Methods for separating thallium from high-fluorine and chlorine flue dust containing thallium

By treating thallium-containing high-fluorine-chlorine flue dust with high-temperature roasting, the problems of cumbersome procedures and high equipment requirements in existing technologies are solved, achieving efficient recovery of thallium and environmentally friendly separation results.

CN116287730BActive Publication Date: 2026-11-17CENT SOUTH UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310193148.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-02
Publication Date
2026-11-17
Estimated Expiration
2043-03-02

AI Technical Summary

Technical Problem

Existing technologies for separating thallium from high-fluoride and chlorine-containing flue dust involve cumbersome steps, require sophisticated equipment, and are not very feasible. Furthermore, commonly used methods pose environmental pollution risks and are costly.

Method used

High-temperature roasting is used to treat thallium-containing high-fluorine-chlorine flue dust. The temperature is controlled above 1000℃ and held for more than 1 hour. The furnace heating and cooling rate is 10℃/min. After roasting, the slag is returned to the lead-zinc smelting system, and the volatilized thallium gas is condensed and recovered.

Benefits of technology

It simplifies the processing procedure, improves the extraction rate of thallium, avoids environmental pollution, reduces equipment requirements and costs, and achieves efficient recovery of thallium.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116287730B_ABST
    Figure CN116287730B_ABST
Patent Text Reader

Abstract

This invention provides a method for separating thallium from thallium-containing high-fluorine-chlorine flue dust, mainly comprising the following steps: calcining the thallium-containing high-fluorine-chlorine flue dust to obtain calcined residue and thallium-containing gas; wherein the calcination temperature is above 1000℃. This invention effectively improves the volatilization rate of thallium by increasing the calcination temperature, achieving efficient thallium volatilization without complex processes or sophisticated equipment. This invention is simple to operate, highly effective, and worthy of promotion.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of comprehensive utilization and treatment of thallium-containing materials, specifically relating to a method for separating thallium from thallium-containing high-fluorine-chlorine flue dust. Background Technology

[0002] Thallium-containing high-fluoride-chlorine dust is a common type of dust generated during zinc smelting. Thallium is widely found in primary metal ores and possesses various properties such as improving alloy strength, hardness, and corrosion resistance.

[0003] However, commonly used techniques often involve extraction using wet or alternating wet and pyrometallurgical methods, which are cumbersome and require sophisticated equipment. Furthermore, the addition of large amounts of additives increases costs and further burdens the environment, making them impractical and resulting in less than ideal thallium extraction results.

[0004] Therefore, it is necessary to provide a method for separating thallium from thallium-containing high-fluorine-chlorine flue dust to solve the technical problems of cumbersome steps, high requirements for equipment and external materials, and poor feasibility in the separation process of thallium from thallium-containing high-fluorine-chlorine flue dust in the above-mentioned commonly used technologies. Summary of the Invention

[0005] To address the technical problems of cumbersome steps, high requirements for equipment and external materials, and poor feasibility in the separation of thallium from thallium-containing high-fluoride-chlorine dust in commonly used technologies, this invention provides a method for separating thallium from thallium-containing high-fluoride-chlorine dust, comprising the following steps: The thallium-containing high-fluorine-chlorine flue dust was roasted to obtain roasted residue and thallium-containing gas. The roasting temperature is above 1000℃.

[0006] Furthermore, the mass fraction of thallium in the thallium-containing high-fluorine-chlorine dust is 0.5-0.7%, and the thallium in the thallium-containing high-fluorine-chlorine dust mainly exists in the form of monovalent thallium.

[0007] Furthermore, the calcination temperature is 1000℃~1200℃, and the holding time after the calcination temperature is reached is greater than 1 hour.

[0008] Furthermore, the thallium solid waste is heated and cooled during the roasting process by means of furnace heating and furnace cooling, respectively; wherein the heating rate of the furnace heating is 10℃ / min, and the cooling rate of the furnace cooling is 10℃ / min.

[0009] Furthermore, the components of the thallium-containing high-fluorine-chlorine flue dust include one or more of lead-zinc sulfate, lead-zinc oxide, and lead-zinc fluorine-chlorine compounds.

[0010] Furthermore, prior to the step of roasting the thallium-containing high-fluorine-chlorine dust, the process also includes drying and dehydrating the thallium-containing high-fluorine-chlorine dust.

[0011] Furthermore, the drying and dehydration process includes drying the thallium-containing high-fluorine-chlorine fume at 60-90°C for 2-10 hours.

[0012] Furthermore, before the step of roasting the thallium-containing high-fluorine-chlorine dust, the process further includes grinding the dried and dehydrated high-fluorine-chlorine dust; wherein the grinding process includes grinding the dried and dehydrated thallium-containing high-fluorine-chlorine dust to 100-400 mesh.

[0013] Furthermore, it also includes smelting the roasted residue to recover valuable metals.

[0014] Furthermore, it also includes capturing thallium-containing gases and condensing them to obtain thallium-containing compounds.

[0015] Compared with existing technologies, this invention provides a method for treating thallium in thallium-containing high-fluorine-chlorine flue dust, solving a long-standing problem in the zinc smelting field—how to selectively recover valuable metals from thallium-containing high-fluorine-chlorine flue dust while avoiding environmental and production burdens; and providing targeted treatment for thallium-containing high-fluorine-chlorine flue dust that exists in the form of flue dust and is difficult to handle.

[0016] Compared to the complex processes in commonly used technologies, this invention directly roasts thallium-containing high-fluoride-chlorine flue dust at a high temperature of 1000℃. Research has found that the main components of thallium-containing high-fluoride-chlorine flue dust include lead-zinc sulfate. Thallium in thallium-containing high-fluoride-chlorine flue dust mainly exists in the form of monovalent thallium, and most of the monovalent thallium begins to volatilize above 600℃. Furthermore, there is a strong correlation between monovalent thallium and the zinc sulfate phase; disrupting the zinc sulfate structure can achieve the release and efficient volatilization of thallium. Zinc sulfate decomposes significantly above 1000℃. That is, during the above roasting process, some monovalent thallium begins to volatilize at 600℃, while another portion is released along with the decomposition of zinc sulfate.

[0017] As can be seen from the above technical solution, the present invention avoids the complexities of continuous conversion between pyrometallurgical and wet processes in the treatment of thallium-containing high-fluorine-chlorine flue dust, as well as the high equipment requirements in the difficult treatment process, thus simplifying the technical solution and providing a technical solution different from commonly used technical concepts, thereby improving the feasibility of the solution. On the other hand, the present invention can release thallium to the maximum extent in thallium-containing high-fluorine-chlorine flue dust, significantly improving the thallium extraction rate and achieving excellent treatment results. Attached Figure Description

[0018] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on the structures shown in these drawings without creative effort.

[0019] Figure 1 The image shows the XRD pattern of thallium-containing high-fluorine-chlorine flue dust in Example 1 of this invention. Figure 2 The chemical phase analysis results of water-soluble zinc and oxidized zinc as a function of calcination temperature in Example 2 of the present invention, as well as the variation of thallium volatilization rate, are shown in the graph. Figure 3 The diagram shows the chemical phase analysis results of lead chloride, lead sulfate, and lead oxide as a function of calcination temperature in Example 2 of the present invention, as well as the variation of thallium volatilization rate. Figure 4 The chemical phase analysis results of water-soluble zinc and oxidized zinc as a function of oxygen concentration in Example 3 of the present invention, as well as the graph showing the variation of thallium volatilization rate; Figure 5 The graph shows the chemical phase analysis results of lead chloride, lead sulfate, and lead oxide as a function of oxygen concentration in Example 3 of this invention, as well as the variation of thallium volatilization rate. Detailed Implementation

[0020] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only a part of the embodiments of the present invention, and not all of them. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0021] Furthermore, the technical solutions of the various embodiments of the present invention can be combined with each other, but only if they are based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be considered that such combination of technical solutions does not exist and is not within the scope of protection claimed by the present invention.

[0022] When numerical ranges are given in the embodiments, it should be understood that, unless otherwise stated in the present invention, both endpoints of each numerical range and any value between the two endpoints may be selected. Unless otherwise defined, all technical and scientific terms used in this invention, as well as the prior art known to those skilled in the art and the description of this invention, may be implemented using any prior art methods, devices, and materials similar to or equivalent to those described, used, or made of materials in the embodiments of this invention.

[0023] Those skilled in the art should know that thallium, as a metal with significant potential applications, has been the subject of extensive research by universities and enterprises on the separation and enrichment of thallium from thallium-containing materials. Although much of this research focuses on waste residue, it remains worthy of exploration. For example, wet thallium leaching involves wet grinding, first adding alkali to the thallium-containing lead sulfide concentrate, then adding acid to remove thallium. This method requires numerous additives, consumes large quantities, and is highly prone to causing secondary pollution, resulting in high subsequent disposal costs. Another example is the extraction of thallium from thallium-containing waste residue using vacuum metallurgy, followed by three-stage evaporation separation of the intermediate products. This method is lengthy, requires highly sophisticated equipment, and is generally not feasible. Thermosetting adhesives can also be used to solidify thallium-containing waste residue. While this can reduce the toxicity of thallium leaching in the short term, it does not truly achieve thallium separation, and its long-term solidification effect remains to be considered.

[0024] Based on the above description of commonly used technologies, it is evident that it is essential to propose a technical solution that is simple in process, highly feasible, has excellent treatment effect, and offers good economic and environmental benefits.

[0025] This invention provides a method for separating thallium from high-fluoride-chlorine flue dust containing thallium, comprising the following steps: The thallium-containing high-fluorine-chlorine flue dust is roasted to obtain roasted residue and thallium-containing gas; wherein the roasting temperature can be above 1000℃.

[0026] Thallium-containing high-fluoride-chlorine dust is a common byproduct of zinc smelting, and its main components include one or more of lead-zinc sulfates, lead-zinc oxides, and lead-zinc fluoride-chlorine compounds. Thallium-containing high-fluoride-chlorine dust may include one or more of lead-based fluoride-chlorine compounds, zinc-based fluoride-chlorine compounds, and cadmium-based fluoride-chlorine compounds; the fluoride-chlorine compounds may contain one or both of the elements fluorine and chlorine, or may contain both fluorine and chlorine simultaneously.

[0027] Furthermore, the mass fraction of thallium in the thallium-containing high-fluorine-chlorine dust can be 0.5% to 0.7%, and the thallium in the thallium-containing high-fluorine-chlorine dust mainly exists in the form of monovalent thallium.

[0028] It should also be noted that monovalent thallium does not exist in an enriched form in thallium-containing high-fluorine-chlorine flue dust, but is unevenly dispersed in various phases of the thallium-containing high-fluorine-chlorine flue dust.

[0029] In some embodiments, the roasted slag can be returned to the lead-zinc smelting system for secondary use, thereby realizing the recovery of valuable metals.

[0030] In other embodiments, a condenser can be connected after the calcination device, and the volatilized thallium-containing gas can be condensed in the condenser to obtain thallium-containing compounds, thus achieving resource recovery while avoiding secondary pollution.

[0031] The main principle involved in this invention is as follows: It is known that thallium in high-fluorine-chlorine flue dust mainly exists in the form of monovalent thallium compounds. In order to achieve efficient volatilization of thallium, the conditions for volatilization of thallium compounds must be met thermodynamically and kinetically, that is, the critical temperature for volatilization of thallium-containing compounds must be reached, while simultaneously releasing thallium contained in other compounds.

[0032] Therefore, controlling the roasting temperature and holding time, and keeping relevant parameters within a certain range, is essential to achieve efficient volatilization of thallium. The reasons for determining a volatilization temperature above 1000℃ include: 1) According to literature reports, thallium in the high-fluorine-chlorine fumes generated during zinc smelting mainly exists in the form of monovalent thallium, which begins to volatilize above 600℃; 2) In experiments, this invention found a strong correlation between thallium suboxide and the zinc sulfate phase. Destroying the zinc sulfate structure can achieve the release and efficient volatilization of thallium, and zinc sulfate decomposes significantly above 1000℃. Based on these factors, the volatilization temperature was determined to be above 1000℃.

[0033] The roasting temperature can be 1000℃~1200℃, and the holding time after reaching the roasting temperature is greater than 1 hour. The thallium solid waste can be heated and cooled during the roasting process by means of furnace heating and furnace cooling, respectively; the heating rate during furnace heating can be 10℃ / min, and the cooling rate during furnace cooling can be 10℃ / min.

[0034] In some embodiments, thallium-containing high-fluorine-chlorine fumes can be roasted in an air atmosphere.

[0035] In the actual roasting process, thallium-containing high-fluorine-chlorine flue dust can be placed in a vertical tube furnace for roasting. When the furnace temperature rises to 1000℃, it is held for more than 1 hour and then cooled down with the furnace to maximize the release of thallium contained in the zinc sulfate phase.

[0036] During the above-mentioned roasting and heat preservation process, monovalent thallium with a volatilization temperature of about 600°C, as well as monovalent thallium stored in other phases with volatilization temperatures below 1000°C, are also released.

[0037] In some embodiments, prior to the calcination treatment of the thallium-containing high-fluorine-chlorine dust, the process further includes drying and dehydrating the thallium-containing high-fluorine-chlorine dust. The drying and dehydration treatment includes drying the thallium-containing high-fluorine-chlorine dust at 60-90°C for 2-10 hours.

[0038] Fluorine-containing chlorine dust can be placed in a forced-air drying oven and dried until the fluorine-containing chlorine dust reaches a constant weight.

[0039] In some embodiments, prior to the calcination treatment of the thallium-containing high-fluorine-chlorine dust, the process further includes grinding the dried and dehydrated high-fluorine-chlorine dust; wherein the grinding treatment includes grinding the dried and dehydrated thallium-containing high-fluorine-chlorine dust to 100-400 mesh. Grinding the fluorine-chlorine dust to 100-400 mesh can increase the heated surface area of ​​the fluorine-chlorine dust, improve the calcination efficiency, and accelerate the reaction process.

[0040] To facilitate a further understanding of the present invention by those skilled in the art, the following examples are provided: Some terms or names in the embodiments can be explained here.

[0041] Example 1 Sampling and analysis of thallium-containing high-fluorine-chlorine dust Thallium-containing high-fluoride-chlorine dust generated during zinc smelting was collected, ground to 100 mesh, digested, and the elemental content in the thallium-containing high-fluoride-chlorine dust was measured and phase analysis was performed.

[0042] In this embodiment, the thallium content in the thallium-containing high-fluorine-chlorine flue dust was measured to be 0.66 wt%. It should be noted that the thallium element distribution in the thallium-containing high-fluorine-chlorine flue dust is uneven, and the overall thallium content of the flue dust is between 0.5 and 0.7 wt%. The calculation of the thallium volatilization rate in subsequent embodiments and comparative examples is based on the content obtained in this digestion.

[0043] The specific analysis results are as follows: 1. See Figure 1 Based on the chemical phase analysis results in this embodiment, the main phases present in the thallium-containing high-fluorine-chlorine flue dust in this embodiment are zinc oxide, lead oxide, zinc sulfate, lead sulfate, lead chloride, etc., and their forms include crystalline and amorphous states.

[0044] 2. In this embodiment, the mass percentage of the main elements in the thallium-containing high-fluorine-chlorine dust is detailed in the table below: As can be seen from the table above, thallium-containing high-fluorine-chlorine flue dust mainly contains valuable metal elements such as Zn and Pb.

[0045] 3. In this embodiment, the chemical phase analysis results (mass percentage) of Zn are shown in the table below: 4. In this embodiment, the chemical phase analysis results (mass percentage) of Pb are shown in the table below: Example 2 Temperature Single Factor Experiment Take 1 kg of thallium-containing high-fluorine-chlorine dust (same as in Example 1) dried to constant weight in an 80℃ forced-air drying oven, grind it, and then pass it through a 100-mesh sieve. Take the material passing through the sieve as the grinding product.

[0046] The ground products were calcined at temperatures of 600℃, 700℃, 800℃, 900℃, 1000℃ and 1100℃ respectively.

[0047] Each roasting process is as follows: 15g of the ground product is placed in a vertical tube furnace under an air atmosphere for roasting; the temperature of each roasting is controlled at the above temperature, the holding time is 1 hour, and the roasted residue is cooled to room temperature with the furnace after roasting.

[0048] In this embodiment, the chemical phase analysis results (mass percentage in the roasted residue) of water-soluble zinc and zinc oxide in the roasted residue as a function of roasting temperature, and the variation of thallium volatilization rate (as a function of roasting temperature) are all referred to [reference needed]. Figure 2 As shown in the figure; where the broken line in the figure represents the thallium volatilization rate.

[0049] Chemical phase analysis results (mass percentage in the roasted residue) of lead chloride, lead sulfate, and lead oxide in the roasted residue as a function of roasting temperature, and the variation of thallium volatilization rate (with roasting temperature) are shown in [reference needed]. Figure 3 As shown in the figure; where the broken line in the figure represents the thallium volatilization rate.

[0050] Example 3 Single-factor experiment on oxygen concentration Take 1 kg of thallium-containing high-fluorine-chlorine dust (same as in Example 1) dried to constant weight in an 80℃ forced-air drying oven, grind it, and then pass it through a 100-mesh sieve. Take the material passing through the sieve as the grinding product.

[0051] The ground products were calcined at oxygen concentrations of 0%, 10%, 20%, 30%, 40%, and 50%, respectively.

[0052] Each roasting process is as follows: 15g of the ground product is placed in a vertical tube furnace under the above oxygen concentration for roasting; the roasting temperature is controlled at 900℃ and the holding time is 1h. After roasting, the roasted residue is cooled to room temperature with the furnace.

[0053] In this embodiment, the chemical phase analysis results (mass percentage in the roasted residue) of water-soluble zinc and oxidized zinc in the roasted residue as a function of oxygen concentration, and the variation of thallium volatilization rate (as a function of oxygen concentration) are all referred to [reference needed]. Figure 4 As shown in the figure; where the broken line in the figure represents the thallium volatilization rate.

[0054] Chemical phase analysis results (mass percentage in roasted slag) of lead chloride, lead sulfate, and lead oxide in the roasted residue as a function of oxygen concentration, and the variation of thallium volatilization rate (with oxygen concentration) are shown in [reference needed]. Figure 5 As shown in the figure; where the broken line in the figure represents the thallium volatilization rate.

[0055] Example 4 Water immersion test Take 1 kg of thallium-containing high-fluorine-chlorine dust (same as in Example 1) dried to constant weight in an 80℃ forced-air drying oven, grind it, and then pass it through a 100-mesh sieve. Take the material passing through the sieve as the grinding product.

[0056] Weigh 0.200g of the ground product into a centrifuge tube, add 50ml of deionized water, and place the tube in a water bath shaker at 150r / min for 2 hours at room temperature. After centrifugation, separate the solid and liquid components, and test the thallium and zinc content in the supernatant. Then take 0.2000g of the ground product, digest it, and measure the thallium content in the thallium-containing high-fluorine-chlorine flue dust.

[0057] Example 5 One kilogram of dried thallium-containing high-fluorine-chlorine dust sample was ground to a fineness of 100 mesh. 15g of the ground thallium-containing high-fluorine-chlorine dust was placed in a corundum crucible and calcined in a vertical tube furnace under air atmosphere. The calcination temperature was 1000℃, and the temperature was maintained at 1000℃ for 1 hour. After calcination, the calcined residue was allowed to cool to room temperature with the furnace.

[0058] The thallium content in the digestion solution was determined by digesting the roasted residue, and the thallium volatilization rate was calculated to be 96.33%.

[0059] Example 6 One kilogram of dried thallium-containing high-fluorine-chlorine dust sample was ground to a fineness of 100 mesh. 15g of the ground thallium-containing high-fluorine-chlorine dust was placed in a corundum crucible and calcined in a vertical tube furnace under air atmosphere. The calcination temperature was 1100℃, and the temperature was maintained at 1100℃ for 1 hour. After calcination, the slag was allowed to cool to room temperature with the furnace.

[0060] The thallium content in the digestion solution was determined by digesting the roasted residue, and the thallium volatilization rate was calculated to be 99.38%.

[0061] Comparative Example 1 One kilogram of dried thallium-containing high-fluorine-chlorine dust sample was ground to a fineness of 100 mesh. 15 g of the ground thallium-containing high-fluorine-chlorine dust was placed in a corundum crucible and calcined in a vertical tube furnace under air atmosphere. The calcination temperature was 900℃, and the temperature was maintained at 900℃ for 1 hour. After calcination, the calcined residue was cooled to room temperature with the furnace. The calcined residue was digested, and the thallium content in the digestion solution was determined. The calculated thallium volatilization rate was 33.97%.

[0062] Based on this comparative example, it is evident that controlling the calcination temperature above 1000℃ is essential. On one hand, below 1000℃, the structure of the main thallium-containing phase remains intact, and thallium is not fully released, resulting in a low thallium volatilization rate of only 33.97%. On the other hand, as can be seen from Example 5, when the temperature is increased to 1000℃, the volatilization rate increases significantly from 33.97% to 96.33%, demonstrating that temperatures above 1000℃ greatly enhance the thallium volatilization rate.

[0063] Therefore, controlling the calcination temperature is essential for disrupting the structure of thallium-containing phases and achieving efficient volatilization of thallium.

[0064] Analysis example 1 Analysis of the occurrence phases of thallium in Examples 2-4 1. See Figure 2-5 It can be seen that in the analysis results of the two sets of single-factor experiments, the volatilization rate of thallium showed a significant correlation with the zinc-containing phase, while the correlation with the lead-containing phase was weak and the regularity was not obvious. Therefore, it is speculated that the occurrence of thallium is related to the zinc-containing phase.

[0065] Further details can be found in the following documents. Figure 2 As the temperature increases, the water-soluble zinc phase decreases, the oxidized zinc phase increases, and the thallium volatilization rate increases. It is speculated that during the heating process, the water-soluble zinc phase is transformed into the oxidized zinc phase, and thallium is released at the same time.

[0066] See details Figure 4 In the single-factor experiment of oxygen concentration, the water-soluble zinc phase first increased and then decreased, while the oxidized zinc phase and thallium volatilization first decreased and then increased. It is also speculated that this is due to the interconversion between the water-soluble zinc phase and the oxidized zinc phase.

[0067] Based on the data from the water immersion experiment, it can be seen that during the water immersion process, water-soluble zinc completely dissolves, and thallium also dissolves almost completely. It is believed that the phase structure of water-soluble zinc is destroyed during the water immersion process, which leads to the release of thallium contained therein, resulting in the simultaneous dissolution of both.

[0068] Since there is a strong correlation between the dissolution relationship of water-soluble zinc and thallium and the changes during the calcination process, it is believed that the occurrence of thallium is strongly correlated with the phase of water-soluble zinc.

[0069] 2. Zinc chloride has a low volatilization temperature (it volatilizes significantly at around 500℃), while zinc sulfate has a high decomposition temperature (it begins to dissociate at 500~600℃ and dissociates violently at around 930~1000℃).

[0070] In the single-factor temperature experiment, as the temperature increased, the water-soluble zinc phase continued to decrease after exceeding 500℃, and the water-soluble zinc phase decreased significantly in the range of 930~1000℃ (the temperature of violent dissociation of zinc sulfate), while the thallium volatilization rate increased significantly.

[0071] Therefore, it is believed that the occurrence of thallium is related to the zinc sulfate phase in water-soluble zinc, and the main occurrence phase of thallium in high-fluorine-chlorine flue dust containing thallium is zinc sulfate.

[0072] The above technical solutions of the present invention are merely preferred embodiments of the present invention and do not limit the patent scope of the present invention. All equivalent structural transformations made under the technical concept of the present invention using the contents of the present invention specification and drawings, or direct / indirect applications in other related technical fields, are included in the patent protection scope of the present invention.

Claims

1. A method for separating thallium from high-fluoride-chlorine flue dust containing thallium, characterized in that, Includes the following steps: The thallium-containing high-fluorine-chlorine flue dust was roasted to obtain roasted residue and thallium-containing gas. The roasting temperature is 1000℃~1200℃, and the holding time after reaching the roasting temperature is greater than 1 hour; the main phases present in the thallium-containing high-fluorine-chlorine flue dust are zinc oxide, lead oxide, zinc sulfate, lead sulfate, and lead chloride; thallium in the thallium-containing high-fluorine-chlorine flue dust mainly exists in the form of monovalent thallium.

2. The method for separating thallium from thallium-containing high-fluorine-chlorine flue dust according to claim 1, characterized in that, The mass fraction of thallium in the thallium-containing high-fluorine-chlorine dust is 0.5-0.7%.

3. The method for separating thallium from thallium-containing high-fluorine-chlorine flue dust according to claim 1, characterized in that, The thallium-containing high-fluorine-chlorine flue dust is heated and cooled during the roasting process by means of furnace heating and furnace cooling, respectively; wherein the heating rate of the furnace heating is 10℃ / min, and the cooling rate of the furnace cooling is 10℃ / min.

4. The method for separating thallium from thallium-containing high-fluorine-chlorine flue dust according to claim 1, characterized in that, Before the roasting treatment of the thallium-containing high-fluorine-chlorine flue dust, the process further includes: drying and dehydrating the thallium-containing high-fluorine-chlorine flue dust.

5. The method for separating thallium from thallium-containing high-fluorine-chlorine flue dust according to claim 4, characterized in that, The drying and dehydration process includes drying the thallium-containing high-fluorine-chlorine dust at 60-90°C for 2-10 hours.

6. The method for separating thallium from thallium-containing high-fluorine-chlorine flue gas according to claim 4, characterized in that, Before the roasting treatment of the thallium-containing high-fluorine-chlorine flue dust, the process further includes grinding the dried and dehydrated thallium-containing high-fluorine-chlorine flue dust; wherein the grinding treatment includes grinding the dried and dehydrated thallium-containing high-fluorine-chlorine flue dust to 100~400 mesh.

7. The method for separating thallium from thallium-containing high-fluorine-chlorine flue dust according to claim 1, characterized in that, It also includes smelting the roasted residue to recover valuable metals.

8. The method for separating thallium from thallium-containing high-fluorine-chlorine flue dust according to claim 1, characterized in that, It also includes capturing thallium-containing gas and condensing it to obtain thallium-containing compounds.