Method for producing zirconia sintered body

By controlling the heating rate and temperature of the short-time sintering process of zirconia, the problem of interlayer striations with different yttrium oxide contents was solved, enabling the production of aesthetically pleasing and uniformly strong zirconia sintered bodies in a short time, suitable for dental restorations.

CN116209409BActive Publication Date: 2024-11-08KURARAY NORITAKE DENTAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202180065597.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2020-09-25
Filing Date
2021-09-24
Publication Date
2024-11-08
Estimated Expiration
2041-09-24

AI Technical Summary

Technical Problem

In existing technologies, striations can easily form between layers with different yttrium oxide content during short-time sintering of zirconium oxide, affecting the aesthetics and strength of dental restorations.

Method used

A specific short-time firing process is adopted, including at least three stages of heating process, controlling the heating rate and temperature range to ensure that the zirconia shaped body or zirconia pre-fired body is sintered in a short time, reducing the difference in light transmittance between layers and suppressing the appearance of streaks.

Benefits of technology

Zirconia sintered bodies can be produced in a short time with inconspicuous interlayer striations and the same color and intensity as conventional long-time fired materials, making them suitable for dental restorations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116209409B_ABST
    Figure CN116209409B_ABST
Patent Text Reader

Abstract

The present invention provides a method for producing a zirconia sintered body, wherein a zirconia formed body or a zirconia calcined body having a plurality of layers with different amounts of a stabilizer is sintered in a short time, thereby making the stripes between the layers with different yttria contents inconspicuous. The present invention relates to a method for producing a zirconia sintered body, comprising a firing step of firing a zirconia formed body or a zirconia calcined body, wherein the zirconia formed body or the zirconia calcined body has a plurality of layers containing a stabilizer, wherein the plurality of layers include layers with different stabilizer contents, wherein the firing step includes at least three stages of a first heating step (H1), a second heating step (H2), and a third heating step (H3), wherein the heating rate of H2 is set to HR2, and the heating rate of H3 is set to HR3, wherein HR2 exceeds 0°C / min. And less than 50℃ / min, HR3=5~150℃ / min, HR3 / HR2>1, the starting temperature in each heating process is below 1000℃ in H1, exceeds 1250℃ and is below 1450℃ in H2, and is above 1450℃ and below 1550℃ in H3, the reaching temperature in each heating process is above 1250℃ and is below 1450℃ in H1, is above 1450℃ and is below 1550℃ in H2, and is above 1500℃ and is below 1750℃ in H3.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a zirconia sintered body. Background Art

[0002] In the past, metals were widely used as dental products (e.g., representative crowns, crowns, prostheses such as dentures, orthodontic products, and dental implant products). However, the color of metal is significantly different from that of natural teeth, which has the disadvantage of lacking aesthetic appeal, and sometimes causes allergies due to metal dissolution. Therefore, in order to solve the problems associated with the use of metals, ceramic materials such as alumina (aluminum oxide) and zirconium oxide (zirconia) are gradually being used in dental products as alternative materials to metals. In particular, zirconium oxide has excellent strength and relatively excellent aesthetic appeal, so its demand has increased in conjunction with its low price.

[0003] On the other hand, in order to make a dental prosthesis using zirconia, the shape of the dental prosthesis is cut out from a block or disk-shaped cutting workpiece (cut workpiece) pre-fired at a temperature about 400°C to 700°C lower than the temperature at which an ideal sintered body is obtained using a CAD / CAM device, and the cut unsintered zirconia processed body is kept at a maximum temperature of 1400°C to 1650°C for sintering. Therefore, the total time from heating up, staying, to cooling down is usually 6 to 12 hours. With regard to this time, the demand for short-time firing has increased in recent years, and firing furnaces capable of short-time firing as described in Patent Documents 1 and 2 have been manufactured.

[0004] Furthermore, in recent years, in order to achieve both strength and aesthetics of dental restorations obtained using zirconia, cutting workpieces having multiple layers with different contents of stabilizers (e.g., yttria), so-called yttria multilayer zirconia mill blanks, have gradually increased (e.g., see Patent Document 3, etc.).

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application No. 2015-531048

[0008] Patent Document 2: Japanese Patent Application No. 2019-524298

[0009] Patent document 3: International Publication No. 2020 / 138316. Summary of the invention

[0010] Problems to be solved by the invention

[0011] Patent Documents 1 to 3 disclose firing furnaces and process conditions for firing ceramics containing zirconium oxide in a short time. However, the present inventors have found that when using the conventional short-time firing process, the obtained sintered body can obtain the color tone and strength of an ideal dental prosthesis, but on the other hand, there is a problem of streaks between layers with different contents of yttrium oxide as a stabilizer.

[0012] Therefore, an object of the present invention is to provide a method for producing a zirconia sintered body, which makes it possible to make the stripes between the layers having different amounts of stabilizers inconspicuous by sintering a zirconia formed body or a zirconia calcined body having a plurality of layers having different amounts of stabilizers in a short time. Another object is to provide a method for producing a zirconia sintered body, which can reproduce the color tone and strength of an ideal dental prosthesis to the same extent as when the zirconia formed body or the zirconia calcined body is fired under normal conditions even though the zirconia formed body or the zirconia calcined body is sintered in a short time.

[0013] Means used to solve problems

[0014] The present inventors have conducted intensive studies to solve the above-mentioned problems and have found that by using a specific short-time firing process for a zirconia formed body or a zirconia calcined body having a plurality of layers with different amounts of stabilizers, a zirconia sintered body with inconspicuous stripes between the layers can be obtained even with a short-time firing. Based on this finding, the present inventors have conducted further studies and have completed the present invention.

[0015] That is, the present invention includes the following technical solutions.

[0016] [1] A method for producing a zirconia sintered body, comprising a firing step of firing a zirconia formed body or a zirconia calcined body,

[0017] The zirconia formed body or calcined zirconia body comprises a plurality of layers containing a stabilizer.

[0018] The plurality of layers include layers having different stabilizer contents.

[0019] The sintering step includes at least three steps of heating steps, namely, a first heating step (H1), a second heating step (H2) and a third heating step (H3).

[0020] The heating rate of the second heating step (H2) is set to HR2.

[0021] When the temperature increase rate in the third temperature increase step (H3) is set to HR3,

[0022] HR2 exceeds 0℃ / min and is less than 50℃ / min,

[0023] HR3 = 5°C / min or more and 150°C / min or less,

[0024] HR3 / HR2>1,

[0025] The starting temperature in each temperature rising step is 1000°C or less in H1, more than 1250°C and less than 1450°C in H2, and more than 1450°C and less than 1550°C in H3.

[0026] The reaching temperature in each temperature rising step is more than 1250° C. and 1450° C. or less in H1, 1450° C. or more and 1550° C. or less in H2, and 1500° C. or more and 1750° C. or less in H3.

[0027] [2] The method for producing a zirconia sintered body according to [1], wherein when the heating rate in the first heating step (H1) is HR1, HR1 is 40 to 500°C / min.

[0028] [3] The method for producing a zirconia sintered body according to [1] or [2], wherein the difference in the content of the stabilizer between the layers having different contents of the stabilizer is 0.1 mol % or more.

[0029] [4] The method for producing a zirconium oxide sintered body according to any one of [1] to [3], wherein the stabilizer is yttrium oxide.

[0030] [5] The method for producing a zirconium oxide sintered body according to [4], wherein the content of the yttrium oxide in all of the plurality of layers is 2.5 mol% or more and 7.5 mol% or less relative to the total molar content of zirconium oxide and yttrium oxide.

[0031] [6] The method for producing a zirconia sintered body according to any one of [1] to [5], wherein HR2 is 2 to 30°C / min.

[0032] [7] The method for producing a zirconia sintered body according to any one of [1] to [6], wherein HR3 is 10 to 100°C / min.

[0033] [8] The method for producing a zirconia sintered body according to any one of [1] to [7], wherein HR3 / HR2>1.5.

[0034] [9] The method for producing a zirconia sintered body according to any one of [1] to [8], wherein the maximum sintering temperature in the above-mentioned temperature rising step is 1400 to 1750°C, and the residence time at the maximum sintering temperature is within 30 minutes.

[0035]

[10] The method for producing a zirconia sintered body according to [9], further comprising a temperature reduction step, wherein the temperature reduction rate from the highest sintering temperature in the temperature increase step to 800°C is 10°C / min or more.

[0036]

[11] A method for producing a zirconia sintered body according to any one of [1] to

[10] , wherein the total sintering time in the sintering step from the start of the temperature increase in the first temperature increase step (H1) to the end of the residence time at the maximum sintering temperature is within 120 minutes.

[0037]

[12] The method for producing a zirconia sintered body according to any one of [1] to

[11] , wherein 55% or more of the zirconia formed body or the zirconia calcined body is monoclinic.

[0038]

[13] The method for producing a zirconia sintered body according to any one of [1] to

[12] , wherein in the zirconia formed body or the zirconia calcined body, at least a portion of the stabilizer is not dissolved in the zirconia.

[0039]

[14] The method for producing a zirconia sintered body according to any one of [1] to

[13] , wherein the zirconia formed body or the zirconia calcined body has a predetermined shape of a dental product.

[0040]

[15] The method for producing a zirconia sintered body according to

[14] , wherein the dental product is a dental prosthesis.

[0041] Effects of the Invention

[0042] According to the method for producing a zirconia sintered body of the present invention, it is possible to provide a method for producing a zirconia sintered body in which a zirconia formed body or a zirconia calcined body having a plurality of layers having different amounts of stabilizers is sintered in a short time, thereby making the stripes between the layers having different amounts of stabilizers inconspicuous. In addition, it is possible to provide a method for producing a zirconia sintered body in which the color tone and strength of an ideal dental prosthesis can be reproduced to the same extent as when the sintering is carried out under normal sintering conditions (total sintering time: 6 to 12 hours) despite sintering in a short time. BRIEF DESCRIPTION OF THE DRAWINGS

[0043] Figure 1 A schematic diagram showing a zirconia calcined body according to the present invention. DETAILED DESCRIPTION

[0044] The reason why the zirconia sintered body without streaks between layers with different amounts of stabilizers can be obtained by sintering the zirconia formed body or zirconia calcined body in a short time (for example, a total sintering time of 120 minutes or less) using the method for producing a zirconia sintered body of the present invention is still unclear, but the present inventors speculate as follows. First, it can be considered that the greater the difference in light transmittance (hereinafter sometimes referred to as ΔL(WB)) between adjacent layers with different amounts of stabilizers in the obtained zirconia sintered body, the more noticeable the streaks become by sintering in a short time, and conversely, the smaller the difference in ΔL(WB), the less noticeable the streaks become.

[0045] The inventors of the present invention have found the following phenomenon when studying the countermeasures: when the temperature is gradually increased according to the amount of stabilizer contained in the layer, the temperature range in which the rate of increase of ΔL(WB) changes is different in the case of short-time sintering. It is considered that based on this phenomenon, by slowing down the rate of temperature increase in a specific temperature range in which the ΔL(WB) of adjacent layers with different amounts of stabilizers increases at the same level (i.e., the ΔL(WB) of the layers is not likely to differ), the ΔL(WB) of the entire zirconia formed body or zirconia calcined body to be heated is increased, and the rate of temperature increase in the temperature range in which the ΔL(WB) is likely to differ is accelerated, and sintering is performed at a high speed, so that the difference in ΔL(WB) between the layers with different amounts of stabilizers is minimized during short-time sintering, thereby comprehensively suppressing the difference in ΔL(WB) between the layers with different amounts of stabilizers, and thus, despite the short sintering time, a zirconia sintered body in which the streaks are not noticeable, that is, the state in which the stacking interface is not clearly confirmed can be obtained.

[0046] Hereinafter, the present invention will be described in detail.

[0047] The firing furnace used in the firing of the present invention is an atmospheric furnace, which can be a box-type furnace, a crucible furnace, a tubular furnace, a furnace bottom lifting furnace, a continuous furnace, a rotary furnace, a resistance heating furnace, an induction heating furnace, a straight-through electric furnace, an IH furnace, a high-frequency furnace, a microwave oven, and the heat release body can use a metal heat release body, silicon carbide, molybdenum disilicide, lanthanum chromium wire, molybdenum, carbon, tungsten, etc., and SiC can also be used as a heat release body base. It can also be a firing furnace obtained by combining any two or more of these. In addition, the firing furnace chamber with a base for placing a zirconia molded body or a zirconia pre-calcined body having a specified shape such as a crown is small in volume, has good thermal efficiency, and can easily maintain the heat in the furnace during firing.

[0048] The zirconia formed body in the present invention is a formed body formed by unfired, i.e., unsintered zirconia. The zirconia formed body in the present invention may be partially stabilized zirconia or completely stabilized zirconia. In the present invention, "unsintered" refers to a state in which the contact parts of the particles of the zirconia powder do not react with each other. The zirconia calcined body of the present invention can be a precursor (intermediate product) of a zirconia sintered body. The zirconia calcined body refers to a substance obtained by agglomerating, for example, zirconia particles (powder) in an incompletely sintered state. It should be noted that in the present specification, the upper limit and lower limit of the numerical range (heating rate, cooling rate, sintering time, temperature, speed ratio, content of each component (such as stabilizer) etc.) can be appropriately combined.

[0049] The method for producing a zirconia sintered body of the present invention includes at least three stages of heating processes. Regarding each heating process, the first heating process is set as H1, the second heating process is set as H2, and the third heating process is set as H3, and each heating process has a different heating rate. In addition, the heating process may be only three stages, or may include other heating processes.

[0050] [First temperature rising step (H1)]

[0051] In the first heating step (H1) of the method for producing a zirconia sintered body of the present invention, the zirconia formed body or the zirconia pre-calcined body is heated in a firing furnace heated to room temperature or above room temperature and below 1000°C, and the temperature is raised to the reaching temperature of the first heating step (H1) at one time. The zirconia formed body or the zirconia pre-calcined body before firing in the first heating step (H1) preferably has a prescribed shape of a dental product. Dental products include, for example, representative dental prostheses such as crowns, tooth crowns, and attached dentures; products for orthodontics; products for dental implants, etc. The zirconia formed body or the zirconia pre-calcined body before heating can be processed using a dental CAD / CAM device, or can be produced by a dental technician through cutting or the like.

[0052] The zirconia formed body or zirconia calcined body before heating may be directly placed on the muffle member of the firing furnace during firing, or may be placed in the furnace using a tray, base, pin made of ceramic or high melting point metal, or may be placed using ceramic beads.

[0053] The starting temperature of the first temperature increasing step (H1) is not particularly limited as long as it is 1000°C or less, and is preferably room temperature to 1000°C, more preferably room temperature to 450°C, further preferably room temperature to 400°C, and particularly preferably room temperature to 300°C. The reaching temperature of the first temperature increasing step (H1) is 1250 to 1450°C, and is preferably 1300°C or more from the viewpoint of further shortening the operation time, and is more preferably 1350°C or more, and further preferably 1400°C or more from the viewpoint of reducing the difference in transparency between layers having different contents of yttrium oxide as a stabilizer.

[0054] In addition, when the heating rate of the first heating step (H1) is set to HR1, from the viewpoint of further shortening the working time, HR1 is preferably 40°C / min or more, more preferably 50°C / min or more, more preferably 60°C / min or more, and particularly preferably 70°C / min or more. In addition, HR1 is preferably 500°C / min or less, more preferably 450°C / min or less, more preferably 400°C / min or less, and particularly preferably 350°C / min or less. When HR1 exceeds 500°C / min, it is possible to induce the occurrence of chipping and cracking during firing. In the case where the zirconia formed body or zirconia calcined body provided to the first heating step (H1) contains water used in processing and a color liquid for coloring, the first heating step (H1) can be started after a drying step of 1 minute or more and 20 minutes or less, preferably 5 minutes or more and 15 minutes or less at 300°C or less. In addition, as a certain suitable embodiment, a method for producing a zirconia sintered body with HR1 / HR3>1 can be cited. More preferably, HR1 / HR3>1.5, and even more preferably, HR1 / HR3>2.

[0055] [Second temperature rising step (H2)]

[0056] In the method for producing a zirconia sintered body of the present invention, when the heating rate of the second heating step (H2) is set to HR2, HR2 exceeds 0°C / min, and is preferably 1°C / min or more, more preferably 2°C / min or more, further preferably 3°C / min or more, and particularly preferably 4°C / min or more from the viewpoint of further shortening the working time. In addition, HR2 is less than 50°C / min, and is preferably less than 40°C / min, more preferably 35°C / min or less, further preferably 30°C / min or less, and particularly preferably 20°C / min or less from the viewpoint of obtaining a zirconia sintered body with better brightness and light transmittance and suppressing the generation of streaks between layers with different yttrium oxide contents.

[0057] The starting temperature of the second temperature raising step (H2) is 1250-1450°C, preferably 1300°C or higher from the viewpoint of further shortening the working time, more preferably 1350°C or higher, and further preferably 1400°C or higher from the viewpoint of reducing the difference in transparency between layers having different contents of yttrium oxide as a stabilizer. The reaching temperature of the second temperature raising step (H2) is 1450-1550°C, preferably 1470°C or higher, more preferably 1490°C or higher, and further preferably 1500°C or higher from the viewpoint of further shortening the working time. In addition, the reaching temperature of H2 is preferably 1540°C or lower, more preferably 1530°C or lower, and further preferably 1520°C or lower from the viewpoint of further improving the brightness, light transmittance, and chroma of the obtained zirconia sintered body, and when the zirconia formed body or the zirconia calcined body contains a composite oxide, the composite oxide has excellent color development and suppresses the generation of streaks between layers having different contents of yttrium oxide.

[0058] [Third Temperature Heating Step (H3)]

[0059] When the heating rate in the third heating step (H3) is HR3, from the viewpoint that when the zirconia formed body or zirconia calcined body having layers with different amounts of stabilizers is fired for a short time, the difference in transparency between the layers with different contents of yttrium oxide as a stabilizer can be reduced and the occurrence of streaks between the layers with different contents of yttrium oxide can be suppressed, HR3 / HR2>1. From the viewpoint that the brightness, light transmittance and chroma of the obtained zirconia sintered body are more excellent, and when the zirconia formed body or zirconia calcined body contains a composite oxide, the color development of the composite oxide is excellent and the occurrence of streaks between the layers with different contents of yttrium oxide can be suppressed, HR3 / HR2>1.2 is preferred, HR3 / HR2>1.5 is more preferred, and HR3 / HR2>2 is further preferred. In addition, HR3 is 5°C / min or more, and from the viewpoint that the working time can be further shortened and the occurrence of streaks between the layers with different contents of yttrium oxide can be suppressed, HR3 is preferably 8°C / min or more, more preferably 9°C / min or more, and further preferably 10°C / min or more. In addition, from the viewpoint of obtaining a zirconia sintered body with better chroma, and from the viewpoint of excellent color development of the composite oxide when the zirconia formed body or the zirconia calcined body contains a composite oxide, and from the viewpoint of suppressing the generation of streaks, HR3 is 150°C / min or less, preferably 100°C / min or less, and more preferably 50°C / min or less.

[0060] The starting temperature of the third temperature raising step (H3) is 1450-1550°C, and is preferably 1470°C or higher, more preferably 1490°C or higher, and further preferably 1500°C or higher, from the viewpoint of further shortening the operation time and suppressing the generation of streaks between layers having different yttria contents. In addition, from the viewpoint that the brightness, light transmittance and chromaticity of the obtained zirconia sintered body are more excellent, and when the zirconia formed body or the zirconia calcined body contains a composite oxide, the starting temperature of H3 is preferably 1540°C or lower, more preferably 1530°C or lower, and further preferably 1520°C or lower.

[0061] The temperature reached in the third temperature raising step (H3) is 1500 to 1750°C, and is preferably 1510°C or higher, more preferably 1530°C or higher, and even more preferably 1550°C or higher, from the viewpoint that the brightness, light transmittance, and chroma of the obtained zirconia sintered body are more excellent, and when the zirconia formed body or the zirconia calcined body contains a composite oxide, the color development of the composite oxide is excellent. In addition, from the viewpoint that the operation time can be further shortened, the brightness, light transmittance, and chroma of the obtained zirconia sintered body are more excellent, and when the zirconia formed body or the zirconia calcined body contains a composite oxide, the color development of the composite oxide is excellent, and the generation of streaks between layers with different yttrium oxide contents is suppressed, the temperature reached in H3 is preferably 1700°C or lower, more preferably 1650°C or lower, and even more preferably 1600°C or lower.

[0062] The zirconia formed body or zirconia calcined body used in the method for producing a zirconia sintered body of the present invention preferably contains a stabilizer capable of suppressing the phase transformation of zirconia in addition to zirconia. The zirconia formed body or zirconia calcined body preferably contains at least a portion of the stabilizer not dissolved in zirconia. The stabilizer is preferably capable of forming partially stabilized zirconia.

[0063] The zirconia formed body or zirconia calcined body used in the method for manufacturing a zirconia sintered body of the present invention has a plurality of layers containing a stabilizer, and the plurality of layers have layers with different stabilizer contents relative to the total moles of zirconium oxide and stabilizers. The number of layers with different stabilizer contents is not particularly limited as long as it is 2 layers or more, and can be 3 layers, 4 layers, 5 layers, or 6 layers. In addition, as a zirconia formed body or a zirconia calcined body, as long as it has layers with different stabilizer contents, it can also further include 2 or more layers with the same stabilizer content. By providing a zirconia formed body or a zirconia calcined body with layers with different stabilizer contents, the light transmittance and strength required according to the part (layer) can be appropriately set in one material for the zirconia sintered body obtained by sintering for a short time. In addition, the difference in the stabilizer content between the layers with different stabilizer contents is preferably 0.1 mol% or more, and from the viewpoint of achieving light transmittance and strength suitable for dental use, it is more preferably 0.3 mol% or more, and further preferably 0.5 mol% or more. Furthermore, the difference in stabilizer content between layers having different stabilizer contents is preferably 3 mol% or less, more preferably 2.5 mol% or less, and further preferably 2 mol% or less from the viewpoint of achieving light transmittance and strength suitable for dental use.

[0064] As the zirconia formed body or zirconia calcined body used in the method for producing a zirconia sintered body of the present invention, from the viewpoint of achieving light transmittance and strength suitable for dental use, it is preferred that: on a straight line extending in a first direction from one end toward the other end of the zirconia calcined body, the content of the stabilizer (suitably yttrium oxide) relative to the total moles of zirconium oxide and the stabilizer from the one end toward the other end does not increase or decrease in a constant manner. In other words, the content of the stabilizer (suitably yttrium oxide) preferably increases or decreases monotonically. Hereinafter, using Figure 1 The calcined zirconium oxide body is shown as a schematic diagram. Figure 1 The increasing tendency or decreasing tendency of the content of the stabilizer does not change in the opposite direction on the straight line extending in the first direction Y from one end P to the other end Q of the zirconia calcined body 10. That is, when the content of the stabilizer tends to decrease on the straight line from the one end P to the other end Q, it is preferred that there is no interval in which the content of the stabilizer substantially increases.

[0065] Examples of the stabilizer include calcium oxide (CaO), magnesium oxide (MgO), yttrium oxide, cerium oxide (CeO2), scandium oxide (Sc2O3), niobium oxide (Nb2O5), lanthanum oxide (La2O3), erbium oxide (Er2O3), praseodymium oxide (Pr6O 11), oxides such as samarium oxide (Sm2O3), europium oxide (Eu2O3) and thulium oxide (Tm2o3). The stabilizer may be used alone or in combination of two or more. The content of the stabilizer in the zirconium oxide calcined body and the sintered body thereof of the present invention can be measured by, for example, inductively coupled plasma (ICP; Inductively Coupled Plasma) emission spectrometry analysis, fluorescent X-ray analysis, etc. In the zirconium oxide calcined body and the sintered body thereof of the present invention, the content of the stabilizer is preferably 0.1 to 18 mol%, more preferably 1 to 15 mol%, and further preferably 2 to 8 mol% relative to the total molar amount of zirconium oxide and the stabilizer. From the viewpoint of the strength and light transmittance of the obtained zirconium oxide sintered body, the zirconium oxide formed body or the zirconium oxide calcined body preferably contains yttrium oxide as a stabilizer. In all the layers of the aforementioned multiple layers of the zirconium oxide formed body or the zirconium oxide calcined body, the content of yttrium oxide is preferably 2.5 mol% or more, more preferably 3 mol% or more, further preferably 3.5 mol% or more, and particularly preferably 3.8 mol% or more relative to the total molar amount of zirconium oxide and yttrium oxide. When the content of yttrium oxide is 2.5 mol% or more, the light transmittance of the zirconium oxide sintered body can be improved. In addition, in all the layers of the aforementioned multiple layers, the content of yttrium oxide is preferably 7.5 mol% or less, more preferably 7.0 mol% or less, further preferably 6.5 mol% or less, and particularly preferably 6.0 mol% or less relative to the total molar amount of zirconium oxide and yttrium oxide. When the content of yttrium oxide is 7.5 mol% or less, the strength reduction of the obtained zirconium oxide sintered body can be suppressed. In a preferred embodiment (X-1), the method for producing a zirconia sintered body includes a plurality of layers containing yttria as a stabilizer contained in a zirconia formed body or a zirconia calcined body, wherein the plurality of layers include two or more layers having different yttria contents, and the layer (Y-1) having the highest yttria content is preferably a plurality of layers containing yttria as a stabilizer contained in the zirconia formed body or the zirconia calcined body. H ) has a yttrium oxide content of 3.5 mol% or more and 7.5 mol% or less, and the layer (Y L ) has a yttrium oxide content of 2.5 mol% or more and 7.0 mol% or less, and the layer (Y H ) in yttrium oxide content / layer (Y L ) satisfies a content of yttrium oxide > 1. In the above-mentioned preferred embodiment (X-1), it is more preferred that the layer (Y H ) has a yttrium oxide content of 3.8 mol% or more and 7.5 mol% or less, and the layer (Y L ) has a yttrium oxide content of 3.0 mol% or more and 6.5 mol% or less, and it is further preferred that the layer (Y H) is greater than or equal to 3.8 mol % and less than or equal to 7.0 mol %, and the yttrium oxide content in the layer (YI) having the lowest yttrium oxide content is greater than or equal to 3.0 mol % and less than or equal to 6.0 mol %.

[0066] In the zirconia formed body or zirconia calcined body of the present invention, it is preferred that at least a portion of the aforementioned stabilizer is not solid-dissolved in zirconia. That a portion of the stabilizer is not solid-dissolved in zirconia can be confirmed, for example, by an XRD diagram. When a peak derived from the stabilizer is confirmed in the XRD diagram of the zirconia calcined body, it indicates that there is a stabilizer that is not solid-dissolved in zirconia in the zirconia formed body or the zirconia calcined body. When all stabilizers are solid-dissolved, basically no peak derived from the stabilizer is confirmed in the XRD diagram. Among them, depending on conditions such as the crystal state of the stabilizer, even if there is no peak of the stabilizer in the XRD diagram, the stabilizer is sometimes not solid-dissolved in zirconia. The main crystal system of zirconia is a tetragonal system and / or a cubic system. When there is no peak of the stabilizer in the XRD diagram, it can be considered that most of the stabilizer, or substantially all of it, is solid-dissolved in zirconia. In the zirconia formed body or zirconia calcined body of the present invention, it may be that all of the stabilizer is not solid-dissolved in zirconia. It should be noted that in the present invention, solid-dissolved stabilizer means, for example, that the element (atom) contained in the stabilizer is solid-dissolved in zirconia.

[0067] In the zirconia formed body or zirconia calcined body of the present invention, the existence ratio of yttrium oxide not dissolved in zirconia (hereinafter sometimes referred to as "undissolved yttrium oxide") is y It can be calculated according to the following mathematical formula (1): The existence rate of undissolved yttrium oxide f y It is preferably greater than 0%, more preferably 1% or more, further preferably 2% or more, and particularly preferably 3% or more. y The upper limit of f may be, for example, 15% or less, depending on the content of yttria in the zirconia formed body or the zirconia calcined body. When the content of yttria is 2.5 mol% or more and less than 4.5 mol%, f y When the content of yttrium oxide is 4.5 mol% or more and less than 5.8 mol%, f y When the content of yttrium oxide is 5.8 mol% or more and less than 7.5 mol%, f y It can be set to 15% or less.

[0068] In the zirconia formed body or the zirconia calcined body of the present invention, when the content of yttria is 2.5 mol% or more and less than 4.5 mol%, f yIt is preferably 0.5% or more, more preferably 1.0% or more, and even more preferably 2.0% or more. When the content of yttrium oxide is 4.5 mol% or more and less than 5.8 mol%, the existence rate of undissolved yttrium oxide is f y When the content of yttrium oxide is 5.8 mol % or more and 7.5 mol % or less, f y In the calcined zirconium oxide of the present invention, when the content of yttrium oxide is 2.5 mol% or more and less than 4.5 mol%, f m / f y It is preferably 20 to 200, more preferably 25 to 100, and even more preferably 30 to 60. When the content of yttrium oxide is 4.5 mol% or more and less than 5.8 mol%, f m / f y It is preferably 5 to 45, more preferably 10 to 40, and still more preferably 15 to 35. When the content of yttrium oxide is 5.8 mol% or more and 7.5 mol% or less, f m / f y It is preferably 2-40, more preferably 5-35, and even more preferably 10-30.

[0069] [Mathematical formula 1]

[0070]

[0071] In mathematical formula (1), I y (111) represents the peak intensity of the (111) plane of yttrium oxide at around 2θ=29° in the XRD pattern based on CuKα radiation. m (111) and I m (11-1) represents the peak intensity of the (111) plane and the (11-1) plane of the monoclinic system of zirconium oxide. t (111) represents the peak intensity of the (111) plane of the tetragonal system of zirconium oxide. c (111) represents the peak intensity of the (111) plane of the cubic crystal system of zirconium oxide.

[0072] For the above mathematical formula (1), by substituting other peaks in place of I y (111) can also be applied to the calculation of the undissolved fraction of stabilizers other than yttrium oxide.

[0073] The main crystal system of zirconium oxide in the zirconium oxide formed body or the zirconium oxide calcined body of the present invention is preferably monoclinic. In the present invention, "the main crystal system is monoclinic" means that the proportion of monoclinic in zirconium oxide calculated by the following mathematical formula (2) is: m In the zirconia formed body or calcined body of the present invention, the ratio of monoclinic crystals in zirconia calculated by the following mathematical formula (2) is: m The proportion of the monoclinic system is preferably 55% or more, more preferably 60% or more, further preferably 70% or more, further preferably 75% or more, particularly preferably 80% or more, more particularly preferably 85% or more, and most preferably 90% or more relative to the total amount of the monoclinic system, tetragonal system, and cubic system. m It can be calculated from the peaks of the X-ray diffraction (XRD) chart using CuKα rays by the following mathematical formula (2): It should be noted that the main crystal system in the zirconia formed body or the zirconia calcined body may contribute to the increase in the shrinkage temperature and the shortening of the sintering time.

[0074] In the zirconia formed body or calcined body of the present invention, peaks of tetragonal and cubic systems are substantially undetectable. That is, the ratio of the monoclinic system is m Can be set to 100%.

[0075] [Mathematical formula 2]

[0076]

[0077] In mathematical formula (2), I m (111) and I m (11-1) represent the peak intensities of the (111) plane and (11-1) plane of the monoclinic system of zirconium oxide, respectively. t (111) represents the peak intensity of the (111) plane of the tetragonal system of zirconium oxide. c (111) represents the peak intensity of the (111) plane of the cubic crystal system of zirconium oxide.

[0078] The zirconia formed body or zirconia calcined body may contain additives as needed. Examples of additives include binders, colorants (including pigments, composite pigments, and fluorescent agents), aluminum oxide (Al2O3), titanium oxide (TiO2), silicon dioxide (SiO2), etc. The additives may be used alone or in combination of two or more.

[0079] Examples of the binder include polyvinyl alcohol, methyl cellulose, carboxymethyl cellulose, acrylic binders, wax binders (paraffin, etc.), polyvinyl butyral, polymethyl methacrylate, ethyl cellulose, polyethylene, polypropylene, ethylene vinyl acetate copolymer, polystyrene, atactic polypropylene, methacrylic resins, and stearic acid.

[0080] Examples of the pigment include oxides of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Pr, Sm, Eu, Gd, Tb, and Er (specifically, NiO, Cr2O3, etc.), preferably oxides of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Pr, Sm, Eu, Gd, and Tb, and more preferably oxides of at least one element selected from the group consisting of Ti, V, Cr, Mn, Fe, Co, Ni, Zn, Y, Zr, Sn, Sb, Bi, Ce, Sm, Eu, Gd, and Tb. In addition, the zirconium oxide formed body or zirconium oxide calcined body of the present invention may not contain Er2O3. Examples of the composite pigments include composite oxides such as (Zr, V) O2, Fe(Fe, Cr) 2 O4, (Ni, Co, Fe) (Fe, Cr) 2 O4·ZrSiO4, and (Co, Zn) Al2 O4. Examples of fluorescent agents include Y2SiO5:Ce, Y2SiO5:Tb, (Y, Gd, Eu) BO3, Y2O3:Eu, YAG:Ce, ZnGa2O4:Zn, BaMgAl 10 O 17 :Eu et al.

[0081] The method for producing the zirconia molded body used in the present invention is not particularly limited, and examples thereof include the following production method, which includes: a step of press-forming a mixed powder containing zirconia (suitably: zirconia powder whose main crystal system is monoclinic) and the above-mentioned stabilizer at a pressure of 175 MPa or more to obtain a zirconia molded body. By press-forming at the above-mentioned pressure, the volume density of the zirconia molded body (and thus the obtained zirconia sintered body) can be increased regardless of the thickness. It should be noted that in this specification, the above-mentioned pressure of 175 MPa or more refers to the maximum pressure during press-forming.

[0082] The method for producing the zirconia calcined body used in the present invention is not particularly limited, and examples thereof include a method for producing a zirconia formed body formed from a raw material powder containing zirconia particles (suitably, zirconia particles whose main crystal system is monoclinic) and a stabilizer, and sintering (i.e., calcining) the zirconia particles at a temperature at which the zirconia particles do not reach sintering. The method for producing a zirconia formed body is as described above. An example of the method for producing a zirconia calcined body of the present invention is described. First, a raw material powder for a zirconia formed body is produced. A mixture is prepared using monoclinic zirconia powder and stabilizer powder (e.g., yttrium oxide powder) to achieve the desired content of the stabilizer (e.g., yttrium oxide). Next, the mixture is added to water to produce a slurry, and wet pulverized and mixed using a ball mill until the desired particle size is reached. The pulverized slurry is dried and granulated using a spray dryer. The obtained powder is calcined at a temperature at which the zirconia particles do not reach sintering (e.g., 800 to 1200°C) to produce a powder (primary powder). Pigments may be added to the primary powder. Afterwards, the primary powder is added to water to prepare a slurry, and wet crushing and mixing is performed using a ball mill until the desired particle size is reached. After adding additives such as a binder to the crushed slurry as needed, it is dried using a spray dryer to prepare a mixed powder (secondary powder). The secondary powder is filled into a specified mold, the upper surface is smoothed to make it flat, an upper mold is set, and the secondary powder is press-formed using a uniaxial press molding machine to obtain a zirconia molded body. As described above, the pressure when the mixed powder is press-formed is preferably above 175 MPa. It should be noted that the obtained zirconia molded body may or may not be further CIP (Cold Isostatic Press) formed.

[0083] The zirconia formed body or zirconia calcined body may have a multilayer structure. When manufacturing a zirconia calcined body with a multilayer structure, the primary powder may be divided into at least 2 parts (preferably 4 parts) in the above manufacturing method in order to make the zirconia formed body with a multilayer structure.

[0084] The density of the calcined zirconium oxide is preferably 2.7 g / cm 3 In addition, the density of the zirconia calcined body is preferably 4.0 g / cm 3 Below, more preferably 3.8 g / cm 3 Below, more preferably 3.6 g / cm 3 If the density is within this range, the molding process can be easily performed. The density can be calculated, for example, in the form of (mass of the calcined body) / (volume of the calcined body).

[0085] In addition, the three-point bending strength of the zirconia calcined body is preferably 15 to 70 MPa, more preferably 18 to 60 MPa, further preferably 20 to 50 MPa, and particularly preferably 20 to 40 MPa. The above-mentioned bending strength can be measured according to ISO 6872:2015, only the size conditions of the test piece are changed, and a test piece with a size of 5 mm×10 mm×50 mm is used for measurement. The surface and C surface of the test piece are surface-finished in the length direction with 600 sandpaper. The test piece is configured in a manner that the widest surface faces the vertical direction (load direction). In the bending test measurement, the spacing is set to 30 mm and the crosshead speed is set to 0.5 mm / min.

[0086] Next, the zirconia formed body obtained by the above operation is pre-calcined to obtain a zirconia calcined body. The pre-calcination temperature is preferably 800°C or higher, more preferably 900°C or higher, and further preferably 950°C or higher. In addition, in order to improve dimensional accuracy, the pre-calcination temperature is preferably 1200°C or lower, more preferably 1150°C or lower, and further preferably 1100°C or lower. It is believed that at this pre-calcination temperature, the stabilizer will not be dissolved.

[0087] In the method for manufacturing a zirconia sintered body of the present invention, under the conditions that the starting temperature, the reaching temperature, the range of the heating rate, and the relationship of HR3 / HR2>1 of each of the above-mentioned heating steps are satisfied, the heating rate of each of the above-mentioned heating steps can be a uniform rate, or it can be changed during the process and set to multiple stages. For example, in a certain embodiment, regarding the second heating step, the temperature can be raised at 50°C / min for 30 seconds from the starting temperature, and after 30 seconds, the temperature can be raised at 10°C / min. In other embodiments, regarding the third heating step, the temperature can be raised at 50°C / min for 30 seconds from the starting temperature, and after 30 seconds, the temperature can be raised at 10°C / min.

[0088] [Stop process]

[0089] In the method for producing a zirconia sintered body of the present invention, the residence time at the highest attainable temperature (maximum sintering temperature) is preferably within 30 minutes, more preferably 10 to 25 minutes, and more preferably 15 to 20 minutes from the viewpoint of further shortening the working time. In addition, the maximum sintering temperature is preferably 1400 to 1750°C, and is preferably 1510°C or higher, more preferably 1530°C or higher, and more preferably 1550°C or higher from the viewpoint of further shortening the working time, further shortening the lightness, light transmittance, and chroma of the obtained zirconia sintered body, and when the zirconia formed body or the zirconia calcined body contains a composite oxide, the color development of the composite oxide is excellent, and the formation of streaks between layers with different yttrium oxide contents is suppressed, the maximum sintering temperature is preferably 1750°C or lower, more preferably 1650°C or lower, and more preferably 1600°C or lower. The dwelling step is preferably immediately after the third temperature rising step. Under the condition that the effect of the present invention is exerted, another temperature rising step may be further provided between the third temperature rising step and the dwelling step. In an embodiment not including a temperature rising step other than the above, the reaching temperature of H3 becomes the highest sintering temperature.

[0090] From the viewpoint of further shortening the operation time, the total calcination time in the calcination process from the start of the temperature increase in the first temperature increase process to the end of the residence time at the maximum calcination temperature is preferably within 120 minutes, more preferably within 90 minutes, and even more preferably within 75 minutes.

[0091] [Cooling process (temperature reduction process)]

[0092] In the method for manufacturing a zirconia sintered body of the present invention, it is preferred to include a step of cooling after maintaining the aforementioned maximum firing temperature for a predetermined time. In the cooling step, the cooling rate from the highest firing temperature in the aforementioned heating step to 800°C is preferably 10°C / min or more, more preferably 30°C / min or more, and further preferably 50°C / min or more. The cooling method may use any one of external air introduction cooling, water cooling, air cooling, slow cooling, and natural cooling, or a combination thereof. The reaching temperature of the cooling step varies depending on the type and performance of the firing furnace, and may be 950°C, 750°C, or 1000°C.

[0093] From the perspective of suitability as a dental product, the color difference ΔE*ab of the zirconium oxide sintered body obtained by the manufacturing method of the present invention is preferably 2.7 or less, more preferably 2.0 or less, further preferably 1.6 or less, and particularly preferably 0.8 or less. The comparative measurement object of the color difference ΔE*ab is the chromaticity of the zirconium oxide sintered body during normal firing (total firing time: 6 to 12 hours). The evaluation method of chromaticity is as described in the examples described below. In addition, in this specification, the aforementioned "total firing time" (also referred to as total firing time) refers to the time in the firing process from the start of the heating of the aforementioned first heating step to the end of the residence time at the aforementioned maximum firing temperature.

[0094] From the perspective of suitability as a dental product, the difference between the lightness index L* of the zirconia sintered body obtained by the manufacturing method of the present invention and the lightness index L* of the zirconia sintered body during normal firing (total firing time: 6 to 12 hours) is preferably 2.0 or less, more preferably 1.5 or less, and further preferably 1.0 or less. The L*, a*, and b* of the zirconia sintered body obtained by the manufacturing method of the present invention can be selected and set according to the target site such as the cervical, body, and incisal.

[0095] The present invention includes various embodiments in which the above-described configurations are combined within the technical concept of the present invention within the scope in which the effects of the present invention are exhibited.

[0096] Example

[0097] Next, embodiments are given to explain the present invention in more detail, but the present invention is not limited to these embodiments at all, and a person having common knowledge in the art can make various modifications within the scope of the technical idea of ​​the present invention.

[0098] [Example 1]

[0099] [Preparation of Raw Material Powder Used in Preparation of Zirconia Calcined Body]

[0100] The method for preparing the raw material powder used to prepare the calcined zirconium oxide used in Example 1 is described. First, a mixture is prepared using monoclinic zirconium oxide powder and yttrium oxide powder in a manner that has the composition described in Table 1 except for the coloring component. Next, the mixture is added to water to prepare a slurry, and wet pulverized and mixed using a ball mill until the average particle size becomes 0.13 μm or less. The pulverized slurry is dried using a spray dryer, and the obtained powder is calcined at a calcination temperature of 950°C for 2 hours to prepare a powder (primary powder). It should be noted that the above-mentioned average particle size can be obtained by a laser diffraction scattering method. Specifically, the laser diffraction scattering method can be used, for example, with a laser diffraction particle size distribution measuring device (SALD-2300: manufactured by Shimadzu Corporation), using a 0.2% sodium hexametaphosphate aqueous solution as a dispersion medium, and measuring on a volume basis. It should be noted that the yttrium oxide content in Table 1 refers to the yttrium oxide content relative to the total mole of zirconium oxide and yttrium oxide.

[0101] To the obtained primary powder, a coloring component was added in the composition described in Table 1. Thereafter, the powder to which the coloring component was added was added to water to prepare a slurry, and wet pulverization and mixing were performed using a ball mill until the average particle size became 0.13 μm or less. After adding a binder to the pulverized slurry, it was dried using a spray dryer to prepare a powder (secondary powder). The prepared secondary powder was used as a raw material powder to manufacture a zirconia calcined body described later.

[0102] [Preparation of a block of calcined zirconia body]

[0103] Next, a method for manufacturing a block of a zirconia calcined body used for manufacturing a zirconia sintered body in the shape of a tooth crown is described. First, 15 g of each of the first layer raw material powder and the second layer raw material powder described in Table 1 are filled in a mold having an inner size of 20 mm × 25 mm, and the mold is pressed at 300 kg / cm using a uniaxial press molding machine. 2 The primary press molding was performed for 90 seconds under a surface pressure of 1700 kg / cm 2 CIP molding was performed for 5 minutes to produce a laminated structure molded body. The obtained molded body was fired at 1000° C. for 2 hours to produce a block of zirconia calcined body.

[0104] The obtained block of the zirconia calcined body was cut into the shape described in the evaluation of each characteristic described later, and sintered according to the sintering process described in Table 2. The results of the evaluation of each characteristic are described later. It should be noted that, regarding the evaluation of ΔL (WB) of the zirconia sintered body, a zirconia sintered body of each layer was prepared as described later and evaluated.

[0105] [Examples 2 to 5, Comparative Example 1 and Reference Example 1]

[0106] Secondary powder was prepared and a block of zirconia calcined body was prepared in the same manner as in Example 1. Zirconia sintered body was prepared in the same manner as in Example 1 except that the firing process was changed as described in Tables 2 and 3, and various properties were evaluated.

[0107] [Evaluation of ΔL(WB) of Each Layer of Zirconia Sintered Body]

[0108] For each of the zirconia sintered bodies of Examples 1 to 5, Comparative Example 1 and Reference Example 1, the zirconia sintered bodies of the first layer and the second layer described in Table 1 were prepared by the following method, and (L*, a*, b*) based on the L*a*b* colorimetric system (JIS Z8781-4: 2013 Colorimetry - Part 4: CIE 1976 L*a*b* color space) was measured. In addition, ΔL(WB) obtained from each (L*, a*, b*) of the zirconia sintered body was calculated. Using the L value (L1*) of the zirconia sintered body when measured against a white background and the L value (L2*) of the zirconia sintered body when measured against a black background, ΔL(WB) was calculated using the following formula (1).

[0109] ΔL(WB)=(L1*)-(L2*) (1)

[0110] First, the size was adjusted in advance and press-formed in such a way as to obtain a zirconia sintered body with a thickness of 1.2 mm, thereby producing a molded body composed of the raw material powder in each layer. Next, the molded body was sintered at 1000°C for 2 hours to produce a zirconia calcined body. As a sintering furnace, InFire HTC speed (manufactured by DENTSPLY SIRONA) was used, and the zirconia calcined body was sintered according to the sintering process shown in Tables 2 and 3 to produce a zirconia sintered body. Both sides of the obtained zirconia sintered body were polished with #600 abrasive paper to produce a zirconia sintered body with a thickness of 1.2 mm. Then, a dental colorimetric device (7band LED light source, Crystaleye) (manufactured by Olympus) was used to measure each layer on a white background and a black background (n=3). The average value of n=3 was used as the evaluation result and is shown in Tables 2 and 3.

[0111] [Evaluation of the aesthetic properties of zirconia sintered bodies in the shape of tooth crowns]

[0112] For the zirconia sintered bodies of each of Examples 1 to 5, Comparative Example 1 and Reference Example 1, the aesthetics were evaluated visually from the perspective of comparison with the appearance of natural teeth using the following method. When evaluating, a commercially available tooth color plate having the same appearance as natural teeth can be used. Specifically, commercially available tooth color plates include, for example, the tooth color plate VITA Classical (trade name) manufactured by VITA. First, using DWX-52DC (manufactured by Roland DG) as a processing machine, the shape of the crown of the front teeth was cut from the block of the obtained zirconia calcined body. For the obtained cut zirconia calcined body, InFire HTC speed (manufactured by DENTSPLY SIRONA) was used as a sintering furnace, and sintering was performed according to the sintering process of Tables 2 and 3 to obtain the zirconia sintered bodies of each of the Examples and Comparative Examples.

[0113] The obtained zirconia sintered body was evaluated by visual inspection of four persons according to the following criteria. When three or more of the four persons judged that a certain criterion was satisfied, the criterion was judged to be satisfied. The results are shown in Tables 2 and 3.

[0114] <Evaluation Criteria>

[0115] ○: No streaks were observed between the layers with different yttrium oxide contents, and there was no problem in dental clinical evaluation.

[0116] △: There are slight streaks between the layers with different yttrium oxide contents, but this is within the acceptable range in terms of dental clinical evaluation.

[0117] ×: The stripes between the layers with different yttrium oxide contents are noticeable and unacceptable in clinical evaluation

[0118] [Strength Evaluation of Zirconia Sintered Body]

[0119] The strength of the zirconia sintered bodies of Examples 1 to 5, Comparative Example 1 and Reference Example 1 was confirmed using the following method. First, DWX-52DC (manufactured by Roland DG) was used as a processing machine to cut out 10 rectangular samples of 1.7 mm × 5.2 mm × 20.2 mm from the obtained zirconia calcined body block. InFire HTC speed (manufactured by DENTSPLY SIRONA) was used as a sintering furnace to sinter the cut zirconia calcined body under the conditions of the sintering process shown in Tables 2 and 3. Using a rotating grinding disc, the sintered zirconia sintered body was ground with #1000 grinding paper to produce a sintered body sample of 1.2 mm × 4 mm × 14 mm in the shape of a rectangular parallelepiped. The sintered body sample was used to measure the three-point bending strength (n=10) under the conditions of a crosshead speed of 0.5 mm / min and a support point distance (span) of 12 mm in accordance with ISO 6872:2015. The average value of n=10 is shown in Tables 2 and 3 as the evaluation results.

[0120] [Evaluation of ΔE*ab of zirconia sintered body in the shape of tooth crown]

[0121] The color difference ΔE*ab (hereinafter also referred to as "ΔE**") between the zirconia sintered bodies of Examples 1 to 5 and Comparative Example 1 and the zirconia sintered bodies fired according to the usual firing process, i.e., the firing process described in Reference Example 1, was calculated by the following method, and the difference in color tone was confirmed. First, the obtained zirconia sintered body block was cut into a crown shape of anterior teeth using DWX-52DC (manufactured by Roland DG) as a processing machine. The obtained zirconia sintered bodies after cutting were fired into samples of the same shape according to the firing processes described in Tables 2 and 3 using InFireHTC speed as a firing furnace. The fired sintered body samples were colorimetrically measured using a dental colorimetric device (manufactured by Olympus Corporation, 7-band LED light source, "Crystaleye"), and the L*a*b* colorimetric system (JIS Z 8781-4: 2013 Colorimetry - Part 4: CIE 9000) was evaluated at each measurement site of the tooth neck, main body, and incisal edge. The lightness, chroma, and color difference ΔE*ab (n=5) in the CIE 1976 L*a*b* color space were calculated. The average value of n=5 is shown in Table 4 as the evaluation result. The color difference ΔE*ab was calculated as follows: using the lightness index L* and chromaticity coordinates a* and b* in the CIE 1976 L*a*b* color space, the color difference ΔE*ab was calculated using the following formula (2) for two samples of the sintered body samples obtained according to the sintering process described in Tables 2 and 3.

[0122] ΔE*={(L1*-L2*) 2 +(a1*-a2*)2 +(b1*-b2*) 2} 1 / 2 (2)

[0123] [Evaluation of various physical properties]

[0124] In Examples 1, 3 to 5 and Reference Example 1, it was confirmed that the difference in ΔL(WB) values ​​in each layer of the zirconia sintered body was 0.79 to 1.03, and in the evaluation of the aesthetics of the zirconia sintered body in the shape of a crown, the stripes between the layers with different yttria contents were not noticeable, and there was no problem in the dental clinical evaluation. In addition, in the evaluation of the strength of the zirconia sintered body, the three-point bending strength of the sintered body sample showed a value equivalent to that of the case where the sintering was carried out according to the usual sintering process (Reference Example 1), which was a strength that was not a problem for dental use. In the evaluation of ΔE*ab of the zirconia sintered body in the shape of a crown, the color difference ΔE*ab compared with the fired sample fired according to the usual sintering process was 2.7 or less.

[0125] In Example 2, the difference in ΔL(WB) values ​​between the layers of the zirconia sintered body was 1.45. In the evaluation of the aesthetics of the zirconia sintered body in the shape of a crown, there were slight streaks between the layers with different yttria contents, but in terms of dental clinical evaluation, it was within an acceptable range. In the evaluation of the strength of the zirconia sintered body, the three-point bending strength of the sintered body sample showed a value equivalent to that of the case where the sintering was carried out according to the usual sintering process, and it was a strength that was not problematic for dental use. In the evaluation of ΔE*ab of the zirconia sintered body in the shape of a crown, the color difference ΔE*ab compared with the fired sample fired according to the usual sintering process was 2.7 or less.

[0126] On the other hand, in Comparative Example 1, the three-point bending strength and ΔE* value that are not problematic for dental use are shown, but the difference in ΔL(WB) values ​​in each layer of the zirconia sintered body is 2.7. In the evaluation of the aesthetics of the zirconia sintered body in the shape of a crown, the stripes between the layers with different yttrium oxide contents are conspicuous, which is an unacceptable result in clinical evaluation. As a reason for the increase in the difference in ΔL(WB) values ​​as in Comparative Example 1, it can be considered that: a firing process occurs in which the temperature band that affects light transmittance and color tone gradually rises at a constant rate. In Patent Document 2 (Japanese Patent Table No. 2019-524298), as shown in FIG. 3, a firing curve at 1000°C and thereafter is a stage, that is, a firing process that gradually rises at a constant rate, so it can be considered that it is the same result as Comparative Example 1.

[0127] [Table 1]

[0128]

[0129] [Table 2]

[0130]

[0131] [Table 3]

[0132]

[0133] [Table 4]

[0134]

[0135] The above results confirm that the zirconia sintered body obtained by the production method of the present invention can suppress the occurrence of streaks between layers with different yttria contents even if the sintering time is short, and is therefore suitable as a dental product (e.g., a dental prosthesis). Furthermore, it can be confirmed that the zirconia sintered body obtained by the production method of the present invention can reproduce the color tone and strength of a dental prosthesis to the same extent as when sintered under normal sintering conditions (total sintering time: 6 to 12 hours) even if sintered in a short time.

[0136] Industrial Applicability

[0137] The method for producing a zirconia sintered body of the present invention can sinter a zirconia formed body or a zirconia calcined body in a short time, and the obtained zirconia sintered body can suppress the generation of striations between layers having different yttria contents, and is therefore useful in the production of dental products (dental prostheses, etc.). Furthermore, the obtained zirconia sintered body can reproduce the aesthetic requirements (color tone and light transmittance) and strength of an ideal dental prosthesis to the same extent as when fired under ordinary firing conditions, even though it is sintered in a short time, and has an excellent color tone and light transmittance like the incisal edge of a natural front tooth, and is therefore useful as a method for producing a dental prosthesis such as a denture for anterior teeth.

[0138] 10 Zirconia sintered body

[0139] P-end

[0140] QThe other end

[0141] LFull length

[0142] Y first direction

Claims

1. A method for producing a zirconia sintered body, comprising a firing step of firing a zirconia formed body or a zirconia calcined body, The zirconia formed body or zirconia calcined body comprises a plurality of layers containing a stabilizer, The plurality of layers include layers having different stabilizer contents. The sintering step includes at least three stages of heating steps, namely, a first heating step (H1), a second heating step (H2), and a third heating step (H3). The heating rate of the second heating step (H2) is set to HR2. When the temperature increase rate in the third temperature increase step (H3) is set to HR3, HR2 is more than 0℃ / min and less than 50℃ / min, HR3 is 5℃ / min or more and 150℃ / min or less, HR3 / HR2>1, The starting temperature in each temperature rising step is 1000°C or less in H1, more than 1250°C and less than 1450°C in H2, and more than 1450°C and less than 1550°C in H3. The reaching temperature in each temperature rising step is more than 1250° C. and 1450° C. or less in H1, 1450° C. or more and 1550° C. or less in H2, and 1500° C. or more and 1750° C. or less in H3.

2. The method for producing a zirconia sintered body according to claim 1, wherein: When the temperature increase rate in the first temperature increase step (H1) is denoted as HR1, HR1 is 40 to 500°C / min.

3. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: The difference in the content of the stabilizer between the layers having different contents of the stabilizer is 0.1 mol % or more.

4. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: The stabilizer is yttrium oxide.

5. The method for producing a zirconia sintered body according to claim 4, wherein: The content of the yttrium oxide in all of the plurality of layers is 2.5 mol % or more and 7.5 mol % or less relative to the total mole of zirconium oxide and yttrium oxide.

6. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: HR2 is 2~30℃ / min.

7. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: HR3 is 10~100℃ / min.

8. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: HR3 / HR2>1.

5.

9. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: The maximum sintering temperature in the temperature raising step is 1500 to 1750° C., and the residence time at the maximum sintering temperature is within 30 minutes. 10 . The method for producing a zirconia sintered body according to claim 9 , further comprising a temperature reduction step, wherein a temperature reduction rate from the highest sintering temperature in the temperature increase step to 800° C. is 10° C. / min or more.

11. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: The total calcination time in the calcination step from the start of the temperature increase in the first temperature increase step (H1) to the end of the residence time at the maximum calcination temperature is within 120 minutes.

12. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: More than 55% of the zirconia formed body or the zirconia calcined body is monoclinic.

13. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: In the zirconia formed body or the zirconia calcined body, at least a part of the stabilizer is not solid-dissolved in the zirconia.

14. The method for producing a zirconia sintered body according to claim 1 or 2, wherein: The zirconia formed body or calcined zirconia body has a predetermined shape of a dental product.

15. The method for producing a zirconia sintered body according to claim 14, wherein: The dental product is a dental prosthesis.