A field-effect transistor with positive and negative photoconductivity switching and its fabrication method
By introducing an indium selenide layer into a graphene field-effect transistor and utilizing mechanical exfoliation and thermal evaporation coating technology, the positive and negative photoconductivity switching of the graphene field-effect transistor was realized, solving the problem of single function in the existing technology and realizing the diversity of device functions and low-cost fabrication.
Patent Information
- Application Number
- CN202310220086.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-03-09
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-03-09
AI Technical Summary
Existing technologies make it difficult to achieve switching between positive and negative photoconductivity in a single graphene field-effect transistor, which limits the functional diversity of the device.
Hexagonal boron nitride, indium selenide, and graphene layers were prepared by mechanical exfoliation and transferred onto a silicon dioxide/P-type heavily doped silicon substrate. Gold electrodes were then prepared using a thermal evaporation coating apparatus to form a field-effect transistor that switches between positive and negative photoconductivity.
It enables the switching of positive and negative photoconductive effects on a single device, enhances the versatility of device functions, and is simple to operate and inexpensive.
Smart Images

Figure CN116314283B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of two-dimensional layered thin-film transistors and their fabrication technology, specifically using graphene as the channel layer and indium selenide as the light absorption layer; and achieving a field-effect transistor with positive / negative photoconductivity switching at different laser power densities through the interaction between the indium selenide layer and the graphene layer. Background Technology
[0002] In recent years, two-dimensional semiconductor materials have become a research hotspot due to their unique structure and excellent physical properties. Common two-dimensional materials include two-dimensional layered materials, two-dimensional perovskites, and two-dimensional nanosheets. Compared with traditional materials, novel two-dimensional semiconductor materials possess atomic-level thickness, large specific surface area, continuously tunable band gaps, and excellent electron transport properties. In particular, for two-dimensional layered materials, the layers are bonded together by weak van der Waals forces, making it possible to stack different materials.
[0003] Two-dimensional graphene has a hexagonal carbon crystal structure, and the outermost electrons of carbon atoms readily interact with adjacent carbon atoms via sp... 2 Hybridization allows the free electrons formed to move freely within the crystal. At room temperature, the carrier mobility of graphene is approximately 130-10000 cm⁻¹. 2 / Vs, its mobility can reach 230-100000 cm under low temperature conditions. 2 The charge carrier mobility of graphene is significantly higher than that of traditional semiconductor materials, reaching / Vs. Furthermore, graphene exhibits excellent conductivity and a zero bandgap, with its energy distribution satisfying the Dirac equation. As a two-dimensional material possessing high carrier mobility, bipolar conductivity, and controllable bandgap, graphene has found widespread application in electronic devices. Compared to traditional optoelectronic devices, graphene-channel transistors can switch between positive and negative photoconductivity, further enriching the application scenarios of graphene devices and providing a new approach for the development of other two-dimensional materials. Summary of the Invention
[0004] The purpose of this invention is to provide a field-effect transistor with positive and negative photoconductivity switching and its fabrication method. The method obtains a hexagonal boron nitride layer, an indium selenide layer and a graphene layer by mechanical exfoliation, and then transfers them sequentially onto a silicon dioxide / P-type heavily doped silicon substrate. The electrode positions are then calibrated by patterning, and finally, a gold electrode is deposited using a thermal evaporation coating instrument.
[0005] The specific technical solution for achieving the objective of this invention is as follows: A method for fabricating a field-effect transistor with positive and negative photoconductivity switching, the method comprising the following specific steps: Step 1: Fabrication of the transistor channel layer A1: Substrate preparation Select a P-type heavily doped silicon substrate with 95-300nm silica. Cut it into squares with a side length of 0.5-5cm using a diamond knife. Place it in acetone, anhydrous ethanol and deionized water for ultrasonic cleaning for 10-30 minutes in sequence. Finally, use a nitrogen gun to blow dry the residual deionized water on the substrate surface for later use. This completes the preparation of the substrate. A2: Preparation of two-dimensional material layers by mechanical exfoliation method First, clean the slides, backing plate, and tweezers with alcohol; second, cut the blue film tape into pieces with an area of 3-10 cm². 2 The PDMS is cut into long strips and the two-dimensional material is picked up with tweezers and adhered to a blue film tape. This is repeated 4-6 times to thin the material. Next, the PDMS is cut into squares with sides of 1-2 cm and adhered to a clean glass slide. The top protective layer is removed, and then the blue film tape with the two-dimensional material is pasted onto the PDMS. After pressing gently 2-4 times, the blue film tape is peeled off, transferring the two-dimensional material to the PDMS. The PDMS with the two-dimensional material is then observed under an optical microscope to identify a uniform two-dimensional material with a thickness of 10-50 nm and a length of 25-100 μm as the target two-dimensional material. Finally, the PDMS containing the sample is cut into squares with sides of 2-5 mm using a knife to serve as the target glass slide. The two-dimensional materials are: hexagonal boron nitride, graphene, and indium selenide. Step 2: Transfer of two-dimensional materials B1: Turning on and adjusting the transfer station Using a transfer stage, the selected target two-dimensional materials are stacked on the substrate in the order of hexagonal boron nitride, indium selenide, and graphene. First, the transfer stage software and control box switch are turned on in sequence, the microscope light brightness is adjusted to 30%-70%, and the transfer stage is leveled using a level. Second, the Z-axis manual device is adjusted to the top, and the electric movement device of the transfer stage is turned on and connected, ensuring that the electric device is in normal working condition. Finally, the external mechanical pump switch of the transfer stage is turned on, thus completing the start-up of the transfer stage. B2: Transfer of hexagonal boron nitride layer First, place the substrate prepared in step A1 at the central hole of the stage, and turn on the VAC switch on the control panel to allow the stage to hold the substrate in place during transfer. Second, focus on the substrate surface by adjusting the coarse / fine adjustment knobs, locate a clean surface, and move it to the center of the field of view using the X and Y axes of the stage. Third, fix the target glass slide with hexagonal boron nitride (BON) selected in step A2 onto the transfer stage fixture, with the BON side facing the substrate. Rotate the fixture to center the PDMS with the two-dimensional material in the field of view. Next, under low magnification, adjust the coarse / fine adjustment knobs to locate and sharpen the BON. Use the X and Y axes of the fixture to move the BON to the center of the screen, and adjust the Z-axis movement speed to 30-1000 μm / s to slowly lower the fixture to a position 2-10 mm from the substrate. During the descent of the stage, the fine adjustment knob is continuously adjusted to maintain a clear view of the sample. Then, the Z-axis movement speed is reduced to 0.1-0.5 μm / s to control the stage to approach the substrate surface at a slower speed. When ripples are observed on the screen, the magnifying lens is used to slowly lower the Z-axis at 0.1-0.5 μm / s. Once the hexagonal boron nitride is fully bonded to the substrate, it is held for 3-4 seconds, then slowly moved upwards along the Z-axis at 0.1-0.3 μm / s until the PDMS is completely separated from the substrate. During this upward movement, the bonding state between the hexagonal boron nitride and the substrate is observed. If separation occurs, the Z-axis is immediately lowered to ensure complete bonding. Finally, after the PDMS is completely separated from the substrate, the coarse / fine adjustment knob of the transfer stage is adjusted to focus on the substrate surface to observe the bonding state between the hexagonal boron nitride and the substrate. If complete bonding is achieved, the hexagonal boron nitride layer has been successfully transferred. B3: Transfer of indium selenide layer First, place the substrate with the hexagonal boron nitride layer prepared in step B2 at the central hole of the stage. Turn on the VAC switch of the control box and adjust the coarse / fine focus knob to focus on the substrate surface under a low-power microscope. Adjust the X and Y axes of the stage to center the hexagonal boron nitride layer in the field of view. Second, clamp the target slide with indium selenide attached to the stage, ensuring that the indium selenide is facing down. Rotate the stage to center the PDMS on the target slide in the field of view and adjust the relative position of the indium selenide and the hexagonal boron nitride layer. Third, adjust the Z-axis movement speed to 30-1000 μm / s to slowly descend to a distance from the hexagonal boron nitride layer. At a position 2-10 mm above the boron layer surface, continuously adjust the fine adjustment knob to maintain a clear field of view as the stage descends. When ripples appear in the field of view, reduce the descent rate of the Z-axis to 0.1-0.5 μm / s, while simultaneously adjusting the microscope magnification. After the indium selenide layer and the hexagonal boron nitride layer are completely bonded, hold for 3-4 seconds, then slowly move the Z-axis upward at a speed of 0.1-0.3 μm / s until the PDMS and indium selenide layer are completely separated. Finally, move the stage to one side and adjust the coarse / fine adjustment knob to focus on the substrate surface to observe the bonding status of the indium selenide layer and the hexagonal boron nitride layer. If they are completely bonded, the transfer is successful. B4: Transfer of graphene layers First, place the substrate with the hexagonal boron nitride / indium selenide layer prepared in step B3 at the central hole of the stage. Turn on the VAC switch of the control box and focus under a low-power microscope. Adjust the X and Y axes of the stage to center the hexagonal boron nitride / indium selenide layer in the field of view. Second, clamp the target slide with the graphene attached onto the stage, ensuring the graphene is facing down. Rotate the stage to center the PDMS on the target slide in the field of view and adjust the relative position of the graphene and the hexagonal boron nitride / indium selenide layer. Third, adjust the Z-axis movement speed to 30-1000 μm / s to slowly lower it to a position 2-10 mm from the surface of the hexagonal boron nitride / indium selenide layer. During the stage descent, continuously adjust the fine adjustment knob to maintain a clear field of view. When ripples appear in the field of view, reduce the descent rate of the Z-axis to 0.1-0.5 μm / s, while simultaneously adjusting the microscope magnification. After the graphene and hexagonal boron nitride / indium selenide layer are fully bonded, let it stand for 3-4 seconds, then slowly move the Z-axis upward at a speed of 0.1-0.3 μm / s until the PDMS and graphene layer are completely separated. Finally, move the stage to one side and adjust the coarse / fine adjustment knob to focus on the substrate surface to observe the bonding status of the graphene layer and the hexagonal boron nitride / indium selenide layer. If they are fully bonded, the transfer is successful. This completes the preparation of the hexagonal boron nitride / indium selenide / graphene sample, i.e., the transfer of two-dimensional materials. Step 3: Fabrication of transistor source and drain electrodes C1: Sample patterning High-temperature adhesive tape was applied around the edges of the copper mesh mask and cut into squares. The operation was performed using a two-dimensional material transfer system: First, the computer host, transfer system software, equipment control box, and microscope were turned on sequentially, and the microscope lamp brightness was adjusted to 30%-70%. Second, a custom-made parallel plate module was placed on the adsorption device, and a level was used to check if the parallel plate module was level; if not, it was adjusted to be level. Next, the sample prepared in step B4 was placed inside the substrate and fixed on the parallel plate. The microscope magnification was adjusted to focus on the substrate surface, and the X and Y axes of the stage were moved to center the sample in the field of view. Subsequently, the copper mesh mask was adhered to the glass slide and fixed on the fixture stage. The copper mesh mask was placed directly below the microscope, and the microscope magnification was adjusted to maximum. The microscope is focused on the surface of a copper mesh mask, and its position is marked on the screen. Then, the microscope is focused on the sample surface, and the sample orientation is adjusted so that the length of the indium selenide layer in the channel is 6-14 nm, and the length of the graphene layer is 15-25 nm. This ensures that only one end of the indium selenide layer and both ends of the graphene layer are visible after the copper mesh mask is attached. The Z-axis is slowly lowered at a rate of 30-1000 μm / s to gradually bring the copper mesh mask into contact with the sample. Once fully attached, ensuring no deviation between the copper mesh mask and sample positions, the glass slide is slowly lifted at a rate of 20-500 μm / s while the edges of the copper mesh mask are pressed by hand to separate it from the slide. Finally, the edges of the copper mesh mask are pressed to ensure a tighter fit with the substrate. This completes the sample patterning process. C2: Source and drain electrodes of vapor-deposited transistors First, the patterned sample prepared in step C1 is fixed on the sample plate of a thermal evaporation coating instrument. Two to five gold particles are placed in the tungsten boat in the chamber, and the chamber is closed. Second, the mechanical pump and molecular pump are turned on in sequence to evacuate the chamber to a vacuum. Finally, the current at both ends of the tungsten boat is slowly increased until the gold particles melt and evaporate. The evaporation rate of the gold particles is controlled to complete the preparation of the 30-100nm source and drain electrodes. Thus, the preparation of the hexagonal boron nitride / indium selenide / graphene field-effect transistor is completed, that is, the positive and negative photoconductivity switching field-effect transistor is obtained.
[0006] A field-effect transistor with positive and negative photoconductivity switching prepared by the above method.
[0007] The greatest advantage of this invention compared to existing technologies lies in its simplicity, low cost, and the ability to achieve different photoconductive effects on a single device. By adding an indium selenide layer to a single graphene field-effect transistor, the device's functionality can be diversified. Attached Figure Description
[0008] Figure 1 This is a schematic diagram of the cross-sectional structure of the field-effect transistor obtained by the method described in this invention; Figure 2 In an embodiment of the present invention, the field-effect transistor operates at a power density of 0.24 mW / cm². 2 Optical response curve under a 405 nm laser wavelength; Figure 3 In an embodiment of the present invention, the field-effect transistor operates at a power density of 36.9 mW / cm². 2 The optical response curve under a 405 nm laser wavelength. Implementation
[0009] The present invention will be further described below with reference to the accompanying drawings, embodiments, and comparative examples.
[0010] See Figure 1 The field-effect transistor with positive and negative photoconductivity switching described in this invention includes a metal electrode 1, an asymmetric indium selenide layer 2, a two-dimensional material channel layer 3, a hexagonal boron nitride layer 4, a dielectric layer 5, and a gate electrode 6; wherein, the gate electrode 6 is a p-type heavily doped silicon substrate, the dielectric layer 5 is a silicon dioxide layer, the two-dimensional material channel layer 3 is a graphene layer, the asymmetric indium selenide layer 2, the hexagonal boron nitride layer 4, and the graphene layer 3 are all prepared by mechanical exfoliation, and the metal electrode 1 is prepared by thermal evaporation coating. Example
[0011] Fabrication of graphene field-effect transistors containing an asymmetric indium selenide layer: (1) Select a P-type heavily doped silicon substrate with 300nm silicon dioxide, and use a diamond knife to cut a square with a side length of 0.5cm. Place it in acetone, anhydrous ethanol and deionized water for ultrasonic cleaning for 15min in sequence. Finally, use a nitrogen gun to blow dry the residual deionized water on the substrate surface for later use. (2) First, select 10 glass slides and wipe them clean with cotton balls soaked in alcohol. At the same time, clean the pad and tweezers with alcohol. Then, cut the blue film tape into pieces with an area of 8cm². 2Using tweezers, separate strips of hexagonal boron nitride, indium selenide, and graphene are picked up and adhered to individual blue adhesive tapes. First, the blue adhesive tape with the hexagonal boron nitride strips is folded in half four times to thin it. The PDMS is then cut into 1cm squares, which are then pasted onto the upper left corner of a clean glass slide, and the top protective layer is removed. Next, the blue adhesive tape with the hexagonal boron nitride strips is pasted onto the PDMS, and after pressing gently twice, the blue adhesive tape is peeled off. Hexagonal boron nitride was transferred onto PDMS. The PDMS with the hexagonal boron nitride was observed under an optical microscope to identify a uniform hexagonal boron nitride thin layer with a thickness of 30 nm and a size of 50 μm. Next, blue film tape with indium selenide (ISS) was folded in half five times to thin it out. The PDMS was then cut into squares with sides of 1 cm, and the squares were pasted onto the upper left corner of a clean glass slide. The top protective layer was removed. Then, blue film tape with ISS was pasted onto the PDMS, pressed lightly twice, and then the blue film tape was peeled off. The ISS was then transferred onto the PDMS. The PDMS with ISS was observed under an optical microscope to identify a uniform ISS layer with a thickness of 20 nm and a size of 25 μm. Finally, blue film tape with graphite (ISS) was folded in half six times to thin it out. The PDMS was then cut into squares with sides of 1 cm, and the squares were pasted onto the upper left corner of a clean glass slide. The top protective layer was then removed, and a blue film tape containing the graphite block was adhered to the PDMS. After pressing gently three times, the blue film tape was peeled off, transferring the graphite onto the PDMS. The PDMS with the graphite was then observed under an optical microscope to identify a graphene thin layer with uniform texture, a thickness of 1 nm, and a size of 35 μm for later use. Finally, the PDMS containing hexagonal boron nitride, indium selenide, and graphene was cut into squares with sides of 5 mm using a knife. This completes the preparation of the hexagonal boron nitride layer, indium selenide layer, and graphene layer. (3) Using a transfer stage, the selected target two-dimensional materials are stacked on the substrate in the order of hexagonal boron nitride, indium selenide, and graphene. First, turn on the transfer stage software and control box switch in sequence, adjust the microscope light brightness to 50%, and use a level to adjust the transfer stage to be horizontal; second, adjust the Z-axis manual device to the top, turn on the electric moving device of the transfer stage and complete the connection, and ensure that the electric device is in normal working condition; finally, turn on the external mechanical pump switch of the transfer stage, thus completing the start-up of the transfer stage. (4) First, place the clean silicon / silica substrate prepared in step (1) at the central hole of the stage, and turn on the "VAC" switch on the control box panel to enable the stage to adsorb the substrate and ensure that the substrate remains fixed during the transfer process; second, focus on the substrate surface by adjusting the coarse / fine adjustment knob, find the clean surface, and move it to the center of the field of view with the help of the X and Y axes of the stage; then, fix the selected target glass slide with hexagonal boron nitride on the transfer stage fixture, so that the side with hexagonal boron nitride faces the substrate; then, rotate the fixture stage to place the PDMS with hexagonal boron nitride in the center of the field of view; then, adjust the coarse / fine adjustment knob under low magnification to find the position of hexagonal boron nitride and adjust it to be clear, use the X and Y axes of the fixture stage to move the hexagonal boron nitride to the center of the screen, and adjust the Z axis movement speed to 500 μm / s to control the fixture stage to slowly descend. The stage is lowered to a position 3 mm from the substrate. During the descent of the stage, the fine adjustment knob is continuously adjusted to maintain a clear view of the sample. Then, the Z-axis movement speed is reduced to 0.5 μm / s to control the stage to approach the substrate surface at a slower speed. When ripples are seen on the screen, the Z-axis is slowly lowered using the magnifying lens. Once the hexagonal boron nitride is fully bonded to the substrate, it is held for 4 seconds and then slowly moved upwards along the Z-axis at a speed of 0.1 μm / s until the PDMS is completely separated from the substrate. During the upward movement, the bonding between the hexagonal boron nitride and the substrate is carefully observed. If it separates from the substrate, the Z-axis is immediately lowered to ensure that the hexagonal boron nitride is fully bonded to the substrate. Finally, after the PDMS is completely separated from the substrate, the coarse / fine adjustment knob of the transfer stage is adjusted to focus on the substrate surface to observe the bonding between the hexagonal boron nitride and the substrate. If they are fully bonded, it indicates that the hexagonal boron nitride layer has been successfully transferred.
[0012] (5) First, place the substrate with the hexagonal boron nitride layer prepared in step (4) at the central hole of the stage, turn on the "VAC" switch of the control box, and adjust the coarse / fine focus knob to focus on the substrate surface under a low magnification microscope. Adjust the X and Y axes of the stage to place the hexagonal boron nitride layer in the center of the field of view. Second, clamp the target slide with indium selenide on the stage and ensure that the indium selenide layer is facing down. Rotate the stage to place the PDMS on the target slide in the center of the field of view and adjust the relative position of the indium selenide and the hexagonal boron nitride layer. Position the indium selenide directly above the boron nitride layer. Adjust the Z-axis movement speed to 500 μm / s, slowly lowering it to a position 3 mm from the surface of the hexagonal boron nitride layer. During the descent of the stage, continuously adjust the fine adjustment knob to maintain a clear field of view. When ripples appear in the field of view, reduce the Z-axis descent speed to 0.5 μm / s, simultaneously adjusting the microscope magnification. After the indium selenide and hexagonal boron nitride layers are completely adhered, hold for 4 seconds, then slowly move the Z-axis upwards at a speed of 0.1 μm / s until the PDMS and indium selenide layers are completely separated. Finally, move the stage to one side and adjust the coarse / fine adjustment knob to focus on the sample surface to observe the adhesion between the indium selenide and hexagonal boron nitride layers. If they are completely adhered, the transfer is successful. (6) Place the substrate with the hexagonal boron nitride / indium selenide layer prepared in step (5) at the central hole of the stage, turn on the "VAC" switch of the control box, and adjust the coarse / fine focus knob to focus on the substrate surface under a low magnification microscope. Adjust the X and Y axes of the stage to place the hexagonal boron nitride / indium selenide layer in the center of the field of view. Next, clamp the target slide with the graphene layer on the stage and ensure that the graphene layer is facing down. Rotate the stage to place the PDMS on the target slide in the center of the field of view. Adjust the relative position of the graphene layer and the hexagonal boron nitride / indium selenide layer. Position the indium selenide directly above the boron nitride / indium selenide layer. Adjust the Z-axis movement rate to 500 μm / s, slowly lowering it to a position 3 mm from the surface of the hexagonal boron nitride / indium selenide layer. Continuously adjust the fine adjustment knob during the stage descent to maintain a clear field of view. When ripples appear in the field of view, reduce the Z-axis descent rate to 0.5 μm / s, simultaneously adjusting the microscope magnification. After the indium selenide layer and the hexagonal boron nitride / indium selenide layer are completely adhered, hold for 4 seconds, then slowly move the Z-axis upwards at a rate of 0.1 μm / s until the PDMS and graphene layer are completely separated. Finally, move the stage to one side and adjust the coarse / fine adjustment knobs to focus on the sample surface to observe the adhesion between the graphene layer and the hexagonal boron nitride / indium selenide layer. If they are completely adhered, the transfer is successful. (7) Apply high-temperature tape around the copper mesh mask and cut it into squares. Use a two-dimensional material transfer system to operate: First, turn on the computer host, transfer system software, equipment control box and microscope in sequence, and adjust the brightness of the microscope lamp source to 60%; Second, place the customized parallel plate module on the adsorption device, and use a level to check whether the parallel plate module is in a horizontal state. If it is not in a horizontal state, adjust it to a horizontal state. Next, place the sample prepared in step (6) in the substrate and fix it on the parallel plate. Adjust the magnification of the microscope to focus it on the substrate surface, and move the X-axis and Y-axis of the stage to center the sample in the field of view. Subsequently, the copper mesh mask was adhered to the glass slide and fixed on the stage. The copper mesh mask was placed directly below the microscope, and the microscope magnification was adjusted to the maximum and focused on the surface of the copper mesh mask. The position of the copper mesh mask was marked on the screen. Then, after focusing the microscope on the sample surface, the orientation of the sample was adjusted so that the length of indium selenide in the channel was 12 μm and the length of graphene in the channel was 15 μm. The Z-axis was slowly lowered at a rate of 500 μm / s to gradually bring the copper mesh mask into contact with the sample. After complete contact, it was ensured that the position of the copper mesh mask was not deviated from the position of the sample. The glass slide was slowly lifted at a rate of 60 μm / s while pressing the edge of the copper mesh mask by hand to separate it from the glass slide. Finally, the edges of the copper mesh mask were pressed to make it adhere more tightly to the substrate. The patterned sample was then fixed on the sample plate of the thermal evaporation coating instrument. Three gold particles were placed inside the tungsten boat in the chamber, and the chamber was closed. The mechanical pump and molecular pump were turned on sequentially to evacuate the chamber to a vacuum. The voltage across the tungsten boat was slowly increased until the gold particles melted and evaporated. The evaporation rate of the gold particles was controlled to complete the fabrication of the 50nm source and drain electrodes. This completed the fabrication of the hexagonal boron nitride / indium selenide / graphene field-effect transistor, whose structure is shown below. Figure 1 As shown.
[0013] The optical and electrical properties of the field-effect transistors fabricated in the examples were analyzed using a Janis ST-500 vacuum probe stage and a Keithley 4200-SCS semiconductor parameter analyzer, as follows: Figure 2 The field-effect transistor fabricated for an embodiment of the present invention has a power density of 0.24 mW / cm². 2 The photoresponse curve under a 405 nm laser wavelength shows that the field-effect transistor exhibits a negative photoconductivity under this illumination condition, meaning that the field-effect transistor shows a decrease in current under illumination.
[0014] Figure 3 The field-effect transistor fabricated in this embodiment of the invention achieves a power density of 36.9 mW / cm². 2The photoresponse curve under a 405 nm laser wavelength shows that the field-effect transistor exhibits a positive photoconductivity under this illumination condition, that is, the field-effect transistor based on the graphene channel layer exhibits the characteristic of current increase under illumination.
[0015] contrast Figure 2 and Figure 3 The data shows that the field-effect transistor based on the graphene channel layer of this invention exhibits different photoconductive effects under different laser power densities, realizing the diversity of semiconductor device functions. Therefore, the field-effect transistor containing an indium selenide layer prepared in this invention can achieve more diverse functions based on a single device, and the preparation process is simple and easy to operate, which is of great significance for enriching the functional diversity of two-dimensional materials.
Claims
1. A method for fabricating a field-effect transistor with positive and negative photoconductivity switching, characterized in that, The method includes the following specific steps: Step 1: Fabrication of the transistor channel layer A1: Substrate preparation Select a P-type heavily doped silicon substrate with 95-300nm silica. Cut it into squares with a side length of 0.5-5cm using a diamond knife. Place it in acetone, anhydrous ethanol and deionized water for ultrasonic cleaning for 10-30 minutes in sequence. Finally, use a nitrogen gun to blow dry the residual deionized water on the substrate surface for later use. This completes the preparation of the substrate. A2: Preparation of two-dimensional material layers by mechanical exfoliation method First, clean the slides, backing plate, and tweezers with alcohol; second, cut the blue film tape into pieces with an area of 3-10 cm². 2 The PDMS is cut into long strips and the two-dimensional material is picked up with tweezers and adhered to a blue film tape. This is repeated 4-6 times to thin the material. Next, the PDMS is cut into squares with sides of 1-2 cm and adhered to a clean glass slide. The top protective layer is removed, and then the blue film tape with the two-dimensional material is pasted onto the PDMS. After pressing gently 2-4 times, the blue film tape is peeled off, transferring the two-dimensional material to the PDMS. The PDMS with the two-dimensional material is then observed under an optical microscope to identify a uniform two-dimensional material with a thickness of 10-50 nm and a length of 25-100 μm as the target two-dimensional material. Finally, the PDMS containing the sample is cut into squares with sides of 2-5 mm using a knife to serve as the target glass slide. The two-dimensional materials are: hexagonal boron nitride, graphene, and indium selenide. Step 2: Transfer of two-dimensional materials B1: Turning on and adjusting the transfer station Using a transfer stage, the selected target two-dimensional materials are stacked on the substrate in the order of hexagonal boron nitride, indium selenide, and graphene. First, the transfer stage software and control box switch are turned on in sequence, the microscope light brightness is adjusted to 30%-70%, and the transfer stage is leveled using a level. Second, the Z-axis manual device is adjusted to the top, and the electric movement device of the transfer stage is turned on and connected, ensuring that the electric device is in normal working condition. Finally, the external mechanical pump switch of the transfer stage is turned on, thus completing the start-up of the transfer stage. B2: Transfer of hexagonal boron nitride layer First, place the substrate prepared in step A1 at the central hole of the stage, turn on the VAC switch on the control box panel to enable the stage to adsorb the substrate and ensure that the substrate remains stationary during the transfer process; second, focus on the substrate surface by adjusting the coarse / fine focus knob, find a clean surface, and move it to the center of the field of view with the help of the X and Y axes of the stage. Next, fix the target glass slide with hexagonal boron nitride (BON) selected in step A2 onto the transfer stage fixture, with the BON-coated side facing the substrate. Rotate the fixture stage to center the PDMS with the two-dimensional material in the field of view. Then, under low magnification, adjust the coarse / fine adjustment knobs to locate and sharpen the BON. Use the X and Y axes of the fixture stage to move the BON to the center of the screen. Adjust the Z-axis movement speed to 30-1000 μm / s to slowly lower the fixture stage to a position 2-10 mm from the substrate. During the descent, continuously adjust the fine adjustment knob to maintain a clear view of the sample. Subsequently, reduce the Z-axis movement speed to 0.1-0.5 μm / s. The stage is controlled to approach the substrate surface at a slower speed. When ripples are seen on the screen, the magnifying lens is controlled to slowly descend at a Z-axis speed of 0.1-0.5 μm / s. After the hexagonal boron nitride is completely bonded to the substrate, it is held for 3-4 seconds and then slowly moved upward along the Z-axis at a speed of 0.1-0.3 μm / s until the PDMS is completely separated from the substrate. During the upward movement, the bonding state between the hexagonal boron nitride and the substrate is observed. If it separates from the substrate, the Z-axis is moved downward in time to ensure that the hexagonal boron nitride is completely bonded to the substrate. Finally, after the PDMS is completely separated from the substrate, the coarse / fine focus knob of the transfer stage is adjusted to focus on the substrate surface to observe the bonding state between the hexagonal boron nitride and the substrate. If they are completely bonded, it means that the hexagonal boron nitride layer has been successfully transferred. B3: Transfer of indium selenide layer First, place the substrate with the hexagonal boron nitride layer prepared in step B2 at the central hole of the stage. Turn on the VAC switch of the control box and adjust the coarse / fine focus knob to focus on the substrate surface under a low-power microscope. Adjust the X and Y axes of the stage to center the hexagonal boron nitride layer in the field of view. Second, clamp the target slide with indium selenide attached to the stage, ensuring that the indium selenide is facing down. Rotate the stage to center the PDMS on the target slide in the field of view and adjust the relative position of the indium selenide and the hexagonal boron nitride layer. Third, adjust the Z-axis movement speed to 30-1000 μm / s to slowly descend to a distance from the hexagonal boron nitride layer. At a position 2-10 mm above the boron layer surface, continuously adjust the fine adjustment knob to maintain a clear field of view as the stage descends. When ripples appear in the field of view, reduce the descent rate of the Z-axis to 0.1-0.5 μm / s, while simultaneously adjusting the microscope magnification. After the indium selenide layer and the hexagonal boron nitride layer are completely bonded, hold for 3-4 seconds, then slowly move the Z-axis upward at a speed of 0.1-0.3 μm / s until the PDMS and indium selenide layer are completely separated. Finally, move the stage to one side and adjust the coarse / fine adjustment knob to focus on the substrate surface to observe the bonding status of the indium selenide layer and the hexagonal boron nitride layer. If they are completely bonded, the transfer is successful. B4: Transfer of graphene layers First, place the substrate with the hexagonal boron nitride / indium selenide layer prepared in step B3 at the central hole of the stage. Turn on the VAC switch of the control box and focus under a low-power microscope. Adjust the X and Y axes of the stage to center the hexagonal boron nitride / indium selenide layer in the field of view. Second, clamp the target slide with the graphene attached onto the stage, ensuring the graphene is facing down. Rotate the stage to center the PDMS on the target slide in the field of view and adjust the relative position of the graphene and the hexagonal boron nitride / indium selenide layer. Third, adjust the Z-axis movement speed to 30-1000 μm / s to slowly lower it to a position 2-10 mm from the surface of the hexagonal boron nitride / indium selenide layer. During the stage descent, continuously adjust the fine adjustment knob to maintain a clear field of view. When ripples appear in the field of view, reduce the descent rate of the Z-axis to 0.1-0.5 μm / s, while simultaneously adjusting the microscope magnification. After the graphene and hexagonal boron nitride / indium selenide layer are fully bonded, let it stand for 3-4 seconds, then slowly move the Z-axis upward at a speed of 0.1-0.3 μm / s until the PDMS and graphene layer are completely separated. Finally, move the stage to one side and adjust the coarse / fine adjustment knob to focus on the substrate surface to observe the bonding status of the graphene layer and the hexagonal boron nitride / indium selenide layer. If they are fully bonded, the transfer is successful. This completes the preparation of the hexagonal boron nitride / indium selenide / graphene sample, i.e., the transfer of two-dimensional materials. Step 3: Fabrication of transistor source and drain electrodes C1: Sample patterning High-temperature adhesive tape was applied around the edges of the copper mesh mask and cut into squares. The operation was performed using a two-dimensional material transfer system: First, the computer host, transfer system software, equipment control box, and microscope were turned on sequentially, and the microscope lamp brightness was adjusted to 30%-70%. Second, a custom-made parallel plate module was placed on the adsorption device, and a level was used to check if the parallel plate module was level; if not, it was adjusted to be level. Next, the sample prepared in step B4 was placed inside the substrate and fixed on the parallel plate. The microscope magnification was adjusted to focus on the substrate surface, and the X and Y axes of the stage were moved to center the sample in the field of view. Subsequently, the copper mesh mask was adhered to the glass slide and fixed on the fixture stage. The copper mesh mask was placed directly below the microscope, and the microscope magnification was adjusted to maximum. The microscope is focused on the surface of a copper mesh mask, and its position is marked on the screen. Then, the microscope is focused on the sample surface, and the sample orientation is adjusted so that the length of the indium selenide layer in the channel is 6-14 nm, and the length of the graphene layer is 15-25 nm. This ensures that only one end of the indium selenide layer and both ends of the graphene layer are visible after the copper mesh mask is attached. The Z-axis is slowly lowered at a rate of 30-1000 μm / s to gradually bring the copper mesh mask into contact with the sample. Once fully attached, ensuring no deviation between the copper mesh mask and sample positions, the glass slide is slowly lifted at a rate of 20-500 μm / s while the edges of the copper mesh mask are pressed by hand to separate it from the slide. Finally, the edges of the copper mesh mask are pressed to ensure a tighter fit with the substrate. This completes the sample patterning process. C2: Source and drain electrodes of vapor-deposited transistors First, the patterned sample prepared in step C1 is fixed on the sample plate of a thermal evaporation coating instrument. Two to five gold particles are placed in the tungsten boat in the chamber, and the chamber is closed. Second, the mechanical pump and molecular pump are turned on in sequence to evacuate the chamber to a vacuum. Finally, the current at both ends of the tungsten boat is slowly increased until the gold particles melt and evaporate. The evaporation rate of the gold particles is controlled to complete the preparation of the 30-100nm source and drain electrodes. Thus, the preparation of the hexagonal boron nitride / indium selenide / graphene field-effect transistor is completed, that is, the positive and negative photoconductivity switching field-effect transistor is obtained.
2. A field-effect transistor with positive and negative photoconductivity switching, prepared by the method of claim 1.