A Cu2O-Bi2O3 composite material with photocatalytic performance and preparation method thereof

By recombining Cu2O with Bi2O3 under alkaline conditions, adjusting the energy band structure to reduce the recombination efficiency of photogenerated carriers, the instability and toxic raw materials of Cu2O and Bi2O3 photocatalytic materials under oxidation conditions are solved, and efficient Photocatalytic performance and green environmental protection preparation process.

CN116251598BActive Publication Date: 2024-11-15HUANGSHAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310343948.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-03
Publication Date
2024-11-15
Estimated Expiration
2043-04-03

AI Technical Summary

Technical Problem

The existing Cu2O and Bi2O3 photocatalytic materials are unstable under oxidation conditions, and the photogenerated electrons and holes are rapidly recombined, resulting in low catalytic efficiency, and the raw materials used during the preparation process are toxic and harmful, affecting environmental protection.

Method used

The preparation method of Cu2O-Bi2O3 composite material is adopted. The Cu2O-Bi2O3 composite is reacted with a sodium hydroxide solution under alkaline conditions to form Cu2O and Bi2O3 composites, and the energy band structure is adjusted to reduce the recombination efficiency of photogenerated carriers. The Cu2O-Bi2O3 composite powder with excellent photocatalytic properties was obtained by ultrasonic and water bath treatment.

Benefits of technology

The photocatalytic performance of Cu2O-Bi2O3 composite material is significantly improved, the electron transfer capacity is enhanced, and the entire preparation process is green and environmentally friendly, with high safety, and the degradation rate reaches about 70%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116251598B_ABST
    Figure CN116251598B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of composite materials, and in particular, is a Cu2O-Bi2O3 composite material with photocatalytic performance and a preparation method thereof. The present invention successfully prepares a Cu2O-Bi2O3 composite material in an orange juice system under alkaline conditions of pH 11 to 13, using green biomolecules in orange juice as a reducing agent, and using copper sulfate pentahydrate, bismuth nitrate pentahydrate and bismuth trioxide as raw materials. The Cu2O and Bi2O3 of the present invention have staggered valence band and conduction band positions. After the Cu2O-Bi2O3 composite material is formed, the recombination efficiency of the photogenerated electrons and holes is greatly reduced, the electron transfer ability is enhanced, and the experimental process is green and environmentally friendly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite materials, and in particular relates to a Cu2O-Bi2O3 composite material with photocatalytic performance and a preparation method thereof. Background Art

[0002] For a long time, with the advent and progress of the industrial age, energy and environmental problems have become increasingly prominent. Photocatalytic technology is a new treatment method that is green, environmentally friendly, sustainable, and can effectively solve environmental pollution and energy shortage problems. It can catalytically degrade heavy metal ions, decompose water to produce hydrogen, reduce carbon dioxide, and degrade organic matter. People have been pursuing the use of photocatalytic sewage treatment technology to replace traditional sewage treatment technology in sewage treatment. There is no doubt that photocatalytic technology, which converts solar energy into chemical energy and electrical energy by using semiconductor materials and can effectively use sunlight to remove organic pollutants and harmful bacteria, has always been considered one of the most practical and widely used technologies in water treatment. In particular, photocatalytic degradation of pollutants under visible light is considered to be a promising sewage treatment method that can use inexhaustible solar energy to solve the global energy crisis. Due to its huge practical application potential, photocatalytic technology has attracted continuous attention and extensive research from researchers at home and abroad. Therefore, it is very necessary to develop photocatalysts with high efficiency and excellent photocatalytic performance. Cuprous oxide (Cu2O) and bismuth trioxide (Bi2O3) both have important development prospects in the field of photocatalytic degradation of pollutants and are photocatalytic materials with good performance.

[0003] Cu2O is a typical metal-vacancy p-type semiconductor material with a narrow band gap (2.17eV) and can be excited by visible light. It has excellent optical, photoelectric, catalytic, and sensing properties, which has attracted widespread attention from researchers. Since Cu2O can absorb visible light, there are still few materials with excellent responsiveness to visible light. Therefore, Cu2O has been widely used in the research of photocatalytic degradation in recent years. However, the instability of single Cu2O under oxidative conditions, the rapid recombination of photogenerated electrons and holes during the reaction, and the transformation of crystal structure have affected its application in the field of photocatalysis, and Cu2O itself has serious photocorrosion. Therefore, it is still necessary to further improve the photocatalytic properties of Cu2O. Bi2O3 is a p-type semiconductor with excellent physical and chemical properties. The spectral response range is one of the important indicators for evaluating the performance of photocatalysts, but the spectral response range of Bi2O3 is narrow. The wide band gap (2.8eV) of Bi2O3 makes it only absorb part of the visible light with a wavelength less than 450nm, which has a great impact on the utilization rate of sunlight. In addition, the photogenerated carriers of Bi2O3 are easy to recombine, that is, the separation probability of photogenerated carriers generated by Bi2O3 when excited by light is low, which seriously affects its catalytic efficiency.

[0004] In addition, the raw materials used in the preparation of composite materials containing Cu2O or Bi2O3 are mostly toxic and harmful, which reduces the safety of the experiment and is not conducive to environmental protection. Summary of the invention

[0005] In order to overcome the defects in the above-mentioned prior art, the present invention provides a Cu2O-Bi2O3 composite material with photocatalytic performance and a preparation method thereof. The Cu2O-Bi2O3 composite material prepared by the present invention has a significantly reduced recombination efficiency of photogenerated electrons and holes, enhanced electron transfer ability, and the experimental process is green and environmentally friendly.

[0006] To achieve one of the above purposes, the present invention adopts the following technical solution:

[0007] A method for preparing a Cu2O-Bi2O3 composite material with photocatalytic performance comprises the following steps:

[0008] S1. Preparation of copper sulfate orange juice mixed solution: Weigh copper sulfate pentahydrate solid and dissolve it in the upper clear liquid after centrifugation of orange juice to prepare 35-55 mL of Cu 2+ A mixed solution of copper sulfate and orange juice with a concentration of 0.05-0.25 mol / L;

[0009] S2. Preparation of Bi2O3: Weigh 2.5-3.5 g of bismuth nitrate pentahydrate solid and add it to 5-15 mL of dilute nitric acid solution to prepare a mixed solution, slowly drip the prepared 6-9 mol / L sodium hydroxide solution into the mixed solution, and adjust the pH of the mixed solution to alkaline; then keep the obtained alkaline mixed solution warm in a water bath, take it out, centrifuge it, rinse it to obtain a precipitate, and then dry, grind, calcine, cool, and grind the precipitate to obtain Bi2O3 powder;

[0010] S3, weigh 2-3g of the Bi2O3 solid in step S2 and disperse it in the copper sulfate orange juice mixed solution in step S1 and continue stirring, then take out the obtained mixed solution and put it into an environment of 50℃-60℃ for ultrasonic treatment;

[0011] S4. Slowly drip the prepared sodium hydroxide solution into the ultrasonic mixed solution in step S3, and adjust the pH of the mixed solution to be alkaline; when the mixed solution gradually changes from yellow-green to red-brown, continue to ultrasonicate the mixed solution and keep it warm, reheat it and keep it warm, and then cool, dry and grind it in sequence to obtain Cu2O-Bi2O3 powder.

[0012] Preferably, in step S2, the concentration of the dilute nitric acid solution is 1 mol / L.

[0013] Preferably, in step S2, the precipitate is dried in a constant temperature forced air drying oven at a temperature of 80°C, ground and then calcined in a box-type electric furnace at a temperature of 450°C for two hours; after calcination, it is taken out after cooling, and the obtained product is ground again to obtain Bi2O3 powder.

[0014] Preferably, in step S1, the beaker containing the mixed solution is placed in a water bath at a temperature of 55°C and continuously stirred magnetically to make it uniformly mixed, and 35-55 mL of Cu 2+ A mixed solution of copper sulfate and orange juice with a concentration of 0.05-0.25 mol / L.

[0015] Preferably, the pH values ​​of the mixed solution in step S2 and the mixed solution in step S4 are both 11-13.

[0016] Preferably, in step S4, the mixed solution gradually changes from yellow-green to reddish brown, and the mixed solution is continued to be ultrasonicated and kept warm for 2-4 hours; the obtained mixture is transferred to a hydrothermal synthesis reactor, heated to 55°C and kept warm for 2-4 hours, taken out and cooled at room temperature, and finally the product is centrifuged and dried in a constant temperature forced air drying oven at 80°C, and ground again to obtain Cu2O-Bi2O3 powder.

[0017] Preferably, the sodium hydroxide solution is prepared by dissolving sodium hydroxide particles in pure water.

[0018] To achieve the second of the above objectives, the present invention provides a Cu2O-Bi2O3 composite material with photocatalytic performance, wherein the particle size of the composite material is 0.6 μm-5 μm.

[0019] The advantages of the present invention are:

[0020] (1) The present invention drips sodium hydroxide solution into a copper sulfate orange juice mixed solution to obtain Cu2O, so that Cu2O and the prepared Bi2O3 powder are compounded to obtain a Cu2O-Bi2O3 composite material, wherein the generated Cu2O can not only improve the response absorption performance of the Cu2O-Bi2O3 composite photocatalyst to light, but also effectively inhibit the recombination of photogenerated carriers in the Cu2O-Bi2O3 composite. In addition, through the energy band structure analysis of the Cu2O-Bi2O3 composite material, it can be seen that Cu2O and Bi2O3 have staggered valence band and conduction band positions. After the Cu2O-Bi2O3 composite material is formed, the recombination efficiency of the photogenerated electrons and holes is greatly reduced, and the electron transfer ability is enhanced. The entire preparation process of the present invention is green and environmentally friendly, and the safety of the experiment is guaranteed.

[0021] (2) The present invention successfully prepares a Cu2O-Bi2O3 composite material in an orange juice system under alkaline conditions of pH 11 to 13, using green biological molecules in the orange juice as a reducing agent, and using copper sulfate pentahydrate, bismuth nitrate pentahydrate and bismuth trioxide as raw materials to adjust the source of Bi2O3; the prepared Cu2O-Bi2O3 composite material is spherical or rod-shaped, with small particles and more small pores on the surface. The specific surface area of ​​the Cu2O-Bi2O3 composite material is larger than that of a single material. The particle size of the Cu2O-Bi2O3 composite material prepared using purchased pharmaceutical Bi2O3 as a raw material is slightly larger than that of the Cu2O-Bi2O3 composite material prepared using bismuth nitrate pentahydrate as a raw material by chemical precipitation. i2O3 composite material; the photocatalytic performance of Cu2O-Bi2O3 composite material samples composited with Bi2O3 from different sources is studied. With the different sources of Bi2O3 in the Cu2O-Bi2O3 composite material, there are some differences in the photocatalytic effect. The degradation rate of the Cu2O-Bi2O3 composite material composited with Bi2O3 prepared by chemical precipitation method using bismuth nitrate pentahydrate as raw material reaches about 60%, and the degradation rate of the Cu2O-Bi2O3 composite material composited with purchased pharmaceutical Bi2O3 reaches about 70%. Therefore, the Cu2O-Bi2O3 composite materials prepared by the present invention have good photocatalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the SEM image of the Cu2O material prepared in Example 1 of the present invention (b is an enlarged view of a).

[0023] Figure 2 This is the XRD diagram of the Cu2O material prepared in Example 1 of the present invention.

[0024] Figure 3 This is the SEM image of the Bi2O3 material prepared in Example 2 of the present invention (b is an enlarged view of a).

[0025] Figure 4 This is the XRD diagram of the Bi2O3 material prepared in Example 2 of the present invention.

[0026] Figure 5 a, b, and c are SEM images of the Cu2O-Bi2O3 composite material prepared in Comparative Example 1 of the present invention, and d, e, and f are SEM images of the Cu2O-Bi2O3 composite material prepared in Example 3 (wherein b and c are enlarged images of a, and e and f are enlarged images of d).

[0027] Figure 6 a is the XRD graph of the Cu2O-Bi2O3 composite material prepared in Comparative Example 1 of the present invention, and b is the XRD graph of the Cu2O-Bi2O3 composite material prepared in Example 3.

[0028] Figure 7 a is the infrared spectrum of the Cu2O-Bi2O3 composite material prepared in Comparative Example 1 of the present invention, and b is the infrared spectrum of the Cu2O-Bi2O3 composite material prepared in Example 3.

[0029] Figure 8 This is the UV spectrum of the Cu2O-Bi2O3 composite material prepared in Comparative Example 1 of the present invention for photocatalytic degradation of malachite green dye.

[0030] Fig. 9 This is the UV spectrum of the Cu2O-Bi2O3 composite material prepared in Example 3 of the present invention for photocatalytic degradation of malachite green dye.

[0031] Fig.10 Schematic diagram of separation of photogenerated charges in photocatalysis of the Cu2O-Bi2O3 composite material synthesized experimentally in the present invention. DETAILED DESCRIPTION

[0032] like Figure 1-7 As shown, a method for preparing a Cu2O-Bi2O3 composite material with photocatalytic properties.

[0033] Example 1

[0034] Preparation of Cu2O

[0035] S1. Weigh 0.80 g of copper sulfate pentahydrate solid and add it to a beaker containing an appropriate amount of the upper clarified liquid after centrifugation of orange juice. Place it in a water bath at 55°C and stir it magnetically to fully dissolve the solid. Prepare 40 mL of Cu 2+ A mixed solution of copper sulfate and orange juice with a concentration of 0.08 mol / L;

[0036] S2, weigh 7.00g of sodium hydroxide particles and add them to deionized water to prepare 20mL of 8.75mol / L sodium hydroxide solution, slowly drip the prepared sodium hydroxide solution into the mixed solution in the water bath, and adjust the pH of the mixed solution to 11; at this time, the mixed system gradually turns into a reddish brown suspension, and continue to stir it magnetically and keep it warm for 3h;

[0037] S3. The mixture obtained above was taken out and cooled at room temperature. Finally, the product obtained after centrifugation was dried in a constant temperature forced air drying oven at 80° C. and ground to obtain Cu2O powder.

[0038] The obtained Cu2O powder was characterized by scanning electron microscopy and X-ray diffraction. Figure 1-2 shown.

[0039] Depend on Figure 1From a and b, we can see that the Cu2O material is spherical, with a particle size ranging from a few hundred nanometers to a few micrometers, and there is agglomeration. A careful inspection reveals that the large particles are composed of many spherical particles with smaller particle sizes.

[0040] Depend on Figure 2 It can be seen that when the diffraction peaks appear at 2θ=36.62° and 42.74°, by comparing with the standard spectrum JCPDS card (JCPDS card number: 74-1230), they correspond to the diffraction peaks of the (111) and (200) crystal planes of the Cu2O cubic phase; when the diffraction peak appears at 2θ=61.90°, by comparing with the standard spectrum JCPDS card (JCPDS card number: 77-0199), it corresponds to the diffraction peak of the (220) crystal plane of the Cu2O cubic phase. It can be seen from the figure that in the Cu2O material prepared in the experiment, compared with other crystal planes, the diffraction peak of the (111) crystal plane of Cu2O is the strongest, indicating that the product mainly grows along this crystal plane.

[0041] Example 2

[0042] Preparation of Bi2O3 (chemical precipitation method)

[0043] S1. Weigh 3.02 g of bismuth nitrate pentahydrate solid and add it to 10 mL of 1 mol / L dilute nitric acid solution. Heat it in a water bath at 90° C. and stir it magnetically to fully dissolve the solid to obtain a bismuth nitrate nitric acid mixture.

[0044] S2, weigh 7.00g of sodium hydroxide particles, put them into an appropriate amount of deionized water, stir them thoroughly to dissolve, and prepare 20mL of 8.75mol / L sodium hydroxide solution;

[0045] S3, slowly dripping the prepared sodium hydroxide solution into the above-mentioned bismuth nitrate and nitric acid mixture, stirring continuously, and adjusting the pH of the mixture to 11; then heating the obtained alkaline mixture in a water bath at 55° C. for 3 h;

[0046] S4. The obtained mixture is taken out and centrifuged, and the precipitate is obtained after being rinsed with deionized water for several times. The precipitate is then dried in a constant temperature forced air drying oven at a temperature of 80°C. After grinding, it is put into a box-type electric furnace for calcination at a temperature of 450°C and a calcination time of two hours. After the calcination is completed, it is cooled and then taken out, and the obtained product is ground again to obtain Bi2O3 powder.

[0047] The obtained Bi2O3 powder was characterized by scanning electron microscopy and X-ray diffraction. Figure 3-4 shown.

[0048] Depend on Figure 3From a and b, we can see that the Bi2O3 material particles are rod-like, with a particle size ranging from several hundred nanometers to several microns. There is agglomeration phenomenon, and many short rods can be aggregated into large spherical particles, showing a loose and porous surface.

[0049] Depend on Figure 4 It can be seen that when the diffraction peaks appear at 2θ=25.89°, 27.58°, 33.43°, 35.21°, and 37.76°, by comparing with the standard spectrum JCPDS card (JCPDS card number: 76-1730), they correspond to the (002), (120), (202), (212), and (112) crystal planes of the Bi2O3 monoclinic phase, respectively; when the diffraction peak appears at 2θ=46.32°, by comparing with the standard spectrum JCPDS card (JCPDS card number: 78-1793), it corresponds to the diffraction peak of the (222) crystal plane of the Bi2O3 tetragonal phase; it can be seen from the figure that in the Bi2O3 material, the diffraction peak of the (120) crystal plane of Bi2O3 is the strongest, indicating that the product mainly grows along this crystal plane.

[0050] Example 3

[0051] S1. Weigh 0.80 g of copper sulfate pentahydrate solid and add it to a beaker containing an appropriate amount of supernatant liquid after centrifugation of orange juice. Place it in a water bath at 55°C and stir magnetically to fully dissolve the solid to prepare 40 mL of Cu 2+ A mixed solution of copper sulfate and orange juice with a concentration of 0.08 mol / L;

[0052] S2, weighing Bi2O3 prepared by chemical precipitation method using bismuth nitrate pentahydrate as raw material (i.e., Bi2O3 prepared in Example 2) solid dispersed in the above copper sulfate orange juice mixed solution and continued to stir, then taking out the obtained mixed system and putting it into 55°C ultrasonic treatment;

[0053] S3, weigh 7.00g of sodium hydroxide particles and dissolve them in an appropriate amount of deionized water to prepare 20mL of 8.75mol / L sodium hydroxide solution, slowly drip the prepared sodium hydroxide solution into the above-mentioned ultrasonic mixed system at 55°C, adjust the pH of the mixed system to 11, at which time the mixed system gradually changes from yellow-green to reddish brown, continue to ultrasonicate the mixed system and keep it warm for 3h;

[0054] S4, transferring the obtained mixture to a hydrothermal synthesis reactor, heating it to 55° C. and keeping it warm for 4 hours, taking it out and cooling it at room temperature;

[0055] S5. Finally, the mixture is centrifuged and the obtained precipitate is placed in a constant temperature forced air drying oven at 80°C for drying. After grinding again, Cu2O-Bi2O3 powder is obtained, which is recorded as sample No. 1.

[0056] Comparative Example 1

[0057] The Bi2O3 prepared by chemical precipitation method in Example 3 was replaced by purchased Bi2O3, and the other steps were the same as Example 3 to obtain Cu2O-Bi2O3 powder, which was recorded as sample No. 2.

[0058] The performance tests of the Cu2O-Bi2O3 powders prepared in Example 3 and Comparative Example 1 were carried out respectively. Figure 5-7 shown.

[0059] Specifically, Figure 5 In a, d, c, and f, it can be seen that when the purchased pharmaceutical Bi2O3 is used, the product is spherical, with a particle size range of several hundred nanometers to several microns, and some small particles agglomerate to form large particles; when Bi2O3 prepared by chemical precipitation method using bismuth nitrate pentahydrate as the raw material, the product is rod-shaped, with a particle size range of several microns to tens of microns, and some small particles aggregate. With the change of the source of Bi2O3 in the Cu2O-Bi2O3 composite material, the particle size changes significantly. The particle size of the Cu2O-Bi2O3 composite material prepared with the purchased pharmaceutical Bi2O3 as the raw material is slightly smaller than that of the Cu2O-Bi2O3 composite material prepared with Bi2O3 prepared by chemical precipitation method using bismuth nitrate pentahydrate as the raw material, and the surface of the material is rougher, with agglomeration, and the aggregates are composed of many spherical particles with smaller particle sizes.

[0060] Figure 6 It can be seen that when the diffraction peak appears at 2θ=32.48°, by comparing with the standard spectrum JCPDS card (JCPDS card number: 34-1354), it corresponds to the (311) crystal plane of the Cu2O cubic phase; when the diffraction peak appears at 2θ=28.06°, 46.45°, and 55.63°, by comparing with the standard spectrum JCPDS card (JCPDS card number: 78-1793), it is found that they correspond to the (201), (222), and (213) crystal planes of the Bi2O3 tetragonal phase, respectively. When the Cu2O-Bi2O3 composite material is prepared by using purchased pharmaceutical Bi2O3 and Bi2O3 prepared by chemical precipitation method using bismuth nitrate pentahydrate as raw materials, the diffraction peak of the (201) crystal plane of Bi2O3 is the strongest, indicating that the product mainly grows toward this crystal plane.

[0061] from Figure 7 It can be seen that the Cu2O-Bi2O3 composites made of Bi2O3 from different sources all have similar characteristic absorption peaks. When the characteristic absorption peak appears at 3430cm -1 When the characteristic absorption peak appears at 1590cm -1When the characteristic absorption peak appears at 1390cm -1 When the characteristic absorption peak appears at 840cm -1 When the characteristic absorption peak appears at 634cm -1 When it is on the left and right, it corresponds to the infrared absorption peak of Cu-O.

[0062] The photocatalytic performance of the Cu2O-Bi2O3 composite materials prepared in Example 3 and Comparative Example 1 was measured respectively:

[0063] 1. Preparation of Malachite Green Dye Solution

[0064] Weigh 0.01g of malachite green dye powder on a balance, pour it into a beaker containing 50mL of deionized water, stir to dissolve and then drain into a 500mL volumetric flask, add deionized water to the scale line of the volumetric flask, and shake well to dissolve the sample fully. The prepared dye concentration is 20.00mg / L.

[0065] 2. Determination of photocatalytic performance

[0066] Weigh 0.04g of sample Cu2O-Bi2O3 powder on weighing paper, then take 40mL of 20.00mg / L malachite green solution in a beaker, turn on the xenon lamp, adjust the light focus, pour the samples into the beaker, stir and heat in a water bath, control the temperature at 30℃, take samples at the beginning of illumination, numbered 0; take samples after 8min of illumination, numbered 1; take samples every 8min thereafter, numbered 2, 3, 4, 5, 6, 7, 8. There are nine samples in total, and each sample must be centrifuged in a centrifuge (speed: 10000 rpm), and after centrifugation, save the sample, and finally perform UV spectrum scanning in a UV spectrophotometer.

[0067] Then the above steps were repeated to measure the photocatalytic performance of Cu2O-Bi2O3 powders composited with Bi2O3 from different sources. The results are as follows: Figure 8-9 shown.

[0068] Depend on Figure 8-9It can be seen that the degradation rate of the Cu2O-Bi2O3 composite material formed by the purchased pharmaceutical Bi2O3 (i.e., the Cu2O-Bi2O3 composite material prepared in Comparative Example 1) reaches about 70%, and the degradation rate of the Cu2O-Bi2O3 composite material formed by Bi2O3 prepared by chemical precipitation method using bismuth nitrate pentahydrate as raw material (i.e., the Cu2O-Bi2O3 composite material prepared in Example 3) reaches about 60%. That is, as the source of Bi2O3 in the Cu2O-Bi2O3 composite material is different, the photocatalytic effect shows some differences, but no matter what source of Bi2O3 is used, the photocatalytic performance of the Cu2O-Bi2O3 composite material prepared is relatively excellent.

[0069] Fig.10 Schematic diagram of the separation of photogenerated charges in the experimentally synthesized Cu2O-Bi2O3 composite material photocatalysis. Fig.10 It can be obtained that single Cu2O and Bi2O3 materials have staggered valence band and conduction band structures. When single Cu2O and Bi2O3 materials are compounded into Cu2O-Bi2O3 composite materials, photogenerated electrons flow out from the conduction band of Cu2O and then flow into the conduction band of Bi2O3, and at the same time, the corresponding holes flow out from the valence band of Bi2O3 and then flow into the valence band of Cu2O, thereby promoting the separation of photogenerated charges and greatly improving the photocatalytic performance of the Cu2O-Bi2O3 composite material, thereby making the Cu2O-Bi2O3 composite material obtained in the experiment have better photocatalytic performance.

[0070] In summary, in the alkaline condition of pH 11-13, in the fruit fresh orange juice system, the green biological molecules in the fresh orange juice were used as reducing agents, and copper sulfate pentahydrate, bismuth nitrate pentahydrate and bismuth trioxide were used as raw materials to successfully prepare the Cu2O-Bi2O3 composite material. The prepared Cu2O-Bi2O3 composite material is spherical or rod-like in shape, with small particles having a small particle size. The large particles formed by the aggregation of small particles have more small pores on the surface, reflecting that it has a large specific surface area. The particle size of the Cu2O-Bi2O3 composite material prepared by the purchased pharmaceutical Bi2O3 as a raw material is slightly larger than that of the Cu2O-Bi2O3 composite material prepared by the chemical precipitation method using bismuth nitrate pentahydrate as a raw material; the X-ray diffraction spectrum shows that the Cu2O-Bi2O3 composite materials from two different sources and the single Cu2O material The crystallinity of the Cu2O-Bi2O3 composite material and the single Bi2O3 material are good; the photocatalytic performance of the Cu2O-Bi2O3 composite material samples was studied and it was found that the photocatalytic effects of the Cu2O-Bi2O3 composite materials composed of Bi2O3 from different sources were slightly different. The degradation rate of the Cu2O-Bi2O3 composite material composed of Bi2O3 prepared by chemical precipitation method using bismuth nitrate pentahydrate as raw material reached about 60%, and the degradation rate of the Cu2O-Bi2O3 composite material composed of purchased pharmaceutical Bi2O3 reached about 70%, and the photocatalytic performance of both was good.

[0071] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a Cu2O-Bi2O3 composite material with photocatalytic performance, characterized in that: The steps include: S1. Preparation of copper sulfate orange juice mixed solution: Weigh copper sulfate pentahydrate solid and dissolve it in the upper clear liquid after centrifugation of orange juice, then put it into a water bath at 55°C and stir it magnetically to mix it evenly, and prepare 35-55mL of Cu 2+ A mixed solution of copper sulfate and orange juice with a concentration of 0.05-0.25 mol / L; S2, preparation of Bi2O3: weigh 2.5-3.5g of bismuth nitrate pentahydrate solid and add it to 5-15mL of dilute nitric acid solution to prepare a mixed solution, slowly drip the prepared 6-9mol / L sodium hydroxide solution into the mixed solution, and adjust the pH of the mixed solution to alkaline; then keep the obtained alkaline mixed solution warm in a water bath, take it out and centrifuge it, rinse it to obtain a precipitate, then dry the precipitate in a constant temperature blast drying oven at 80°C, grind it and put it into a box-type electric furnace for calcination, the calcination temperature is 450°C, the calcination time is two hours, after the calcination is completed, wait for it to cool down and take it out, grind it to obtain Bi2O3 powder; S3, weigh 2-3g of the Bi2O3 solid in step S2 and disperse it in the copper sulfate orange juice mixed solution in step S1 and continue stirring, then take out the obtained mixed solution and put it into an environment of 50℃-60℃ for ultrasonic treatment; S4. Slowly drip the prepared sodium hydroxide solution into the ultrasonic mixed solution in step S3, and adjust the pH of the mixed solution to be alkaline; when the mixed solution gradually changes from yellow-green to red-brown, continue to ultrasonicate the mixed solution and keep it warm, reheat it and keep it warm, and then cool, dry and grind it in sequence to obtain Cu2O-Bi2O3 powder.

2. The method for preparing a Cu2O-Bi2O3 composite material with photocatalytic performance according to claim 1, characterized in that: In step S2, the concentration of the dilute nitric acid solution is 1 mol / L.

3. The method for preparing a Cu2O-Bi2O3 composite material with photocatalytic performance according to claim 1, characterized in that: The pH values ​​of the mixed solution in step S2 and the mixed solution in step S4 are both 11-13.

4. The method for preparing a Cu2O-Bi2O3 composite material with photocatalytic performance according to claim 1, characterized in that: In step S4, the mixed solution gradually changes from yellow-green to reddish brown, and the mixed solution is further ultrasonicated and kept warm for 2-4 hours; the resulting mixture is transferred to a hydrothermal synthesis reactor, heated to 55°C and kept warm for 2-4 hours, taken out and cooled at room temperature, and finally the product is centrifuged and dried in a constant temperature forced air drying oven at 80°C, and ground again to obtain Cu2O-Bi2O3 powder.

5. The method for preparing a Cu2O-Bi2O3 composite material with photocatalytic performance according to claim 1, characterized in that: The sodium hydroxide solution is prepared by dissolving sodium hydroxide particles in pure water.

6. A Cu2O-Bi2O3 composite material with photocatalytic performance as claimed in any one of claims 1 to 5, characterized in that: The particle size of the composite material is 0.6 μm-5 μm.