A method for doping and defect passivation of perovskite films

By modifying the perovskite film with alkali metal polymer, the problem of interface defects in perovskite solar cells was solved, the photovoltaic performance and stability were improved, the power conversion efficiency reached 23.6%, and 83 were maintained under high temperature and high humidity conditions. % initial efficiency.

CN116284513BActive Publication Date: 2024-11-19FUDAN UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310267159.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-16
Publication Date
2024-11-19
Estimated Expiration
2043-03-16

AI Technical Summary

Technical Problem

The defects in perovskite thin film interface and grain boundary in perovskite solar cells affect photovoltaic performance and stability, and the prior art is difficult to effectively control the crystallization process, resulting in insufficient device performance and durability.

Method used

Multifunctional alkali metal polymers are prepared through acid-base neutralization reactions, which are used to regulate the crystallization process of FAPbI3 perovskite film, modify the surface of the perovskite film, reduce interface defects, and improve carrier transmission efficiency.

Benefits of technology

Significantly improves the power conversion efficiency of perovskite solar cells, enhances operating stability, and reduces environmental impact, the power conversion efficiency is increased from 21.2% to 23.6%, and maintains an initial 83% under high temperature and high humidity conditions. efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

The present invention relates to the technical field of optoelectronic materials and devices, and further to the preparation of alkali metal functionalized polymer materials. Specifically, an alkali metal functionalized polymer is disclosed, wherein the polymer is obtained by an acid-base neutralization reaction of an alkali metal salt and a high molecular organic compound containing an acidic group in an organic solution; the alkali metal functionalized polymer can be used to modify a photoelectric conversion material, further regulate the crystallization process of a photoelectric material film, significantly improve power conversion efficiency, and at the same time improve operational stability and minimize environmental impact.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of photoelectric materials and devices, and further to the preparation of alkali metal polymer materials, and specifically to the preparation and application of materials capable of modifying photoelectric conversion. Background Art

[0002] Solar energy generated by nuclear fusion is the most important form of natural energy on Earth. It is a recognized environmentally friendly clean energy. It has the advantages of wide distribution, large reserves, and no pollution. It provides the energy necessary for plant photosynthesis and can also provide power support for other green energy sources such as hydropower and wind power in nature. It is one of the most promising new energy sources. Solar cell devices can be used to convert solar energy, which is a nearly inexhaustible energy source, into electricity that is indispensable and can be found everywhere in modern society. As a new solar energy application technology, solar cell devices have become the focus of researchers in recent years. The research boom triggered by solar cell technology has become more and more intense. Photovoltaic devices in the field of solar cells have developed rapidly, and the best energy conversion efficiency has been constantly refreshed.

[0003] At present, various solar cells have been derived. According to their different materials and preparation technologies, the research on solar cell devices has roughly gone through three stages of development. The first generation of solar cells represented by silicon-based solar cells mainly include monocrystalline silicon, polycrystalline silicon and amorphous silicon. Silicon-based solar cells have many excellent characteristics, such as high photoelectric conversion efficiency, large absorption spectrum range and green, safe and reliable raw materials. However, silicon-based solar cells still have defects that cannot be ignored, such as the need for high-purity silicon materials in the production process, and the complex and high-cost preparation process, as well as a certain degree of environmental pollution. These problems are bottlenecks that hinder the further development of silicon-based solar cells.

[0004] Thin-film solar cells represented by multi-organic compounds such as cadmium telluride (CdTe), copper indium gallium selenide (CIS or CIGS), and gallium arsenide (GaAs) are the second stage in the development of solar cells. Compared with traditional silicon solar cells, thin-film solar cells greatly reduce the consumption of raw materials and increase production. They also have a shorter spectral absorption range and an ideal energy band gap (1.45eV), which reduces the recombination of carriers at grain boundaries and improves the collection efficiency of photogenerated carriers. However, the current maximum efficiency of thin-film solar cells can reach 30%, but the cost has remained high, and the reserves of some elements on the earth are limited and toxic, which can easily cause serious pollution to the environment. This makes thin-film solar cells unable to become the main development direction of solar cell technology.

[0005] The current mainstream third-generation solar cells are mainly represented by organic solar cells, quantum dot solar cells, dye-sensitized solar cells, and perovskite solar cells. As one of the mainstream technologies of the new generation of solar cells, organic solar cells have developed rapidly in recent decades and made great progress due to their advantages such as light weight, low cost, flexible translucency, wide material sources, simple preparation process, and easy large-scale commercial production. Despite this, the conversion efficiency is still low compared with polycrystalline silicon and monocrystalline silicon solar cells. Quantum dot solar cells use quantum dots as photosensitizing materials. They have high theoretical energy conversion efficiency and low preparation cost. At present, the energy conversion efficiency of quantum dot solar cells has exceeded 14%, but it is still far from the ideal performance. Dye-sensitized solar cells are mainly composed of photosensitizing dyes and nano-iron dioxide. They have the advantages of material acquisition, relatively low input cost, relatively simple preparation technology, great commercial development potential, and green and harmless raw materials and preparation processes. However, there is still a lot of room for development in terms of durability, high efficiency, stability, etc. These problems restrict the application process of dye-sensitized solar cells. Among them, perovskite materials have excellent photoelectric properties such as direct band gap and adjustable bandgap width, low carrier recombination rate, and high carrier migration length, making perovskite solar cells the most popular solar photovoltaic device at present, with energy conversion efficiency reaching more than 25%. Of course, perovskite solar cells also have some problems to be optimized, such as device stability needs to be improved and the material contains soluble heavy metal lead (Pb).

[0006] In the production process, the preparation of a flat, high-coverage, and low-pore perovskite film is the basis for achieving a high-photovoltaic conversion efficiency device. The quality of the perovskite film is a key parameter that affects the photovoltaic performance of the device. In particular, defects at the interface and grain boundaries (GBs) of the perovskite film are not conducive to the photovoltaic performance and stability of perovskite solar cells. Among them, when the perovskite light absorption layer in the perovskite solar cell is prepared by the solution method, the preparation process involves a complex crystallization growth process, and its nucleation and crystallization growth process is difficult to control, which often leads to poor crystallization quality or crystal defects, which is usually caused by improperly coordinated metal elements. Surface engineering has been widely used to reduce defects at the interface of perovskite films. Defects in perovskite films act as carrier recombination centers, greatly limiting the open circuit voltage (V OC ). At the same time, these defects promote the rapid penetration of water molecules and ion migration in the perovskite layer, accelerating the degradation of the device in the ambient environment.

[0007] So far, a variety of passivation materials have been widely used in perovskite solar cells to suppress defect formation or reduce defect density through molecular interactions with under-coordinated metal cations or halide anions. In particular, passivation of perovskite interfaces is considered an effective means to suppress non-radiative recombination losses and simultaneously improve photovoltage. For example, crown ethers are used to modify the surface properties of perovskite films and passivate defects. It is reported that the multifunctional passivator 2,5-thiophenedicarboxylic acid can effectively target interface defects and improve the operational stability of organic-inorganic lead halide perovskite solar cells. Studies have also found that phenethylamine iodide (PEAI) and other amine analogs can effectively reduce defects and suppress non-radiative recombination, and continuously improve performance. Recently, halides such as quaternary ammonium halides, diammonium iodide, potassium halides and iodopentafluorobenzene have been used to passivate dangling bonds in the perovskite layer by utilizing relevant intermolecular interactions; there are reports on the study of alkali metal salt doping to improve the performance of polymer solar cells, using acetic acid and cesium acetate as dopants, and controlling the concentration of alkali metal salts to explore the effect of different doping concentrations on the experimental results; the experimental results show that alkali metal salts doping the ZnO electron transport layer does improve the electrical properties of polymer solar cell devices; at the same time, the defect states inside and on the surface of the ZnO film modified with alkali metal salts are reduced, providing more convenient conditions for the transport of carriers, and the light absorption capacity of the active layer is also improved to a certain extent, generating more excitons, which significantly enhances the photocurrent. Summary of the invention

[0008] Based on the problem that defects in perovskite film interfaces and grain boundaries (GBs) are not conducive to the photovoltaic performance and stability of perovskite solar cells, this study uses multifunctional alkali metal polymers to regulate the crystallization process of FAPbI3 perovskite films, significantly improving the power conversion efficiency (PCE), while improving operational stability and minimizing environmental impact. Based on this study, the present invention was completed.

[0009] In a first aspect, the present invention provides an alkali metal polymer, wherein the polymer is obtained by an acid-base neutralization reaction of an alkali metal salt and a high molecular organic compound containing an acidic group in an organic solution, and the structural formula thereof is shown in FIG.

[0010]

[0011] Among them, R1, R2, R3 = C, H, O, S, N, CH2, CF2; n = 10-100000000.

[0012] Furthermore, the alkali metal is selected from one or more of lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), and francium (Fr).

[0013] Furthermore, the alkali metal salt is selected from carbonates, bicarbonates, alkali metal nitrates, alkali metal sulfates, etc. formed by the alkali metal.

[0014] Furthermore, the alkali metal salt is preferably a carbonate and / or a bicarbonate.

[0015] In one embodiment, the alkali metal carbonate is selected from one or more of K2CO3, Rb2CO3, and Cs2CO3.

[0016] Furthermore, the acidic group refers to a carboxylic acid group (-COOH).

[0017] Further, the polymer compound containing an acidic group is selected from a polymer compound containing a carboxylic acid group or a mixture thereof;

[0018] Furthermore, the polymer compound having the acidic group is preferably: polyacrylic acid (PAA)

[0019] Furthermore, the organic solution refers to a solvent used to synthesize an organic or inorganic alkali metal polymer, which is selected from one or more of toluene, n-hexane, chloroform, iodobenzene, chlorobenzene, o-dichlorobenzene, anisole, ethyl acetate, methyl acetate, sec-butanol, and acetonitrile.

[0020] In a second aspect, the present invention provides an alkali metal polymer modified photoelectric conversion material.

[0021] Furthermore, the modification is to spin-coat an organic solution containing an alkali metal polymer onto the surface of the photoelectric conversion material to improve the crystallization process of the photoelectric material.

[0022] Furthermore, the photoelectric conversion material is selected from FAPbI3, MAPbI3, CsPbI3, (FAPbI3) 1-x (MAPbBr3) x One or more of;

[0023] In one embodiment, the photoelectric conversion material is preferably a perovskite thin film (FAPbI3).

[0024] In a third aspect, the present invention provides a photovoltaic device prepared from a photovoltaic conversion material modified with an alkali metal polymer.

[0025] Furthermore, the photoelectric device includes a laminated substrate, a metal anode, a hole collection layer, a hole transport layer, a light absorption layer, an electron transport layer and a conductive base.

[0026] Furthermore, the light absorbing layer is prepared from a photoelectric conversion material modified by an alkali metal polymer.

[0027] Furthermore, the photoelectric conversion material is selected from FAPbI3, MAPbI3, CsPbI3, (FAPbI3) 1-x (MAPbBr3) x One or more of .

[0028] In one embodiment, the prepared optoelectronic device is a perovskite solar cell.

[0029] In a fourth aspect, the present invention provides a method for preparing an alkali metal polymer, the preparation method comprising the following steps:

[0030] S1: mixing a polymer compound containing an acidic group and an alkali metal salt in an organic solvent;

[0031] S2 stirs the mixed solution to synthesize an alkali metal salt polymer.

[0032] S3: filtering the solution to obtain the alkali metal salt polymer.

[0033] Furthermore, the organic solvent is preferably chlorobenzene, o-dichlorobenzene, toluene, anisole, ethyl acetate and the like.

[0034] Furthermore, the polymer compound having an acidic group and the alkali metal salt are mixed in a molar ratio of 1:1-3.

[0035] In a fifth aspect, the present invention provides a method for preparing a photoelectric device prepared from a photoelectric conversion material modified with an alkali metal polymer, the method comprising the following steps:

[0036] S01 prepares the etched, cleaned and dried substrate material, and spin-coats or immerses it in a mesoporous layer-by-layer solution to complete the dense layer and the mesoporous layer to form a mesoporous substrate;

[0037] S02 preparing a precursor solution of a photoelectric conversion material, and spin-coating the precursor solution of the photoelectric conversion material onto a mesoporous substrate using a one-step solution method to prepare a photoelectric conversion material film;

[0038] S03, after the spin coating is completed, an organic solution of the alkali metal polymer is dropped onto the film prepared in S02, and annealed to obtain a photoelectric conversion material film modified by the alkali metal polymer;

[0039] S04 prepares a hole transport layer precursor solution, applies the solution to the above-mentioned alkali metal polymer-modified photoelectric conversion material film, and completes the device manufacturing by thermal evaporation deposition of gold electrodes.

[0040] Furthermore, the substrate material is preferably FTO, ITO flexible substrate or the like.

[0041] Furthermore, the mesoporous layer solution is selected from one or more of TiO2, SnO2, NiOx, PTAA, and SAM, preferably mesoporous TiO2 slurry.

[0042] Furthermore, the precursor solution of the photoelectric conversion material as described in S02 includes dimethylformamide (DMF), dimethyl sulfoxide (DMSO), 1,4-butyrolactone, DMA, methylamine, acetonitrile, etc.

[0043] Furthermore, the precursor solution is coated by a one-step spin coating method, with a spin coating speed of 1000-6000 rpm and a spin coating time of 10-30 seconds.

[0044] Furthermore, as described in S04, the hole transport layer precursor is preferably a spiro-OMeTAD solution.

[0045] In a sixth aspect, the present invention provides a use of an alkali metal polymer in a solar cell.

[0046] Furthermore, the solar cell is selected from FAPbI3, MAPbI3, CsPbI3, (FAPbI3) 1-x (MAPbBr3) x One or more of . BRIEF DESCRIPTION OF THE DRAWINGS

[0047] Figure 1 .Synthesis process of alkali metal polyacrylic acid

[0048] Figure 2 .Figure a is the molecular structure of PAA and PAA-Rb polymers. Figure b is a schematic diagram of the preparation of perovskite film by modified anti-solvent. Figure c is the XRD spectrum of the perovskite film. Surface SEM images and cross-sectional SEM (upper right corner of the figure) of the perovskite film of the experimental control group (Figure d), PAA treatment group (Figure e) and Rb-PAA treatment group (Figure f), the scale bar is 0.5μm. XPS nuclear energy level spectra of Pb 4f (Figure g) and Rb3d (Figure h). Figure i is the TOF-SIMS depth distribution map of the perovskite solar cell in the Rb-PAA treatment group.

[0049] Figure 3 Schematic diagram of the preparation of alkali metal polyacrylic acid passivated perovskite films.

[0050] Figure 4 .Statistical graph of photovoltaic parameters of different alkali metal polyacrylic acids.

[0051] Figure 5 .Performance optimization at different concentrations.

[0052] Figure 6 .Small-angle XRD of perovskite film at 0.8°.

[0053] Figure 7 .XPS nuclear energy level spectrum of oxygen

[0054] Figure 8 .Effect of Rb-PAA treatment on the optical and electrical properties of perovskite films. (a) UV-Vis and PL spectra. (b) Time-resolved photoluminescence (TRPL) spectra. UV photoelectron spectroscopy (UPS) spectra in the secondary electron cutoff (c) and valence band (d) regions for control and treated perovskite films. Kelvin probe force microscopy (KPFM) images of control (e), PAA-treated (f), and Rb-PAA-treated (g). (h) Corresponding surface potentials of Figs. 2e–g.

[0055] Fig. 9 Atomic force microscopy (AFM) images of control, PAA, and Rb-PAA samples

[0056] Fig.10 .Photovoltaic device performance. (a) Photovoltaic indicators of devices without Rb-PAA doping (control), doped with PAA, and treated with Rb-PAA (target). (b) JV curves of champion target PSC measured in reverse and forward scanning modes. (c) EQE spectrum (left axis) and integrated Jsc (right axis) of champion target PSC. (d) Stable V of layered structure glass / FTO / dense-TiO2 / meso-TiO2 / perovskite / interface layer / HTL OC and the quasi-Fermi level splitting ΔEF / q.

[0057] Fig.11 Comparison of the best efficiency of control, PAA and Rb-PAA samples

[0058] Fig.12 .Device stability and environmental impact. (a) Stability of control and target PSCs without encapsulation under 1 sun simulated illumination in ambient air. (b) Stability of unencapsulated control and target PSCs on a hot plate at about 65 °C in dry air. (c) Schematic diagram of lead leakage test. (d) Evaluation of lead leakage when solar cells are immersed in water, and the lead concentration in the water is determined by inductively coupled plasma optical emission spectroscopy (ICP-OES) measurement.

[0059] Fig.13 Stability of control, PAA, and target PSCs under simulated illumination of 1 sun in ambient air for 160 h. DETAILED DESCRIPTION

[0060] Alkali metals: refers to all metal elements in the IA group of the periodic table, including lithium (Li), sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), and francium (Fr). The first five exist in nature, and francium can only be produced by nuclear reactions. Alkali metals are elements with strong metallic properties, and their simple substances are also typical metals, showing strong electrical and thermal conductivity. Alkali metals have high reactivity in simple substances and exist only as salts in nature.

[0061] Band gap: The band gap is the energy difference between the lowest point of the conduction band and the highest point of the valence band; it is also called the energy gap. The larger the band gap, the more difficult it is for electrons to be excited from the valence band to the conduction band, the lower the intrinsic carrier concentration, and the lower the conductivity.

[0062] The microstructure of perovskite crystals is a three-dimensional skeleton composed of an octahedral array connected by vertices, in which metal cations are located at the body center, halogen anions are located at the face center, and organic or inorganic cations are located in the gaps of the octahedron, forming a coordination effect with the surrounding 12 ions. Perovskite is a material that can generate electricity and emit light, with low preparation cost, high fluorescence quantum efficiency, high color purity, and adjustable color.

[0063] Organic-inorganic lead halide perovskite solar cells (PSCs) have attracted extensive attention due to their low-cost manufacturing, flexibility, and high efficiency. The power conversion efficiency (PCE) of PSCs has rapidly jumped from 3.8% to a certified value of 25.7% in more than a decade. Although FAPbI3-based PSCs hold bright prospects in the field of next-generation photovoltaics, they still suffer from poor operational stability and potential negative environmental impacts due to easy degradation under ambient conditions and the toxic lead component.

[0064] Example 1 Synthesis of Alkali Metal Polymer

[0065] The alkali metal polyacrylic acid compound was synthesized by mixing polyacrylic acid (PAA) and alkali metal carbonates (K2CO3, Rb2CO3 and Cs2CO3) in a molar ratio of 1:1.5 in 1 mL of anhydrous chlorobenzene and stirring uniformly at room temperature. The amount of acrylic acid (PAA) was 0.01 mg / mL.

[0066] Example 2 Preparation of perovskite solar cells

[0067] (1) Fluorine-doped tin oxide glass substrate (FTO) was etched using zinc powder and concentrated hydrochloric acid (1 M).

[0068] (2) The etched FTO substrate was cleaned in ultrasound using a 2% commercial detergent (Hellmanex) aqueous solution, ethanol, and acetone for 15 minutes, rinsed with deionized water, and then dried using compressed air.

[0069] (3) Diisopropyl di(acetylacetonate) titanate with a content of 75% was diluted with ethanol at a volume ratio of 1:9, and 4% acetylacetone was added to finally prepare a titanium dioxide electron transport layer precursor solution.

[0070] (4) After the dried FTO substrate was treated with ultraviolet ozone for 15 minutes, a precursor solution of diisopropoxybis(acetylacetonate)titanium was deposited on the cleaned FTO substrate by spray pyrolysis at 450° C. using oxygen as a carrier gas.

[0071] (5) After the titanium dioxide electron transport layer is cooled to room temperature, the substrate is treated with ultraviolet ozone for 15 minutes, and the mesoporous TiO2 (mp-TiO2) solution dispersed in advance with ethanol (the weight ratio with ethanol is 1:6) is spin-coated on the dense layer TiO2 at a speed of 4000 rpm to obtain a mesoporous layer with a thickness of 100 to 150 nm. The mesoporous TiO2 film is gradually heated to 450°C for sintering, maintained at this temperature for 30 minutes, and cooled to room temperature.

[0072] (6) Before use, the mesoporous TiO2 film was treated with 0.1 M Li-TFSI acetonitrile solution, spun at 3000 rpm for 20 seconds, and then sintered at 450 °C for 30 minutes.

[0073] (7) After the above mesoporous film was cooled to 150 °C, the substrate was transferred to a dry air glove box (relative humidity <15%) to deposit the perovskite film.

[0074] (8) Lead iodide (1.51 M, Alfa Aesar), formamidine iodide (1.47 M, Greatcell), methylammonium bromide (0.045 M, Greatcell), lead bromide (0.045 M, TCI), and methylammonium chloride (0.6 M, Sigma Aldrich) powders were mixed and dissolved in a mixed solution of DMF and DMSO (mixing ratio of 4:1) to prepare a perovskite precursor solution.

[0075] (9) The perovskite precursor solution was spin-coated onto a mesoporous TiO2 (mp-TiO2) substrate. The precursor solution was spin-coated in a two-step process, where it was spun at 1000 rpm for 10 seconds and then 6000 rpm for 25 seconds. 10 seconds before the end of the second spin coating step, 200-300 μl of chlorobenzene solution containing or not containing alkali metal functionalized polymer was dropped onto the perovskite film. The film was then placed on a heating stage at 150°C for annealing for 10 minutes to obtain a perovskite film.

[0076] (10) A hole transport layer precursor solution was prepared by adding 40 mM Li-TFSI (99.95%, Sigma-Aldrich) and 270 mM tBP (96%, Sigma-Aldrich) additives to a 75 mM spiro-OMeTAD solution. The solution was dynamically spin-coated on the perovskite film at a speed of 3000 rpm for 30 s. Subsequently, a gold electrode (~70 nm) was deposited by thermal evaporation to complete the device fabrication.

[0077] Example 3 Results Analysis

[0078] (1) Synthesis of alkali metal polymers

[0079] Alkali metal salt polyacrylic acid (PAA) complexes are synthesized by mixing PAA organic polymer with alkali metal carbonate in chlorobenzene (CB), such as Figure 1 and Figure 2 a. The synthesized alkali metal functionalized PAA complex solution was used as an antisolvent for the preparation of perovskite films ( Figure 3 ). Unless otherwise specified, the present invention uses (FAPbI3) 0.97 (MAPbBr3) 0.03 Solar cell devices are prepared based on FAPbI3 component perovskite.

[0080] As shown in the photovoltaic performance of solar cells (e.g. Figure 4-5 The best condition was a Rb-PAA complex at a concentration of 0.1 mg / mL, which was used for further studies (denoted as Rb-PAB).

[0081] (2) Analysis of the crystallinity and structural characteristics of perovskite films by X-ray diffraction at different incident angles

[0082] like Figure 2 c and Figure 6 As shown, both the control film and the target film show a well-crystallized photosensitive α phase of the 3D perovskite, with two sharp peaks at 14.2° and 28.4°, belonging to (110) and (220), respectively, indicating that all films have good crystallinity. Small angle X-ray diffraction (SAXS) of the perovskite film at an angle of 0.8° (see Figure 6 ), a small signal of PbI2 appears at 12.7° in the control film, which is well known for the prepared perovskite recipe; excess PbI2. In contrast, the signal of excess PbI2 in the PAA and Rb-PAA treated films is drastically suppressed, especially in the latter film; as shown in Figure 2The morphology of the perovskite surface was analyzed by scanning electron microscopy (SEM) top view images as shown in Figures df. All control and treated perovskite films have similar dense structures with grain sizes in the hundreds of nanometers range and no observable pinholes. Meanwhile, the grain size of the Rb-PAA treated perovskite film (1.44 μm) is slightly larger than that of the PAA treated film (1.14 μm) and the control film (1.02 μm), resulting in fewer grain boundaries and defects.

[0083] (3) The surface composition of perovskite films was studied by X-ray photoelectron spectroscopy (XPS).

[0084] XPS spectra in the Pb4f range ( Figure 2 g) shows two signals in the control film with binding energies of 138.5 and 143.3 eV, which can be attributed to Pb 4f7 / 2 and Pb 4f5 / 2, as well as two small main peaks at 136.6 and 141.6 eV, which are due to the presence of metallic lead (PbO). The signal of metallic Pb disappears in the Rb-PAA treated film, indicating that polyacrylic acid is able to bind to the under-coordinated Pb responsible for the formation of metallic Pb. 2+ ion binding, as evidenced by a slight shift of the peak position toward lower binding energies. This will greatly benefit the operational stability of PSCs in the presence of elemental lead. The XPS spectrum of the Rb3d level range in the treated film shows two signals at 109.9 and 111.5 eV assigned to the Rb 3d3 / 2 and 3d5 / 2 levels, respectively ( Figure 2 h), while no signal was observed in the control perovskite film. This result proves that Rb + has been successfully transferred to the target perovskite film. In addition, the presence of an O1s level peak at 533.1 eV indicates the presence of polyacrylic acid ( Figure 7 ). It can be inferred that PAA is mainly distributed on the top surface of the perovskite film because the long chain structure will produce large-sized areas with steric hindrance. Benefiting from this, PAA can coordinate C=O with under-coordinated Pb 2+ ions, acting as passivators at the film surface between the perovskite and the HTL, thereby reducing the trap states on the top surface.

[0085] (4)Rb + Distribution in the perovskite bulk

[0086] In the synthesis process of Rb-PAA complex, the reaction between Rb2CO3 and PAA (polyacrylic acid) is a simple acid-base neutralization reaction, and the product Rb-PAA is an ionic compound, that is, a bond between molecules. + ions and -COO- groups are soft ionic bonds rather than solid covalent bonds. +The separation of ions from the Rb-PAA complex is much easier, especially in chlorobenzene solution and even in the as-prepared wet perovskite film. During the antisolvent droplet addition process, chlorobenzene can take away DMF and DMSO from the wet perovskite film, while the Rb-PAA complex will also be evenly distributed in the bulk of the perovskite film. Due to the large molecular size domains of the sterically hindered PAA polymer, the PAA polymer is redistributed during the annealing process and mainly exists on the film surface, while the easily separated Rb + ions, will remain primarily in the bulk of the perovskite film.

[0087] To further study Rb + The distribution of ions in the perovskite bulk was investigated using time-of-flight secondary ion mass spectrometry (TOF-SIMS) to measure the depth profile in the target perovskite film ( Figure 2 i) Rb+ ions are mainly present in bulk perovskite, indicating that Rb + ions were successfully incorporated into the perovskite from the Rb-PAA complex. More interestingly, at the beginning of sputtering, PAA mainly occupied the surface of the perovskite, indicated by the strong –COO- signal ( Figure 2 i), which enables the Rb-PAA complex to play a synergistic passivation role through the PAA polymer and Rb + ions. At the same time, Rb + Ions and Pb 2+ and I - The ion distribution is uniform, and further doping with rubidium ions can obtain a more uniform passivation effect. (5) Optical and electronic properties of perovskite films.

[0088] like Figure 8 As shown in Figure a, the UV-Vis absorption spectrum shows that the absorption edge is located around 800nm, with a good light absorption range, indicating that Rb-PAA and PAA treatment do not change the optical properties (i.e., optical band gap) of the perovskite film. This result further shows that the incorporation of PAA has no effect on the crystallization of perovskite, and that Rb + The Rb-PAA-treated film has no incorporation into the lattice to form Rb-based perovskites, resulting in a narrower bandgap perovskite structure. Photoluminescence (PL) spectroscopy shows that the emission intensity of the Rb-PAA-treated film is about 2 times higher than that of the PAA-only or untreated film, indicating that Rb-doped films + It can effectively reduce the defect density, thereby minimizing non-radiative recombination. + The radius of FA, MA, and Cs is much smaller than that of FA, MA, and Cs and is not shown to be incorporated into the bulk perovskite by occupying the A cation site, so it is determined that it is incorporated into the bulk perovskite by the Rb-rich + phase to passivate grain boundary defects.

[0089] (6) Research on carrier transport and recombination in perovskite layers

[0090] The carrier transport and recombination in the perovskite layer were investigated by time-resolved photoluminescence (TRPL) measurements. Figure 8 From the TRPL spectrum shown in b, the recombination in TRPL is mainly first-order trap-assisted recombination. + Due to the passivation effect of PAA, the fitted lifetime of the perovskite film increases dramatically from 470 ns to 1059 ns (Table 1). The longer carrier lifetime indicates a lower non-radiative recombination rate associated with the reduction of trap states in the perovskite film, leading to a higher Voc of the PSC. + The enhanced PL intensity and significantly prolonged charge carrier lifetime of the perovskite film are attributed to the reduced defects. + The perovskite films have longer carrier lifetimes, which is also consistent with micrometer-sized grains with fewer grain boundaries, which act as recombination centers and carrier traps.

[0091] Table 1 TRPL results of single exponential fitting.

[0092]

[0093] The effect of Rb-PAA treatment on the energy level of perovskite films was studied by ultraviolet photoelectron spectroscopy (UPS) characterization, such as Figure 8 As shown in cd, there is no obvious change in the VBM and CBM values ​​of all samples, indicating that the Rb-PAA treatment does not change the electronic structure of the perovskite film.

[0094] In addition to these structural changes, Kelvin probe force microscopy (KPFM) showed that the electronic structure of the surface of the treated perovskite films was different from that of the control samples. Figure 8 eh and Fig. 9 As shown, the target Rb-PAA doped perovskite film has a higher and more uniform surface with a more uniform surface potential distribution in the range of ±5 mV, while the others show a similar range of ±10 mV. This indicates that the number of grain boundaries in the perovskite layer is reduced after Rb-PAA treatment, thus reducing the defect density and carrier recombination.

[0095] (7) Study on PSC photovoltaic performance and stability

[0096] In order to study the photovoltaic performance of the corresponding PSCs, a widely used conventional device structure was adopted, namely FTO / dense layer (TiO2, ~50nm) / mesoporous layer (TiO2, ~150nm) / (FAPbI3)0.97(MAPbBr3)0.03 perovskite layer (~650nm) / hole transport layer (Spiro-OMeTAD, ~150nm) / Au (~80nm). The target device treated with Rb-PAA was compared with the device without any passivation and the device passivated with PAA, where PAA and Rb + All dissolved in CB as antisolvent. Fig.10 a and Fig.11 As shown, this base-functionalized polymer passivation strategy significantly improves the performance of PSCs compared to the control. The improvement in the overall performance of the device is mainly attributed to the improvement in open circuit voltage (Voc) and fill factor (FF). After the addition of Rb-PAA, Voc increased from 1.10±0.02V to 1.170±0.005V, and FF increased from 76.9±1.2% to 80.9±1%. These improvements significantly increased the power conversion efficiency (PCE) (on average) from 21.2±1.1% to 23.6±0.5%. The content of MAPbBr3 in the FAPbI3-based perovskite was further reduced from 3mol% to 1.5mol%, which significantly improved the photovoltaic performance of the target device. As Fig.10 As shown in b, the reverse scan PCE of the champion Rb-PAA polymer-treated device is 24.93%, Voc is 1.185 V, and Jsc is 25.42 mA / cm 2 , FF is 82.8%, PCE is 24.69% For the forward scan, Voc is 1.179 V, Jsc is 25.49 mA / cm 2 , FF is 82.2% and the stable efficiency is 24.74%. The external quantum efficiency (EQE) of the device was measured ( Fig.10 c), and the integrated current matches well with the Jsc value obtained from the JV curve.

[0097] The above results indicate that the interfacial non-radiative recombination process is suppressed by introducing base-functionalized polymers into the bulk and the surface of FAPbI3-based perovskite films ( Fig.10 d).

[0098] To further explore this, we measured the photoluminescence quantum yield (PLQY) and calculated the quasi-Fermi level splitting (ΔE F ).like Fig. 9 As shown, the PLQY of the target device is about 16 times higher than that of the control sample. The interfacial layer leads to a significant reduction in interfacial recombination at the perovskite / HTL interface and grain boundaries, which means that the defect chemistry is improved. According to the PLQY, ΔE FIt can be calculated by the following equation:

[0099] ΔE F =qV OC,rad +k B Tln(PLQY)

[0100] where q is the elementary charge, V OC,rad Yes V OC The radiation limit, k B is the Boltzmann constant, T is the device temperature (25°C). ΔE of the films treated differently F / q Fig.10 d. The control film showed a ΔE of 1.131 meV F , while the target film after Rb-PAA passivation showed a ΔE of 51 meV F Increase. Due to ΔE F / q is the theoretical maximum V of a PSC with this layered structure OC,rad , the quasi-steady-state V OC,rad , that is, it is stable after two minutes of exposure to 1 sun simulated light conditions. Compared with the control sample, the V OC,rad The increase from 1.098V to 1.165mV is 67mV, which is consistent with ΔE F The trend seen in the measurements is consistent; stable V OC,rad and ΔE F The offsets between / q are 34mV and 17mV, corresponding to the control and target devices, respectively.

[0101] Regarding the MPP operation stability of PSC under 1 sun intensity in dry airflow, such as Fig.12 a. After 500 h of operation, the PSC passivated with Rb-PAA retained 83% of its initial efficiency, while the efficiency of the PSC without Rb-PAA polymer treatment was 30%.

[0102] To investigate whether the improved stability mainly comes from the PAA polymer or from the synergistic passivation of the Rb-PAA complex, operational stability tests of PAA-treated PSCs were also compared under the same measurement conditions as before. Fig.12 As shown in a, the PAA-treated PSCs showed better stability than the control device, but still lower than the Rb-PAA-treated PSCs. Therefore, we concluded that the enhanced operational stability of the Rb-PAA-treated PSCs was attributed to the interaction between PAA and Rb + synergistic passivation effect.

[0103] To further test the thermal stability, the PSCs with and without Rb-PAA passivation were aged at 65 °C and 30% RH. Fig.12 b. It was observed that after 600 h, the PSCs passivated with Rb-PAA decreased by less than 10%, compared to about 20% for the control sample. The enhanced environmental and operational stability can be attributed to the lower defect concentration at the interface between the hole transport material and the perovskite absorber layer, as well as fewer impurities (including excess PbI2 and non-perovskite polytypes) on the surface and inside the FAPbI3. + caused by the injection.

[0104] From the above conclusions, it can be concluded that the high thermal stability can be attributed to the rigidity of the ligands containing carbonyl groups and hydrogen bond donors, thereby maintaining the passivation of various cationic and anionic defects through coordination and hydrogen bonding. The strong binding of the ligands on the surface leads to the suppression of interfacial recombination and the migration of halides into the hole transport layer (HTL); in addition, due to the interaction between the C=O bonds and lead, the PAA polymer has the potential to inhibit lead leakage. This was explored by immersing the solar cells in water and quantifying the lead content ( Fig.12 c, d), the presence of PAA polymer can mitigate the harmful effects of lead on the environment. This has been shown by the optimal concentration of PAA used in solar cell manufacturing, which is quite low, and increasing this content may further suppress the impact of lead on the environment.

[0105] In summary, the present invention uses the synthesized Rb-PAA complex solution to control the crystallization and defect formation of FAPbI3-rich perovskites. Electro-optical characterization shows that the PAA polymer can not only act as a carrier of alkali ions but also passivate surface defects through its multiple C=O functional groups. The Rb-PAA-treated perovskite films exhibit less non-radiative charge carrier recombination, i.e., lower defect density, and significantly improved charge extraction from the perovskite film to the HTL. Compared with the control sample, V of the Rb-PAA-treated device was observed. OC The results showed that the best performing device produced a high PCE of 24.93%, while the operational stability was also improved. The Rb-PAA treated PSC retained more than 83% of the initial efficiency after 500 hours of continuous operation under a standard simulated solar intensity illumination, and retained more than 90% of the initial efficiency after aging for 600 hours on a hot plate at about 65°C in dry air (RH was 20%) (see Fig.13 ). At the same time, due to the interaction between PAA and Pb 2+The strong interaction between the two leads also inhibits the leakage of lead, which is crucial for the commercialization of PSCs. This work provides a simple and effective method to fabricate perovskite photovoltaic cells with excellent performance and operational stability.

Claims

1. A photoelectric conversion material modified by an alkali metal polymer, wherein the modification is to spin-coat an organic solution containing the alkali metal polymer as an anti-solvent on the surface of the photoelectric conversion material to participate in improving the crystallization process of the photoelectric material; the alkali metal polymer is obtained by an acid-base neutralization reaction of an alkali metal salt and a polymer organic compound containing an acidic group in an organic solution, and the polymer organic compound containing an acidic group is polyacrylic acid (PAA); the alkali metal salt is an alkali metal carbonate, bicarbonate, alkali metal nitrate, or alkali metal sulfate formed by rubidium (Rb); the organic solution containing the alkali metal polymer is used as an anti-solvent and spin-coated on a film of a perovskite photoelectric conversion material, which can passivate defects at the crystallization interface of a precursor solution of the photoelectric conversion material and improve the crystallization process.

2. The alkali metal polymer modified photoelectric conversion material according to claim 1, characterized in that: The photoelectric conversion material is selected from FAPbI3, MAPbI3, CsPbI3, (FAPbI3) 1-x (MAPbBr3) x One or more of .

3. A photoelectric device prepared from a photoelectric conversion material modified with an alkali metal polymer, characterized in that: The photoelectric device comprises a stacked substrate, a metal anode, a hole collection layer, a hole transport layer, a light absorption layer, an electron transport layer and a conductive substrate, and is characterized in that the light absorption layer is a photoelectric conversion material modified by an alkali metal polymer, the alkali metal polymer is obtained by an acid-base neutralization reaction of an alkali metal salt and a polymer organic compound containing an acidic group in an organic solution, and the polymer organic compound containing an acidic group is polyacrylic acid (PAA); the alkali metal salt is an alkali metal carbonate, bicarbonate, alkali metal nitrate, or alkali metal sulfate formed by rubidium (Rb); the organic solution containing the alkali metal polymer is used as an anti-solvent and is spin-coated on a film of a perovskite photoelectric conversion material, which can passivate defects in the crystallization interface of a precursor solution of the photoelectric conversion material and improve the crystallization process.

4. The photoelectric device prepared from the photoelectric conversion material modified by the alkali metal polymer according to claim 3, characterized in that: The photoelectric conversion material is selected from FAPbI3, MAPbI3, CsPbI3 and / or (FAPbI3) 1-x (MAPbBr3) x One or more of .

5. A method for preparing a photoelectric device prepared from the photoelectric conversion material modified by an alkali metal polymer according to claim 1 or 3, the preparation method comprising the following steps: S01 prepares the etched, cleaned and dried substrate material, and spin-coats or immerses it in a mesoporous layer solution to complete the dense layer and the mesoporous layer to form a mesoporous substrate; S02 preparing a precursor solution of a photoelectric conversion material, and spin-coating the precursor solution of the photoelectric conversion material onto a mesoporous substrate using a one-step solution method to prepare a perovskite photoelectric conversion material film; S03, after the spin coating is completed, an organic solution of an alkali metal polymer is dropped as an anti-solvent on the film prepared in S02, and after annealing, an alkali metal polymer-modified perovskite photoelectric conversion material film is obtained; S04 prepares a hole transport layer precursor solution, applies the solution on an alkali metal polymer modified perovskite photoelectric conversion material film, and completes device manufacturing by thermal evaporation deposition of a gold electrode; Among them, the precursor solution of the photoelectric conversion material S02 includes dimethylformamide (DMF), dimethyl sulfoxide (DMSO), 1,4-butyrolactone, DMA, methylamine, and acetonitrile; the precursor solution uses a one-step spin coating method, the spin coating speed is 1000-6000rpm; the spin coating time is 10-30 seconds.

6. The method for preparing a photoelectric device prepared from a photoelectric conversion material modified by an alkali metal polymer according to claim 5, characterized in that: The mesoporous layer solution is selected from TiO2, SnO2, NiO x , PTAA, SAM or more.