Selective low-temperature epitaxial deposition

By using the co-flow of chlorinated silicon, antimony and phosphorus precursors on the hGAA structure, selective formation of NMOS source/drain regions at low temperatures was achieved, solving the incompatibility and selectivity loss problems in the formation of NMOS source/drain regions in the prior art, reducing production costs and improving growth rate and selectivity.

CN116261770BActive Publication Date: 2026-11-17APPLIED MATERIALS INC
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202180059332.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2021-04-15
Filing Date
2021-12-29
Publication Date
2026-11-17
Estimated Expiration
2041-12-29

AI Technical Summary

Technical Problem

Existing technologies suffer from precursor incompatibility and selectivity loss when forming NMOS source/drain regions at low temperatures. Furthermore, traditional methods increase device manufacturing costs and may lead to dopant diffusion. A method is needed to form NMOS source/drain regions on hGAA structures without additional etching operations.

Method used

By employing the co-flow of chlorinated silicon-containing precursors, antimony-containing precursors, and phosphorus-containing precursors, antimony-doped source/drain regions are formed through epitaxial deposition at a temperature below approximately 550°C. Selective etching and deposition are performed using chlorinated silicon-containing precursors, while antimony-containing precursors lower the temperature and increase the growth rate of the crystal portion. Phosphorus-containing precursors are used for doping to form a selective epitaxial layer.

Benefits of technology

It enables selective formation of NMOS source/drain regions at low temperatures, reduces dopant diffusion, lowers production costs, improves growth rate and selectivity, reduces dicing, and lowers parasitic capacitance and leakage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116261770B_ABST
    Figure CN116261770B_ABST
Patent Text Reader

Abstract

This paper describes a method for the selective formation of epitaxial layers. In this method, an epitaxial layer is deposited to form source and drain regions around a horizontally all-around gate (hGAA structure). The method includes a combination of co-flowing silicon-containing precursors, antimony-containing precursors, and n-type doped precursors. The resulting source and drain regions are selectively grown from crystalline nanosheets or nanowires of the hGAA structure, rather than selectively grown from amorphous gate structures and dielectric layers. The source and drain regions are mainly along... <110> directional growth.
Need to check novelty before this filing date? Find Prior Art

Description

background Technical Field

[0002] Embodiments of this disclosure generally relate to methods for forming semiconductor devices. More specifically, this application relates to an epitaxial deposition method for horizontal gate all around (hGAA) device structures. Background Technology

[0004] As transistor device feature sizes continue to shrink to achieve greater circuit density and higher performance, there is a need to improve transistor device structures to improve electrostatic coupling and reduce negative effects such as parasitic capacitance and off-stage leakage. Examples of transistor device structures include planar structures, FinFET structures, and horizontal gate-all-around (hGAA) structures. The hGAA device structure comprises several lattice-matched channels suspended in a stacked configuration and connected by source / drain regions.

[0005] However, challenges associated with hGAA structures include the formation of n-channel metal-oxide-semiconductor (NMOS) source / drain regions at low temperatures. Conventional methods for forming NMOS source / drain regions at low temperatures result in precursor incompatibility and selectivity loss. Conventional methods also utilize separate etching and deposition steps, which increases the cost of device fabrication. However, increasing the formation temperature of the NMOS source / drain regions may increase the diffusion rate of dopants throughout the hGAA structure and require longer ramp-up / ramp-down times.

[0006] Therefore, there is a need for a method to form NMOS source / drain regions on the hGAA structure at a lower temperature without additional etching operations. Summary of the Invention

[0007] This disclosure generally includes methods for forming source / drain regions on a semiconductor structure. More specifically, embodiments of this disclosure include a method for forming a semiconductor device. This method of forming a semiconductor device includes: forming a multilayer material on a substrate, wherein the multilayer material includes a plurality of crystalline first layers and a plurality of non-crystalline second layers arranged in an alternating pattern. Source regions and drain regions are selectively formed on the plurality of crystalline first layers of the substrate, wherein the formed source and drain regions contain a content greater than about 5 x 10⁻⁶. 20 atoms / cm 3The antimony concentration. The steps of forming the source region and the drain region further include the following steps: flowing a chlorinated silicon-containing precursor; co-flowing an antimony-containing precursor with the chlorinated silicon-containing precursor; co-flowing an n-type doped precursor with the chlorinated silicon-containing precursor and the antimony-containing precursor; and heating the substrate to a temperature of less than about 550°C.

[0008] In another embodiment, a semiconductor device is described. This semiconductor device includes a multi-material layer. The multi-material layer includes: a plurality of first layers comprising a crystalline silicon material; and a plurality of second layers comprising a metal material and a high-k material on the outer surface of the metal material. The plurality of second layers and the plurality of first layers are arranged in an alternating pattern. This semiconductor device further includes a source region and a drain region. The source region and the drain region are epitaxial layers and include silicon material, antimony dopant, and n-type dopant.

[0009] In yet another embodiment, a method for forming a semiconductor device is described. This method for forming a semiconductor device includes: primarily along... <110> Source and drain regions are selectively grown on the substrate. The source and drain regions contain a density greater than approximately 5 x 10⁻⁶. 20 atoms / cm 3 The antimony concentration. The step of selectively growing the source region and the drain region further includes the following steps: flowing a chlorinated silicon-containing precursor into a processing chamber having the substrate; co-flowing the antimony-containing precursor into the processing chamber along with the chlorinated silicon-containing precursor; co-flowing the phosphorus-doped precursor into the processing chamber along with the chlorinated silicon-containing precursor and the antimony-containing precursor; and heating the substrate to a temperature of less than about 550°C during the flow of the chlorinated silicon-containing precursor, the antimony-containing precursor, and the phosphorus-doped precursor. Attached Figure Description

[0010] The features described above in this manner can be understood in detail. More specific descriptions of the present disclosure, which have been briefly summarized above, can be obtained by referring to the embodiments, some of which are illustrated in the accompanying drawings. However, it should be noted that the drawings are merely illustrative examples and should not be considered as limiting the scope of the present disclosure; other equivalent and effective embodiments are permissible.

[0011] Figure 1 According to one embodiment, a schematic isometric view of the hGAA structure is shown.

[0012] Figures 2A-2C According to one embodiment, the figure shows... Figure 1 A schematic cross-sectional view of the hGAA structure.

[0013] Figure 3 According to one embodiment, the diagram is formed Figure 1 and Figures 2A-2C The method for the hGAA structure.

[0014] To facilitate understanding, the same reference numerals have been used as much as possible to represent common elements in the various figures. It is anticipated that elements and features of one embodiment may be beneficially incorporated into other embodiments without further explanation. Detailed Implementation

[0015] This disclosure generally relates to a method for forming a semiconductor device. A method is provided for epitaxially depositing n-channel metal-oxide-semiconductor (NMOS) source / drain regions within a horizontally all-around gate (hGAA) device structure. This method is performed at a temperature less than about 550°C. This method includes using chlorinated silicon-containing precursors, antimony-containing precursors, and phosphorus-containing precursors.

[0016] Chlorinated silicon-containing precursors are used to continuously etch the epitaxial layer as it is formed, and to improve the selectivity of the epitaxial layer as it is deposited onto the superlattice structure. The epitaxial layer is formed only on the crystalline portion of the superlattice structure and not on oxidized or amorphous surfaces. Antimony-containing precursors lower the deposition temperature of the epitaxial layer and increase the growth rate of the epitaxial layer on the crystalline portion of the superlattice structure. Phosphorus-containing precursors dope the epitaxial layer with phosphorus and enable it to adhere better to the crystalline portion of the superlattice structure.

[0017] It has been shown that the growth rate of the epitaxial layer relative to the exposed crystal surface of the superlattice structure varies with the addition of different concentrations of antimony in the epitaxial layer. In the embodiments described herein, the concentration of antimony in the epitaxial layer is greater than about 5 x 10⁻⁶. 20 atoms / cm 3 And mainly along <110> directional growth. It has been shown that antimony concentration causes growth along [the direction of growth]. <110> The main crystal growth direction. Mainly along <110> Directional crystal growth reduces the faceting of epitaxial layers on superlattice structures. This is used for directional crystal growth. <111> Previous methods for directional growth rates were limited in terms of growth due to the cutting.

[0018] Figure 1According to one embodiment, a schematic isometric view of a horizontal all-around gate (hGAA) structure 100 is illustrated. The hGAA structure 100 includes multiple material layers 105 used in the hGAA structure 100, the multiple material layers 105 having alternating first layers 106 and second layers 108, with spacers 110 formed in the second layers 108. The hGAA structure 100 utilizes the multiple material layers 105 as nanowires (e.g., channels) between the source 114a and drain 114b and the gate structure 112. Figure 1 As shown in the cross-sectional view of the multi-layer material 105, nanowire spacers 110 formed at the bottom (or end) of each of the second layers 108 help manage the interface between the second layer 108 and the source / drain electrodes 114a, 114b in order to reduce parasitic capacitance and maintain minimal device leakage.

[0019] The hGAA structure 100 includes a multi-material layer 105 disposed on the top surface 103 of a substrate 102, such as on top of an optional material layer 104 disposed on the substrate 102. In embodiments where the optional material layer 104 is absent, the multi-material layer 105 is formed directly on the substrate 102.

[0020] The substrate 102 may be, for example, crystalline silicon (e.g., Si). <100> or Si <111> Materials such as silicon oxide, strained silicon, silicon-germanium, germanium, doped or undoped polycrystalline silicon, doped or undoped silicon wafers and patterned or unpatterned silicon-on-insulator (SOI) wafers, carbon-doped silicon oxide, silicon nitride, doped silicon, germanium, gallium arsenide, glass, or sapphire. The substrate 102 can have various sizes, such as 200 mm, 300 mm, 450 mm, or other diameters, and can be a rectangular or square panel. Unless otherwise stated, the examples described herein are performed on substrates having a diameter of 200 mm, 300 mm, or 450 mm.

[0021] In one example, optional material layer 102 is an insulating material. Suitable examples of insulating materials may include silicon oxide, silicon nitride, silicon oxynitride, or any suitable insulating material. Alternatively, optional material layer 104 may be any suitable material including conductive or non-conductive materials as desired. Multiple material layers 105 include at least one pair of layers, each pair comprising a first layer 106 and a second layer 108. Although Figure 1The example depicted shows four pairs of layers covered by a first layer 106, but each pair includes a first layer 106 and a second layer 108 (alternating pairs, each pair containing a first layer 106 and a second layer 108). An additional first layer 106 is provided on top of the multilayer material 105. The number of these pairs can vary based on the needs of different processes, having the required additional first layer 106 or second layer 108, or not having the required additional first layer 106 or second layer 108. In one embodiment, the thickness of each individual first layer 106 can be approximately... Peace Treaty Between, such as And the thickness of each individual second layer is approximately 108. Peace Treaty Between, such as The multi-material layer 105 may have a value between approximately Peace Treaty The total thickness between, such as between approximately Peace Treaty The total thickness between.

[0022] The first layer 106 is a crystalline layer, such as a single-crystal, polycrystalline, or single-crystal silicon layer. The first layer 106 is formed using epitaxial deposition. Alternatively, the first layer 106 is a doped silicon layer, including p-type doped silicon layers or n-type doped layers. Suitable p-type dopants include B dopants, Al dopants, Ga dopants, In dopants, or the like. Suitable n-type dopants include N dopants, P dopants, As dopants, Sb dopants, or the like. In yet another example, the first layer 106 is a group III-V material, such as a GaAs layer.

[0023] The second layer 108 is an amorphous material layer. In some embodiments, the second layer 108 is a Ge-containing layer, such as a SiGe layer, a Ge layer, or other suitable layers. Alternatively, the second layer 108 is a doped silicon layer, including a p-type doped silicon layer or an n-type doped layer. In yet another example, the second layer 108 is a III-V group material, such as a GaAs layer. In still another example, the first layer 106 is a silicon layer and the second layer 108 is a metallic material with a high-k material coated on its outer surface. Suitable examples of high-k materials include hafnium dioxide (HfO2), zirconium dioxide (ZrO2), hafnium silicate (HfSiO4), hafnium aluminum oxide (HfAlO), zirconium silicate (ZrSiO4), tantalum dioxide (TaO2), aluminum oxide, aluminum-doped hafnium dioxide, bismuth strontium titanium (BST), or platinum zirconium titanium (PZT), etc. In one particular embodiment, the coating is a hafnium dioxide (HfO2) layer. In some embodiments, the second layer 108 is a material similar to the gate structure 112, to form a wraparound gate around the first layer 106.

[0024] Each spacer 110 is formed adjacent to an end of the second layer 108 and can be considered part of the second layer 108. The spacer 110 is a dielectric spacer or air gap. The spacer 110 can be formed by etching away a portion of each of the second layers 108 using an etching precursor to form a recess at the end of each of the second layers 108. The spacer 110 is formed adjacent to each of the second layers 108 in these recesses. A pad layer (not shown) may be additionally deposited in these recesses prior to the deposition of the spacer 110. The spacer 110 is formed of a dielectric material and is separately formed as each of the nanowires or nanosheets of the first layer 106. In some embodiments, the spacer 110 is selected as a silicon-containing material, which reduces the parasitic capacitance between the gate and source / drain structures in the hGAA nanowire structure; such a material is a low-k material. Silicon-containing or low-k materials may be silicon nitride, silicon oxide, silicon oxynitride, silicon carbide, silicon carbide, silicon carbonitride, doped silicon layers, or other suitable materials, such as Black available from Applied Materials. Material.

[0025] In one embodiment, spacer 110 is a low-k material (e.g., dielectric constant less than 4) or a material containing silicon oxide / silicon nitride / silicon carbide. In other embodiments, spacer 110 is an air gap.

[0026] A gate structure 112 is disposed above and around a multilayer material layer 105. According to one embodiment, the gate structure 112 includes a gate electrode layer and may additionally include a gate dielectric layer, a gate spacer, and a mask layer. The gate electrode layer of the gate structure 112 includes a polysilicon layer or a metal layer covered by a polysilicon layer. The gate electrode layer may include a metal nitride (such as titanium nitride (TiN), tantalum nitride (TaN), or molybdenum nitride (MoN)). x Metal carbides (such as tantalum carbide (TaC) or hafnium carbide (HfC)), metal nitride carbides (such as TaCN), and metal oxides (such as molybdenum oxide (MoO)) x ), metal nitrides (such as molybdenum oxynitride (MoO) x N y ( )), metal silicides (such as nickel silicide), or combinations thereof. The gate electrode layer is disposed on top of and around the multi-material layer 105.

[0027] Optionally, the gate dielectric layer may be disposed below the gate electrode layer and below the multimaterial layer 105. The optional gate dielectric layer may include silicon oxide (SiO2). xThe gate dielectric layer can be formed by thermally oxidizing one or more layers of the first layer 106 and / or the second layer 108, or by any suitable deposition process. Suitable materials for forming the gate dielectric layer include silicon oxide, silicon nitride, oxide nitride, and metal oxides such as hafnium oxide (HfO2) and hafnium zirconium oxide (HfZrO2). x ), hafnium silicon oxide (HfSiO) x Hafnium titanium oxide (HfTiO) x ), Hafnium aluminum oxide (HfAlO) x (and combinations thereof) and multilayers thereof. Gate spacers are formed on the sidewalls of the gate electrode layer. Each gate spacer includes a nitride portion and / or an oxide portion. A mask layer is formed on top of the gate electrode layer and may include silicon nitride.

[0028] This paper describes the composition and formation of antimony-doped source / drain regions 114a and 114b on an hGAA structure 100.

[0029] Figures 2A-2C According to one embodiment, the figure shows Figure 1 A schematic cross-sectional view of the formation of the hGAA structure 100. (Using...) Figure 3 Method 300 forms the hGAA structure 100. The hGAA structure 100 described herein is an n-channel metal-oxide-semiconductor (NMOS) device. Therefore, the dopant in the hGAA structure 100 is an n-type dopant, such as phosphorus, arsenic, antimony, or any combination thereof. According to one embodiment, the dopant includes phosphorus (P).

[0030] about Figure 1 The multiple material layers 105 and gate structure 112 are formed on the substrate 102 and optional material layer 104 during the first operation 302. After the first operation 302, the hGAA structure 100 is similar to Figure 2A The structure described herein is a combination of multiple material layers 105 and gate structure 112. During a first operation, the multiple material layers 105 are formed as follows: multiple alternating first layers 106 and second layers 108 are formed using multiple deposition operations. A portion of the second layer 108 is etched back, and spacers 110 are formed.

[0031] A gate structure 112 is formed around the multilayer material 105. In some embodiments, the gate electrode layer of the gate structure 112 is a material similar to that of each layer of the second layer 108 in the multilayer material 105. The gate structure 112 and the second layer 108 form a surrounding gate around each of the first layer 106. The first layer 106 acts as a nanowire or nanosheet disposed within the surrounding gate. After the source / drain regions are formed, the first layer 106 serves as a channel between the source / drain regions.

[0032] After the membrane stack is formed during the first operation 302, as Figure 2B The antimony-doped source / drain regions 114a and 114b are shown to be formed during the second operation 304. During the second operation 302, a deposition gas mixture is introduced into the processing chamber to deposit the antimony-doped source / drain regions 114a and 114b. Figure 2B As shown, antimony-doped source / drain regions 114a and 114b are deposited on each of the first layer 106 and the substrate 102 in the multilayer material layers 105. The antimony-doped source / drain regions 114a and 114b have a thickness ranging from about 1 nm to about 10 nm. The antimony-doped source / drain regions 114a and 114b are deposited by epitaxial deposition, such as selective epitaxial deposition in an epitaxial deposition chamber. In the embodiment shown herein, the antimony-doped source / drain regions 114a and 114b are deposited on the exposed portion of the substrate 102 made of a crystalline material (such as Si) and on the first layer 106, and the antimony-doped source / drain regions 114a and 114b are not deposited on the spacer 110 or the gate structure 112 made of a dielectric material. The deposition process can be carried out under the following conditions: a chamber pressure ranging from about 1 to about 600 tor (such as from about 200 to about 300 tor), and a deposition temperature (substrate temperature) of less than about 550°C (such as less than about 500°C, such as less than about 450°C).

[0033] A chlorinated silicon precursor and an antimony (Sb)-containing precursor are co-flowed into the processing chamber. The chlorinated silicon precursor includes precursors containing both silicon and chlorine, such as dichlorosilane (SiCl2H2) (DCS), trichlorosilane (SiCl3H) (TCS), or any mixture thereof. In some embodiments, a mixture of DCS and TCS is used. The mixture of DCS and TCS comprises a DCS to TCS ratio of about 1:10 to about 10:1. In some embodiments, it has been shown that when DCS is present, TCS only grows antimony-doped source / drain regions 114a, 114b, and when DCS is not co-flowed, antimony-doped source / drain regions 114a, 114b are not formed or are formed at a significantly reduced rate. It has been shown that DCS increases the growth rate of antimony-doped source / drain regions 114a, 114b. In some embodiments, other suitable chlorinated silicon precursors may be used. Chlorinated silicon precursors enable the growth of antimony-doped source / drain regions 114a, 114b. With the growth of the antimony-doped source / drain regions 114a, 114b, no etch-back operation is performed. It has been shown that the chlorine in the chlorinated silicon precursor improves the crystal growth of the epitaxial layer without additional etch-back processing. Chlorinated silicon precursors may have flow rates ranging from about 1 sccm to about 1000 sccm, such as 1 sccm to about 500 sccm, or 10 sccm to about 1000 sccm. In the embodiments described herein, each of the DCS or TCS has a flow rate ranging from about 1 sccm to about 1000 sccm, such as 1 sccm to about 500 sccm, or 10 sccm to about 1000 sccm.

[0034] Antimony-containing precursors include one or a combination of the following: (stibine; SbH3), antimony trichloride (SbCl3), antimony tetrachloride (SbCl4), antimony pentachloride (SbCl5), triphenyl antimony ((C6H5)3Sb), antimony trihydrogenate (SbH3), antimony trioxide (Sb2O3), antimony pentoxide (Sb2O5), antimony trifluoride (SbF3), antimony tribromide (SbBr3), antimony triiodide (Sbl3), antimony pentafluoride (SbF5), triethyl antimony (C6H5)3Sb 15The precursors used are Sb (TESb) and trimethylantimony (TMSb). In the embodiments described herein, TESb is used. The antimony-containing precursor may have a flow rate ranging from about 0.1 sccm to about 100 sccm. In some embodiments, a carrier gas such as nitrogen (N2) or hydrogen (H2) may flow with the chlorinated silicon-containing precursor and the arsenic-containing precursor. In the operations described herein, no additional etchant flows with the semiconductor-containing precursor and the antimony-containing precursor for selective etchback.

[0035] The amount of excessive point defects in the antimony-doped source / drain regions 114a, 114b can be controlled by changing processing conditions such as the partial voltage of the precursors, the proportion of the precursors, the processing temperature, and / or the layer thickness. The amount of excessive point defects in the antimony-doped source / drain regions 114a, 114b can be controlled to allow Sb atoms to diffuse into the first layer 106 of the multilayer material layer 105. During the deposition of the antimony-doped source / drain regions 114a, 114b, Sb atoms can diffuse into the first layer 106 of the multilayer material layer 105. P-doped materials are added to the antimony-doped source / drain regions 114a, 114b using P-containing precursors. The P-containing precursors flow simultaneously to both the chloride-containing silicon-containing precursor and the antimony-containing precursor. The resistivity of the antimony-doped source / drain regions 114a and 114b is approximately 0.8 mΩ·cm, while the resistivity of the p-doped antimony-doped semiconductor layer is further reduced to approximately 0.5 mΩ·cm to approximately 0.6 mΩ·cm. In the example described herein, the p-containing precursor is phosphine (PH3).

[0036] Each of the chlorinated silicon-containing precursor, arsenic-containing precursor, and P-containing precursor is simultaneously co-infused into the processing chamber. This co-infusion improves the conductivity of the antimony-doped source / drain regions 114a and 114b and allows the deposition temperature to be less than 550°C. In some embodiments, the P-containing precursor is a common n-type doped precursor. In the embodiments described herein, the ratio of the chlorinated silicon-containing precursor to the arsenic-containing precursor and to the P-containing precursor flowing into the processing chamber is approximately 5:1:5 to approximately 20:1:20. As described herein, the ratio of the chlorinated silicon-containing precursor to the arsenic-containing precursor and to the P-containing precursor can be the ratio of DCS and TCS to TESb and PH3.

[0037] The deposited antimony-doped source / drain regions 114a and 114b have a density greater than approximately 5 x 10⁻⁶. 20 atoms / cm 3 Antimony concentrations, such as greater than approximately 1 x 10⁻⁶. 21 atoms / cm 3 Such as greater than approximately 2x1021 atoms / cm 3 The phosphorus dopant concentration in the deposited antimony-doped source / drain regions 114a and 114b is approximately 1 x 10⁻⁶. 20 atoms / cm 3 Approximately 5x10 21 atoms / cm 3 The low-temperature deposition of antimony-doped source / drain regions 114a and 114b further reduces the migration of antimony into the multilayer material layer 105 and other parts of the substrate, since antimony diffusion can cause performance degradation.

[0038] The concentration of antimony dopant in the antimony-doped source / drain regions 114a and 114b alters the growth rate of the antimony-doped source / drain regions 114a and 114b. It has been found that, under conditions of lower antimony dopant concentrations or in embodiments without co-flow of antimony dopant, the deposition rate of the antimony-doped source / drain regions 114a and 114b at temperatures below 550°C is significantly reduced. In some embodiments, it has been found that the concentration of antimony in the antimony-doped source / drain regions 114a and 114b increases the deposition rate by more than twice compared to treatment without any antimony-containing precursor. In some embodiments, without the simultaneous co-flow of both antimony-containing and chlorinated silicon-containing precursors, the growth rate of the antimony-doped source / drain regions 114a and 114b is close to zero at both crystalline and amorphous sites on the substrate at temperatures below 550°C. The antimony in the antimony-containing precursor readily reduces the surface activation energy of the first layer 106, thereby forming antimony-doped source / drain regions 114a, 114b. The growth rate of the antimony-doped source / drain regions 114a, 114b is highly selective to the crystal structure, such that the growth rate of the antimony-doped source / drain regions 114a, 114b on the first layer 106 is about 100 times greater than the growth rate of the antimony-doped source / drain regions 114a, 114b on the spacer 110 and the gate structure 112, for example, about 150 times greater. In some embodiments, the growth rate of the antimony-doped source / drain regions 114a, 114b is about 10 Å / min to about 20 Å / min.

[0039] During the processing described herein, the growth rate of the antimony-doped source / drain regions 114a and 114b mainly follows along <110> Direction, so that along <110> The growth rate of the antimony-doped source / drain regions 114a and 114b in the directional direction is higher than that along the direction of growth. <100> or <111> The growth rate in any direction is more than 50% higher, such as compared to along... <100> or <111> The growth rate in any direction is more than 100% higher. Along <110> Direction compared to <100> or <111> The high growth rate in the direction reduces the cutting of the antimony-doped source / drain regions 114a, 114b and allows the antimony-doped source / drain regions 114a, 114b to grow continuously from the surface of the first layer 106.

[0040] The selective deposition and directional growth rate of the antimony-doped source / drain regions 114a and 114b form a gap 111 between the spacer 110 and the antimony-doped source / drain regions 114a and 114b. The gap 111 is an air gap and separates the spacer 110 from the antimony-doped source / drain regions 114a and 114b, further isolating the spacer 110 from the source / drain regions 116a and 116b. The contact resistance between the first layer 106 and the antimony-doped source / drain regions 114a and 114b is approximately 0.3 mΩ·cm. 2 Approximately 3mΩ-·cm 2 .

[0041] In some embodiments, antimony-doped source / drain regions 114a and 114b are deposited in a first processing chamber, and antimony-doped source / drain regions 114a and 114b are doped with P in a second processing chamber. In other embodiments, the formation of antimony-doped source / drain regions 114a and 114b and the doping of antimony-doped source / drain regions 114a and 114b are performed in a single chamber.

[0042] Following the second operation 304, a third operation 306 is performed to heat-treat the hGAA structure 100. The heat treatment of the hGAA structure is a spike anneal. The spike anneal is performed at a temperature of approximately 900°C to approximately 1200°C for approximately 1 second to approximately 30 seconds. Due to the large size of Sb atoms, Sb atoms do not diffuse at the same rate as P dopant. The short duration of the spike anneal thus suppresses Sb atom diffusion while allowing some P dopant to diffuse in the first layer 106 to form a structure like... Figure 2C The doped region 120 of the first layer 106 of the multi-material layer 105 shown.

[0043] Because the temperatures of the second and third operations are kept below approximately 550°C, the diffusion of dopants and the warpage of the multilayer material 105 are reduced.

[0044] After the antimony-doped source / drain regions 114a, 114b are formed, a capping layer (not shown) may optionally be deposited over the hGAA structure 100. The capping layer is a silicon-containing layer and is deposited on top of each of the antimony-doped source / drain regions 114a, 114b and spacer 110, such that the capping layer fills the gap 111.

[0045] Although the foregoing relates to embodiments of the present disclosure, other and further embodiments of the present disclosure may be devised without departing from the basic scope of the present disclosure, and the scope of the present disclosure is determined by the appended claims.

Claims

1. A method for forming a semiconductor device, comprising the following steps: A multi-material layer is formed on a substrate, wherein the multi-material layer includes a plurality of crystalline first layers and a plurality of amorphous second layers arranged in an alternating pattern; and selectively forming source regions and drain regions on the plurality of crystalline first layers of the substrate, wherein the source regions and the drain regions formed contain a concentration of antimony greater than 5 x 10 20 atoms / cm 3 2 , the step of forming the source regions and the drain regions further comprising the steps of: Silicon-containing precursors undergoing flow chlorination; The antimony-containing precursor flows together with the chlorinated silicon-containing precursor; The n-type doped precursor flows together with the chlorinated silicon-containing precursor and the antimony-containing precursor; and The substrate is heated to a temperature of less than 550°C.

2. The method of claim 1, wherein the n-type doped precursor is a phosphorus-containing precursor.

3. The method of claim 1, wherein the antimony concentration in the source region and the drain region is greater than 2 x 10 21 atoms / cm 3 .

4. The method of claim 1, wherein the growth rate of the source region and the drain region on the plurality of crystal first layers is greater than 50 times the growth rate on the plurality of amorphous second layers.

5. The method of claim 4, wherein the plurality of amorphous second layers further comprises dielectric spacers disposed on the outer portions of the plurality of amorphous second layers.

6. The method of claim 5, wherein during the selective formation of the source region and the drain region, a plurality of gaps are formed adjacent to the plurality of amorphous second layers.

7. The method of claim 1, wherein the chlorinated silicon-containing precursor is one or a combination of dichlorosilane and trichlorosilane.

8. The method of claim 7, wherein the antimony-containing precursor is one or a combination of the following: antimony trichloride, antimony tetrachloride, antimony pentachloride, triphenyl antimony, antimony trihydrogenate, antimony trioxide, antimony pentoxide, antimony trifluoride, antimony tribromide, antimony triiodide, antimony pentafluoride, triethyl antimony, and trimethyl antimony.

9. The method of claim 8, wherein the antimony-containing precursor is triethylantimony.

10. A semiconductor device, comprising: Multiple material layers, including: Multiple first layers, including crystalline silicon material; and Multiple second layers, comprising a metallic material and a high-k material on the outer surface of the metallic material, wherein the multiple second layers are arranged in an alternating pattern with the multiple first layers; Source region; and A drain region, wherein the source region and the drain region are epitaxial layers and include silicon material, antimony dopant, and n-type dopant; and wherein the antimony dopant has a concentration greater than 5 x 10 20 atoms / cm 3 .

11. The semiconductor device of claim 10, wherein the n-type dopant is one or a combination of nitrogen, phosphorus, arsenic or antimony.

12. The semiconductor device of claim 11, wherein the n-type dopant is phosphorus.

13. The semiconductor device of claim 10, wherein each of the plurality of second layers is part of a gate structure.

14. The semiconductor device of claim 10, wherein dielectric spacers are formed on the outer ends of the plurality of second layers.

15. The semiconductor device of claim 10, wherein the plurality of first layers are formed into nanosheets or nanowires.

16. A method of forming a semiconductor device, comprising the following steps: selectively growing a source region and a drain region on a substrate in a <110> direction, wherein the source region and the drain region contain a concentration of antimony greater than 5 x 10 20 atoms / cm 3 The step of selectively growing the source region and the drain region further comprises the step of: The chlorinated silicon-containing precursor is introduced into a processing chamber containing the substrate; The antimony-containing precursor and the chlorinated silicon-containing precursor are allowed to flow together into the processing chamber; The phosphorus-doped precursor, along with the chlorinated silicon-containing precursor and the antimony-containing precursor, flows together into the processing chamber; and During the flow of the chlorinated silicon-containing precursor, the antimony-containing precursor, and the phosphorus-doped precursor, the substrate is heated to a temperature of less than 550°C.

17. The method of claim 16, wherein a multiple material layer is disposed on a substrate, and the multiple material layer comprises a plurality of crystalline first layers and a plurality of amorphous second layers arranged in an alternating pattern, wherein the source region and the drain region are selectively grown on the plurality of crystalline first layers.

18. The method of claim 16, wherein the chlorinated silicon-containing precursor is one or a combination of dichlorosilane and trichlorosilane, and the antimony-containing precursor is triethylantimony.

19. The method of claim 16, wherein the growth rate of the source region and the drain region is from 10 Å / min to 20 Å / min.

Citation Information

Patent Citations

  • Horizontal gate all around device nanowire air gap spacer formation

    CN109564934A

  • Methods of forming self aligned spacers for nanowire device structures

    US20180358436A1