less, and the mechanical property retention rate of the PET composition can be improved.

[0016] Preferably, the intrinsic viscosity of the polyethylene terephthalate at 25° C. is 0.5 to 0.8 dL / g. Specifically, the intrinsic viscosity test method of the polyethylene terephthalate is based on GB / T14190-2017.

[0017] Preferably, the glass fiber is modified glass fiber.

[0018] Further preferably, the glass fiber is a glass fiber modified by a coupling agent, and the coupling agent is one or more of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane or isopropyl di(methacryl) isostearyl titanate.

[0019] More preferably, the mass ratio of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane and isopropyl di(methacryl)isostearoyl titanate is 1:(1-3): 1. Most preferably, the mass ratio is 1:2:1.

[0020] Preferably, the MgO content in the glass fiber is ≥10%.

[0021] In the present application, the MgO content in the glass fiber can be 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, etc., but the present application is not limited thereto.

[0022] The inventors found that different types of modified glass fibers have obvious differences in the wetting and coating effects in the PET system. After long-term research, the inventors found that glass fibers treated with γ-methacryloxypropyltrimethoxysilane have better wetting and coating effects in the PET system, while isopropyl di(methacryl) isostearyl titanate has a better wetting-promoting effect on the PET system and glass fibers. In addition, the inventors found that when the MgO content in the glass fiber is ≥10%, it can better improve the mechanical properties of the composition. The present invention improves the mechanical property retention rate and heat resistance stability of the PET system after continuous baking for 1000 hours at 210°C by adding hydrotalcite, modifying the glass fiber and limiting the MgO content in the glass fiber, and the retention rate of tensile strength and notched impact strength is above 94%.

[0023] Preferably, the brominated flame retardant is selected from one or more of brominated polystyrene, polybrominated styrene, brominated polycarbonate, brominated epoxy resin or brominated polypentabromobenzyl acrylate.

[0024] In addition, the present invention also provides a method for preparing a PET composition, comprising mixing a brominated flame retardant, a synergistic flame retardant, hydrotalcite, a lubricant and isopropoxy distearoyloxyaluminate, adding polyethylene terephthalate and glass fiber, and melt-extruding to obtain the PET composition.

[0025] Preferably, the temperature of the melt extrusion is 220-280°C.

[0026] Preferably, the screw speed during the melt extrusion is 200-450 rpm.

[0027] Preferably, the ratio of the barrel length to the screw diameter of the twin-screw extruder is (32-48):1.

[0028] Furthermore, the present invention also protects the application of the above PET composition in the field of electronics and electrical appliances. Specifically, the PET composition can be used as a color change resistant material or a high temperature aging resistant material in lighting fixtures, cooling fans, connectors, coil skeletons, electrical appliance housings and other types of electronic and electrical products, especially in situations where there are extremely high requirements for the color change and mechanical property retention rate of the material after long-term high temperature baking.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The invention adopts oxidized polyethylene wax with a specific molecular weight, isopropoxy distearyloxyaluminate and hydrotalcite, and optimizes the Sb in the synergistic flame retardant. 2 O 3 The content of PET is 200mg / L; under the joint action of these additives and other components in the system, a PET composition with minimal color difference change under high temperature and long-term baking is prepared. After the PET composition is baked continuously for 1000 hours at 210°C, the color difference change △E≤1. It can better improve the discoloration degree and trend of the PET composition under long-term high temperature, and meet and realize the stringent requirements of some industries and customers on the color change performance of plastic materials. DETAILED DESCRIPTION

[0031] The present invention is further described below with reference to specific examples, but the examples do not limit the present invention in any form. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.

[0032] Examples and Comparative Examples Raw Materials Description:

[0033] Polyethylene terephthalate (PET resin 1), with an intrinsic viscosity of 0.68 dL / g at 25°C, brand FG600, from Yizheng Chemical Fiber Company.

[0034] Polyethylene terephthalate (PET resin 2), intrinsic viscosity at 25°C is 0.88 dL / g, brand CR-8828, Zhuhai China Resources Company.

[0035] Synergistic flame retardant 1: sodium antimonate, Sb 2 O 3 The content of Sb in sodium antimonate is 0.03%, brand name SA-F, Chengdu Kaifei High Energy Chemical Industry Co., Ltd. 2 O 3 The content is determined in accordance with SJ / T 10087.8-91.

[0036] Synergistic flame retardant 2: sodium antimonate, Sb 2 O 3 The content of Sb in sodium antimonate is 0.15%, brand ATSA-62, Guangzhou Ante Antimony Metal Co., Ltd. 2 O 3 The content is determined in accordance with SJ / T 10087.8-91.

[0037] Synergistic flame retardant 3: Antimony white, brand S-05N, Changde Chenzhou Antimony Products Co., Ltd.

[0038] Hydrotalcite 1, DHT-4A-2, particle size D 50 =0.5μm, Kyowa Chemical Industry Co., Ltd.

[0039] Hydrotalcite 2, LDH-A, particle size D 50 =0.65μm, Jiangxi Hongyuan Chemical Co., Ltd.

[0040] Lubricant 1: Oxidized polyethylene wax, weight average molecular weight 3500, brand PED 521, Guangzhou Rongda Chemical Co., Ltd.

[0041] Lubricant 2: oxidized polyethylene wax, weight average molecular weight of 2800, brand Luwax OA3, from BASF, Germany.

[0042] Lubricant 3: oxidized polyethylene wax, weight average molecular weight of 4800, brand PEWO-0520, Nanjing Tianshi New Material Technology Co., Ltd.

[0043] Lubricant 4: pentaerythritol stearate, commercially available.

[0044] Isopropoxy distearyloxyaluminate 1, brand HW-133, Zhejiang Feidian Chemical Co., Ltd.

[0045] Isopropoxy distearyloxyaluminate 2, brand RZ-AL18, Jinan Rongzheng Chemical Co., Ltd.

[0046] Coupling agent 1: N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, commercially available.

[0047] Coupling agent 2: γ-methacryloxypropyltrimethoxysilane, commercially available.

[0048] Coupling agent 3: isopropyl di(methacryloyl) isostearyl titanate, commercially available.

[0049] The coupling agent 4,3-glycidyloxypropyltrimethoxysilane is commercially available.

[0050] Coupling agent 5, bis(dioctyloxypyrophosphate)ethylene titanate, commercially available.

[0051] Glass fiber 1: brand HMG436S-10-4.0, Taishan Glass Fiber Co., Ltd.;

[0052] Modified glass fiber 1-1: glass fiber 1 is dispersed in a coupling agent, and stirred and mixed at 20-40° C. for 5-8 minutes to obtain modified glass fiber 1-1, wherein the MgO content of the modified glass fiber 1-1 is 16%; wherein the coupling agent is a mixture of coupling agent 1, coupling agent 2 and coupling agent 3, and the mass ratio of the three is 1:2:1;

[0053] Modified glass fiber 1-2: Disperse glass fiber 1 in coupling agent, stir and mix at 20-40° C. for 5-8 minutes to obtain modified glass fiber 1-2, wherein the MgO content is 16%; wherein the coupling agent is a mixture of coupling agent 1, coupling agent 2 and coupling agent 3, and the mass ratio of the three is 2:1:1;

[0054] Modified glass fiber 1-3: Disperse glass fiber 1 in a coupling agent, stir and mix at 20-40° C. for 5-8 minutes to obtain modified glass fiber 1-3, whose MgO content is 16%; wherein the coupling agent is coupling agent 4, i.e. 3-glycidyloxypropyltrimethoxysilane.

[0055] Glass fiber 2: grade ECS13-4.5-534A(E), Jushi Group Co., Ltd.

[0056] Modified glass fiber 2-1: Disperse glass fiber 2 in a coupling agent, stir and mix at 20-40°C for 5-8 minutes to obtain modified glass fiber 2-1, whose MgO content is 4%; wherein the coupling agent is a mixture of coupling agent 1, coupling agent 2 and coupling agent 3, and the mass ratio of the three is 1:2:1.

[0057] Brominated flame retardant: brominated polystyrene, commercially available.

[0058] Unless otherwise specified, the components (eg, brominated flame retardants) used in the parallel examples and comparative examples are all the same commercially available products.

[0059] Example 1

[0060] The weight parts of the raw materials used in Example 1 are shown in Table 1.

[0061] A method for preparing a PET composition, the specific steps comprising:

[0062] (1) According to the weight proportions in Table 1, the brominated flame retardant, synergistic flame retardant, hydrotalcite, lubricant, and isopropoxy distearyloxyaluminate were weighed and put into a high-speed mixer for dry mixing for 3 to 5 minutes at a speed of 500 to 800 rpm.

[0063] (2) adding the mixture obtained in step (1), polyethylene terephthalate and modified glass fiber 1-1 into a twin-screw extruder through a feeder, wherein the temperature of zone 1 from the feed port to the die is 220-250° C., the temperature of zone 2 is 260-280° C., the temperature of zone 3 is 255-275° C., the temperature of zone 4 is 255-275° C., the temperature of zone 5 is 255-275° C., the temperature of zone 6 is 260-280° C., the temperature of zone 7 is 260-280° C., the temperature of zone 8 is 240-260° C., the temperature of zone 9 is 240-260° C., the temperature of zone 10 is 260-280° C., the screw speed is 200-450 rpm, the aspect ratio is 40:1, mixing, dispersing, melt extruding and granulating are carried out to obtain a PET composition.

[0064] Embodiments 2 to 12

[0065] The weight parts of the raw materials used in the following examples are shown in Table 1.

[0066] The specific preparation steps of the following examples are the same as those of Example 1.

[0067] The difference between Example 5 and Example 1 is that modified glass fiber 1-3 is used, and an equal amount of coupling agent 4:3-glycidyloxypropyltrimethoxysilane is used alone to modify glass fiber 1.

[0068] The difference between Example 6 and Example 1 is that modified glass fiber 1-2 is used.

[0069] Comparative Examples 1 to 11

[0070] The weight parts of the raw materials used in the following comparative examples are shown in Table 2.

[0071] The specific preparation steps of each comparative example are the same as those of Example 1. Table 1 shows the formula components of each example:

[0072] Table 1

[0073]

[0074] Table 2 shows the formula components of each comparative example:

[0075] Table 2

[0076]

[0077]

[0078] The raw materials used in the above examples and comparative examples and the prepared PET compositions were tested according to the following test methods:

[0079] The test method for intrinsic viscosity of polyethylene terephthalate is based on GB / T 14190-2017.

[0080] MgO content in modified glass fiber (%): measured in accordance with GB / T 1549-2008.

[0081] Tensile strength (MPa): tested using the test method of ISO527:2000.

[0082] Notched impact strength (kJ / m 2 ): Tested using the ISO180:2000 test method.

[0083] Flame retardancy: tested using the UL94-2003 test method.

[0084] Color difference: The test was conducted using a colorimeter (equipment model CE7000A, Gretag Macbeth, USA).

[0085] Tables 3 and 4 are the performance test results of the embodiments and comparative examples, respectively, wherein the tensile strength retention rate, notched impact strength retention rate and color difference ΔE are the data measured at 210° C. after baking for 1000 hours.

[0086] Table 3

[0087]

[0088]

[0089] Table 4

[0090]

[0091] As can be seen from Table 3, after the PET compositions prepared in Examples 1 to 12 were baked at 210° C. for 1000 h, the color difference change ΔE was less than 1, and the color difference change was extremely small under long-term high-temperature baking; in addition, the tensile strength retention rate and notched impact strength retention rate of the PET compositions were ≥94%.

[0092] The intrinsic viscosity of the PET resin in Example 3 is 0.88 dL / g. The PET composition prepared in Example 1 has a smaller color difference ΔE than the PET composition in Example 3, and has a better mechanical property retention rate.

[0093] The particle size D50 of the hydrotalcite in Example 4 is 0.65 μm. The color difference change ΔE of the PET composition prepared in Example 4 is significantly different from that of the PET composition prepared in Example 1, and the mechanical property retention rate is worse than that in Example 1.

[0094] In Example 5 and Example 6, respectively, glass fibers modified with a single coupling agent and glass fibers modified with coupling agent 1, coupling agent 2 and coupling agent 3 in a mass ratio of 2:1:1 were used. It can be seen that the color difference change ΔE and mechanical property retention rate of the PET compositions prepared in Example 5 and Example 6 are worse than those of the PET composition in Example 1.

[0095] Example 7 uses modified glass fiber with a magnesium oxide content of 16%. It can be seen that the color difference change ΔE and mechanical property retention rate of the PET composition prepared in Example 7 are worse than those of the PET composition in Example 1.

[0096] As can be seen from Table 4, Comparative Examples 1 to 4 are comparative examples lacking isopropoxy distearoyloxyaluminate, lubricant, lubricant and isopropoxy distearoyloxyaluminate, and hydrotalcite, respectively. It can be seen that the color difference change ΔE of the PET compositions prepared in Comparative Examples 1 to 4 is much greater than that of the PET composition in Example 1, indicating that isopropoxy distearoyloxyaluminate, lubricant, and hydrotalcite are extremely important for the control of color difference and are indispensable. In addition, the mechanical property retention rate of the PET compositions prepared in Comparative Examples 1 to 4 is also much lower than that of the PET composition in Example 1.

[0097] Comparative Examples 5 and 6 are comparative examples using coupling agent 4 (silane coupling agent) and coupling agent 5 (titanate coupling agent), respectively. It can be seen from Comparative Examples 5 and 6 that the color difference ΔE of the prepared PET composition is much worse than that of the PET composition in Example 1, and the mechanical property retention rate is reduced to a certain extent.

[0098] Comparative Examples 7 and 8 are comparative examples using oxidized polyethylene waxes of different molecular weights. It can be seen that the color difference ΔE of the PET compositions prepared in Comparative Examples 7 and 8 is much worse than that of the PET composition in Example 1. This indicates that the oxidized polyethylene wax of a specific molecular weight has a great influence on the color difference change. In addition, the mechanical property retention rate of the PET compositions prepared in Comparative Examples 7 and 8 has a certain degree of decrease.

[0099] Comparative Example 9 is a comparative example using other lubricants, and the color difference ΔE of the PET composition prepared in Comparative Example 9 is much worse than that of the PET composition in Example 1. This indicates that a specific type of lubricant has a great influence on the control of the color difference ΔE.

[0100] Comparative Example 10 is a comparative example using other synergistic flame retardants. It can be seen that the specific synergistic flame retardant has a great influence on the color difference ΔE and mechanical property retention rate of the PET composition.

[0101] Comparative Example 11 is Sb in sodium antimonate 2 O 3 The comparative example with content>0.05%. 2 O 3 The content has a certain degree of influence on the color difference ΔE and mechanical property retention rate of the PET composition.

[0102] The foregoing examples are merely illustrative and are used to explain some features of the method of the present invention. The appended claims are intended to require the widest possible range that can be imagined, and the embodiments presented herein are demonstrated by the applicant's actual test results. Therefore, the applicant's intention is that the appended claims are not limited by the selection of examples that illustrate the features of the present invention. Some numerical ranges used in the claims also include sub-ranges therein, and changes in these ranges should also be interpreted as being covered by the appended claims where possible.

Claims

1. A PET composition, characterized in that The composition comprises the following components by weight: 28 to 76 parts of polyethylene terephthalate, 10 to 20 parts of brominated flame retardant, 2 to 6 parts of synergistic flame retardant, 10 to 40 parts of glass fiber, 1 to 3 parts of hydrotalcite, 0.5 to 2 parts of lubricant, and 0.2 to 1 part of isopropoxy distearyloxyaluminate; The lubricant is an oxidized polyethylene wax with a weight average molecular weight of 3200 to 4000; The synergistic flame retardant is sodium antimonate with a Sb2O3 content of ≤0.05%; The particle size D of the hydrotalcite 50 ≤0.70μm.

2. The PET composition according to claim 1, characterized in that: The intrinsic viscosity of the polyethylene terephthalate at 25° C. is 0.5 to 0.8 dL / g.

3. The PET composition according to claim 1, characterized in that: The particle size D of the hydrotalcite 50 ≤0.60μm.

4. The PET composition according to any one of claims 1 to 3, characterized in that: The glass fiber is modified glass fiber.

5. The PET composition according to claim 4, characterized in that: The glass fiber is a glass fiber modified by a coupling agent; the coupling agent is one or more of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane or isopropyl di(methacryl) isostearyl titanate.

6. The PET composition according to claim 5, characterized in that: The mass ratio of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-methacryloxypropyltrimethoxysilane and isopropyl di(methacryl) isostearyl titanate is 1:(1-3):

1.

7. The PET composition according to claim 4, characterized in that: The MgO content in the glass fiber is ≥10%.

8. The PET composition according to claim 1, characterized in that: The brominated flame retardant is selected from one or more of brominated polystyrene, brominated polycarbonate, brominated epoxy resin or brominated polypentabromobenzyl acrylate.

9. The PET composition according to claim 1, characterized in that: The brominated flame retardant is polybrominated styrene.

10. The method for preparing the PET composition according to any one of claims 1 to 9, characterized in that: The bromine flame retardant, the synergistic flame retardant, the hydrotalcite, the lubricant and the isopropoxy distearyloxyaluminate are mixed, and then polyethylene terephthalate and glass fiber are added, and melt extruded to obtain a PET composition.

11. Use of the PET composition according to any one of claims 1 to 9 in the field of electronics and electrical appliances.

Citation Information

Patent Citations

  • Flame-retardant polyester material with high glow wire ignition temperature and preparation method thereof

    CN102250450A

  • Rare earth modified bottle preform polyester material

    CN113025004A