A method for preparing a quartz tube

By grinding the inner wall of the quartz tube, the problem of increasing inner wall stress caused by polycrystalline silicon thin film deposition is solved, and the stability and service life of the quartz tube are improved.

CN116217054BActive Publication Date: 2024-11-29ZHEJIANG JINGSHENG PHOTONICS TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202211730102.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-12-27
Publication Date
2024-11-29
Estimated Expiration
2042-12-27

AI Technical Summary

Technical Problem

During the manufacturing process of quartz tubes, the inner wall stress increases due to the deposition of polycrystalline silicon thin film, which affects stability and service life.

Method used

The inner wall surface of the quartz tube is polished by a grinding machine to form a frosted surface, increasing the surface area and focus point of the inner wall to avoid uneven deposition of the polycrystalline silicon film.

Benefits of technology

It improves the overall uniformity of the quartz tube, reduces the inner wall stress, and extends the service life of the quartz tube.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116217054B_ABST
    Figure CN116217054B_ABST
Patent Text Reader

Abstract

The present invention provides a method for preparing a quartz tube, which comprises the following steps: S1, adding quartz raw material into a crucible, heating the crucible with a heating device, so that the quartz raw material in the crucible forms a quartz liquid, S2, passing the quartz liquid into a former inside the crucible, and using a tube drawing machine to draw the quartz liquid flowing out of the former into a quartz tube, S3, cutting the quartz tube with a cutting device, S4, grinding the inner wall surface of the quartz tube with a grinder, and S5, cleaning the ground quartz tube. The quartz tube manufactured by the method for preparing the quartz tube of the embodiment of the present invention has the advantages of good stability and long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of quartz tube production, and in particular to a method for preparing a quartz tube. Background Art

[0002] In the manufacturing process of the quartz tube in the related art, since the polysilicon film deposited by LPCVD (low pressure chemical vapor deposition) is formed by thermal decomposition of silane, and the inlet of silane is toward the inner wall of the quartz tube, the polysilicon film deposited on the inner wall of the quartz tube becomes thicker and thicker with the increase of deposition times, making the uniformity of the polysilicon film deposited on the silicon wafer worse, thereby affecting the stability of the quartz tube. In addition, as the polysilicon film accumulates on the inner wall of the quartz tube, the stress of the inner wall of the quartz tube increases and becomes fragile, thereby shortening the service life of the quartz tube. Summary of the invention

[0003] The present invention aims to solve one of the technical problems in the related art at least to a certain extent.

[0004] To this end, an embodiment of the present invention provides a method for preparing a quartz tube. The quartz tube manufactured by the preparation method has the advantages of good stability and long service life.

[0005] The method for preparing the quartz tube according to the embodiment of the present invention comprises the following steps:

[0006] S1, adding quartz raw material into a crucible, and heating the crucible by using a heating device to form a quartz liquid from the quartz raw material in the crucible;

[0007] S2, passing the quartz liquid into the former inside the crucible, and using a tube drawing machine to draw the quartz liquid flowing out of the former into a quartz tube;

[0008] S3, using a cutting device to cut the quartz tube;

[0009] S4, grinding the inner wall surface of the quartz tube by using a grinder;

[0010] S5. Cleaning the quartz tube after the sandblasting process.

[0011] In the preparation method of the quartz tube of the embodiment of the present invention, the inner wall surface of the quartz tube is polished, which can make the overall uniformity of the quartz tube better and avoid the increase of the stress of the inner wall of the quartz tube, thereby improving the stability and service life of the quartz tube.

[0012] Therefore, the quartz tube manufactured by the preparation method of the quartz tube according to the embodiment of the present invention has the advantages of good stability and long service life.

[0013] In some embodiments, in step S5, the quartz tube after sandblasting is cleaned by water washing.

[0014] In some embodiments, in step S5, the quartz tube after the sandblasting treatment is first cleaned by acid washing, and then the quartz tube after the acid washing is cleaned by water washing.

[0015] In some embodiments, the following steps are also included:

[0016] S7, performing a size inspection on the cleaned quartz tube, wherein the inspection of the quartz tube includes measuring whether the length dimension of the quartz tube, the thickness dimension of the tube wall of the quartz tube, and the diameter dimension of the quartz tube meet a preset range.

[0017] In some embodiments, step S7 further includes: detecting the completeness of the polishing of the inner wall surface of the quartz tube.

[0018] In some embodiments, if the sandblasting of the inner wall of the quartz tube is detected to be missing or missing, steps S4-S6 are repeated.

[0019] In some embodiments, in step S4, the mesh size of the inner wall surface of the polished quartz tube is detected. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 It is a schematic flow chart of a method for preparing a quartz tube according to an embodiment of the present invention. DETAILED DESCRIPTION

[0021] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.

[0022] As shown in the figure, the method for preparing the quartz tube according to the embodiment of the present invention comprises the following steps:

[0023] S1. Add quartz raw material into a crucible, and heat the crucible with a heating device to form quartz liquid from the quartz raw material in the crucible. The heating device generally uses a high-temperature boiler for heating, that is, the crucible with the quartz raw material is placed in the high-temperature boiler, and the temperature in the high-temperature boiler is heated to 1800°C-2300°C, so as to liquefy the quartz raw material more quickly to form quartz liquid.

[0024] S2, passing the quartz liquid into the former inside the crucible, and using a tube drawing machine to draw the quartz liquid flowing out of the former into a quartz tube. It should be noted that the bottom of the crucible has a former, and the quartz raw material is liquefied to form a quartz liquid, which can flow into the former through a pipeline connected to the former, so as to facilitate the subsequent drawing and forming using the tube drawing machine.

[0025] S3. Cut the quartz tube using a cutting device. It is understandable that the cutting device may be a cutting machine. Specifically, taking the quartz tube used in the solar tube device as an example, the quartz tube is cut into a desired length using a cutting device, and the length is generally 2800 mm-3500 mm. Of course, the quartz tube may also be cut according to the specific usage scenario so that the quartz tube is adapted to its installation position.

[0026] S4, grinding the inner wall of the quartz tube using a grinder. It is understandable that grinding the inner wall of the quartz tube using a grinder not only forms a frosted surface on the inner wall of the quartz tube, but also increases the surface area of ​​the inner wall of the quartz tube.

[0027] It should be noted that during the use of the quartz tube, amorphous silicon can be deposited on the inner wall of the quartz tube. If the inner wall of the quartz tube is relatively smooth, the fulcrum point of the inner wall of the quartz tube will be single, so amorphous silicon will accumulate on the inner wall of the quartz tube, thereby increasing the damage to the quartz tube.

[0028] Therefore, in the preparation method of the quartz tube of the embodiment of the present invention, the inner wall surface of the quartz tube is polished to form a frosted surface on the inner wall surface of the quartz tube, thereby increasing the fulcrum points of the inner wall surface of the quartz tube, so that the deposited polysilicon can be more evenly and more easily attached to the inner wall surface of the quartz tube, thereby reducing the damage to the quartz tube caused by the stress generated by the stacking of polysilicon.

[0029] In addition, grinding the inner wall of the quartz tube using a grinder can also increase the area of ​​the inner wall of the quartz tube, which is further beneficial to the deposition of polysilicon.

[0030] Preferably, after the inner wall surface of the quartz tube is polished by a grinder, the mesh number of the inner wall surface of the polished quartz tube is detected so that the mesh number of the inner wall surface of the quartz tube is 500-1000 mesh. If the mesh number of the inner wall surface of the quartz tube is not within the range of 500-1000 mesh, the inner wall surface of the quartz tube can be polished again accordingly, or the grinding disk of the grinder can be replaced.

[0031] S6. Cleaning the polished quartz tube. It is understandable that after polishing the inner wall of the quartz tube, some impurities such as dust adhering to the inner wall of the quartz tube will inevitably remain on the inner wall of the quartz tube, which may affect the stability of the quartz tube in subsequent use.

[0032] Therefore, optionally, the polished quartz tube is washed with water to remove impurities such as dust attached to the wall surface of the quartz tube.

[0033] Preferably, the polished quartz tube can be first pickled, that is, the wall of the quartz tube is cleaned by acidic solution (such as hydrofluoric acid solution, hydrochloric acid solution, etc.), and then the quartz tube is cleaned again by water washing to further improve the degree of cleaning the wall of the quartz tube.

[0034] In other words, the preparation method of the quartz tube in the embodiment of the present invention adopts the grinding treatment on the inner wall surface of the quartz tube, which can make the overall uniformity of the quartz tube better and also avoid the increase of the stress on the inner wall of the quartz tube, thereby improving the stability and service life of the quartz tube.

[0035] Therefore, the quartz tube manufactured by the preparation method of the quartz tube according to the embodiment of the present invention has the advantages of good stability and long service life.

[0036] In some embodiments, the preparation method of the quartz tube of the embodiment of the present invention also includes the following steps: S6, performing size detection on the quartz tube after cleaning, wherein the detection of the quartz tube includes measuring the length dimension of the quartz tube, the thickness dimension of the quartz tube wall and the diameter dimension of the quartz tube to see whether they meet the preset range.

[0037] It can be understood that, taking the quartz tube used in solar tube equipment as an example, the inspection of the quartz tube is: to inspect whether the length of the quartz tube is between 2800mm-3500mm, to inspect whether the wall thickness of the quartz tube is between 1mm-10mm, and to inspect whether the diameter of the quartz tube is between 420mm-520mm, so as to determine whether the produced quartz tube meets the standards.

[0038] In some embodiments, step S6 also includes: detecting the completeness of the polishing of the inner wall surface of the quartz tube.

[0039] It is understandable that after the quartz tube passes the size inspection, it is also necessary to inspect the completeness of the inner wall surface of the quartz tube. That is, during the grinding process, due to the influence of human or equipment factors, the inner wall surface of the quartz sand may be missing or chipped. If the completeness of the inner wall surface of the quartz tube is not inspected and the quartz tube is installed in the equipment for use, the polysilicon may be unevenly deposited on the inner wall surface of the quartz tube, thereby causing the inner wall stress of the quartz tube to increase and become brittle, thereby shortening the service life of the quartz tube.

[0040] Therefore, if the grinding of the inner wall of the quartz tube is detected to be missing or missing, steps S4-S6 are repeated. In other words, when the inner wall of the quartz tube is missing or missing, grinding, cleaning, size detection and the completeness of the grinding of the inner wall of the quartz tube can be performed in sequence to ensure the final quality of the quartz tube.

[0041] In the description of the present invention, it is to be understood that the terms “center”, “longitudinal”, “lateral”, “length”, “width”, “thickness”, “up”, “down”, “front”, “back”, “left”, “right”, “vertical”, “horizontal”, “top”, “bottom”, “inside”, “outside”, “clockwise”, “counterclockwise”, “axial”, “radial”, “circumferential”, etc., indicating orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as limiting the present invention.

[0042] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0043] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral one; it can be a mechanical connection, an electrical connection, or communication with each other; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0044] In the present invention, unless otherwise clearly specified and limited, a first feature being "above" or "below" a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being "above", "above" or "above" a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being "below", "below" or "below" a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.

[0045] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0046] Although the above embodiments have been shown and described, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. Changes, modifications, substitutions and variations of the above embodiments by those of ordinary skill in the art are all within the scope of protection of the present invention.

Claims

1. A method for preparing a quartz tube, characterized in that: The following steps are involved: S1, adding quartz raw material into a crucible, and heating the crucible by using a heating device to form a quartz liquid from the quartz raw material in the crucible; S2, passing the quartz liquid into the former inside the crucible, and using a tube drawing machine to draw the quartz liquid flowing out of the former into a quartz tube; S3, using a cutting device to cut the quartz tube; S4, grinding the inner wall surface of the quartz tube by using a grinding machine; S5, cleaning the polished quartz tube; In step S4, the inner wall surface of the quartz tube is formed into a frosted surface, and the mesh number of the inner wall surface of the quartz tube after grinding is detected, so that the mesh number of the inner wall surface of the quartz tube is 500 meshes-1000 meshes.

2. The method for preparing a quartz tube according to claim 1, characterized in that: In step S5, the polished quartz tube is cleaned by water washing.

3. The method for preparing a quartz tube according to claim 1, characterized in that: In step S5, the polished quartz tube is first cleaned by pickling, and then cleaned by water.

4. The method for preparing a quartz tube according to any one of claims 1 to 3, characterized in that: The following steps are also included: S6. Performing a size inspection on the cleaned quartz tube, wherein the inspection of the quartz tube includes measuring whether the length of the quartz tube, the thickness of the wall of the quartz tube, and the diameter of the quartz tube meet a preset range.

5. The method for preparing a quartz tube according to claim 4, characterized in that: In step S6, the process also includes: detecting the completeness of the polishing of the inner wall surface of the quartz tube.

6. The method for preparing a quartz tube according to claim 5, characterized in that: If omissions or missing corners are found on the inner wall of the quartz tube, steps S4-S6 are repeated.

Citation Information

Patent Citations

  • Continuous melting method for producing flange for semiconductor industry

    CN107117799A

  • Quartz tube production method

    CN114804595A