A method for preparing a solar cell

By configuring the target group, the consumption value of the control TCO film layer is not more than 80%, which solves the problem of film thickness uneven due to uneven target consumption, and improves the uniformity of the film layer and the utilization rate of the target material.

CN116314464BActive Publication Date: 2024-11-26TONGWEI SOLAR (JINTANG) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310315898.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-11-26
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

During the preparation of TCO film layer of solar cells, uneven target consumption leads to uneven film thickness, affecting the appearance and performance of the battery.

Method used

By configuring the target group, ensure that the consumption value of at least one TCO target is not greater than 80%, and TCO targets with different consumption values ​​are set in the target group to control their consumption differences to ensure uniformity and extension of the membrane layer. The service life of the target material.

Benefits of technology

It effectively improves the uniformity of the TCO film, reduces the thickness deviation of the film formation at both ends and middle of the battery matrix, extends the service life of the target material, and avoids the waste of the target material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN116314464B_ABST
    Figure CN116314464B_ABST
Patent Text Reader

Abstract

A method for preparing a solar cell belongs to the technical field of solar cells. The method comprises: configuring a TCO target material to obtain a target material group; preparing a TCO film on a cell substrate using the target material group to obtain a solar cell; in the process of preparing the TCO film, the target material group always includes at least one target material with a target material consumption value of no more than 80%; along the extension direction of the target material, the cross-sectional areas of the TCO target material with a consumption value of 0 are all equal; by controlling the target material group to always maintain at least one target material with a consumption value of no more than 80%, the phenomenon that the film formed at the two ends of the cell substrate corresponding to the target material is thicker than the film formed at the middle position of the target material can be improved, thereby effectively improving the uniformity of the TCO film.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of solar cells, and in particular, to a method for preparing a solar cell. Background Art

[0002] SHJ (Silicon Herterojunction) silicon heterojunction cells, also known as HIT (Heterojunction with intrinsic thin layer) cells, have the characteristics of high efficiency and high Voc. The cells are generally based on N-type silicon wafers, and the manufacturing process is generally: texturing, deposition of amorphous silicon, deposition of TCO, screen printing and testing. In addition to meeting the properties of high transmittance and high conductivity, the appearance of TCO should also be as uniform as possible. If the color deviation is too large, it is easy to cause color difference between the pieces, resulting in poor appearance at the component end. The color is mainly affected by the thickness of the TCO film. Among them, the preparation of TCO is made by target sputtering deposition. As the target material is consumed, the thickness uniformity of the TCO film layer becomes worse and worse. Summary of the invention

[0003] The purpose of the present application is to provide a method for preparing a solar cell to improve the problem of poor thickness uniformity of the current TCO film layer.

[0004] The inventors found during the invention process that when the TCO target is not consumed (e.g. Figure 1 ), the TCO target will be gradually consumed under the action of the magnetic field, and uneven etching will occur at both ends and in the middle of the TCO target, that is, the etching at both ends of the TCO target is deeper than that in the middle of the TCO target (such as Figure 2 ), at this time, the magnetic field enhances the deposition on the ends, resulting in a larger etching amount per unit time, which in turn leads to a thicker TCO film thickness on the battery substrate. Therefore, the film formed at both ends of the target corresponding to the battery substrate will be thicker than the film formed in the middle of the target. This phenomenon is more obvious when the target consumption value is larger, especially when the consumption value exceeds 80%.

[0005] Therefore, the present invention provides a method for preparing a solar cell, the method comprising:

[0006] The TCO target is configured to obtain a target set;

[0007] Using a target material group to prepare a TCO film on a cell substrate to obtain a solar cell;

[0008] During the preparation of the TCO film, the target group always includes at least one TCO target whose consumption value is not greater than 80%;

[0009] Along the extension direction of the TCO target, the cross-sectional areas of the TCO target with a target consumption value of 0 are all equal.

[0010] TCO target material consumption value X 消 The calculation formula is: X 消 =m 消 / m 初 , m 消 is the mass of TCO target after consumption, m 初 is the mass of unconsumed TCO target.

[0011] By controlling the consumption value X of at least one TCO target in the target group to be used, 消 Meeting the requirement of no more than 80% can improve the phenomenon that the film formed at both ends of the target corresponding to the silicon substrate is thicker than the film formed at the middle position of the target corresponding to the silicon substrate, thereby effectively improving the uniformity of the TCO film.

[0012] As an optional embodiment, the target material group includes a plurality of TCO targets; during the TCO film preparation process, the target material group always includes at least one third of the TCO targets with a consumption value X 消 Not more than 80%.

[0013] Satisfy consumption value X 消 The more the number of targets not exceeding 80%, the better the improvement effect on the phenomenon that the film formed at both ends of the corresponding target of the battery substrate is thicker than the film formed in the middle of the corresponding target. 消 The number of targets is not greater than 80%, and the number of targets should be a positive integer. In specific implementation, the consumption value X 消 The minimum number of targets not exceeding 80% is obtained by multiplying one third by the total number and then rounding off. For example, when the total number of targets in the target group is 5, the consumption value X is met. 消 Not more than 80% of the targets are 2 or more.

[0014] As an optional embodiment, during the TCO film preparation process, the target material group always includes at least one-half of the TCO target material consumption value X 消 Not more than 80%.

[0015] Those skilled in the art can determine the consumption value X according to the requirements of the product. 消 The number of targets not exceeding 80% is selected, and the consumption value X is satisfied. 消 The number of targets is not greater than 80%, and the number of targets should be a positive integer. In specific implementation, the consumption value X 消 The minimum number of targets not exceeding 80% is obtained by multiplying half by the total number and then rounding off. For example, when the total number of targets in the target group is 5, the consumption value X is met.消 Not more than 80% of the targets are 3 or more.

[0016] As an optional implementation, the target material group includes a plurality of TCO targets; the consumption values ​​of the plurality of TCO targets are different, wherein the extreme difference in target material consumption values ​​between the TCO targets with different consumption values ​​is not less than 20%.

[0017] By adopting the above design, when configuring the target material group, the consumption value difference between the targets is limited to no less than 20%. When preparing the TCO film in the future, it is not necessary to monitor each target material in real time to see if it meets the consumption value X of the target material. 消 The requirement of not more than 80% is met. Since the sputtering power for each target material is the same, it is only necessary to determine whether there is a target material whose consumption value reaches 100%. When the consumption value of a target material reaches 100%, naturally at least one target material in the target material group will have a consumption value that is not more than 80%. At the same time, if it can be ensured that after a certain target material is consumed, at least one target material's consumption value meets a smaller set consumption value, then during the entire preparation process there will always be a target material consumption value that meets the set value, thereby improving the uniformity of the TCO film.

[0018] As an optional implementation manner, the consumption value difference between TCO targets with different consumption values ​​is not less than 40%.

[0019] When configuring the stand-by target material group, the greater the extreme difference in consumption values ​​between the target materials, the more it can be ensured that after a certain target material is consumed, at least one target material's consumption value meets a smaller set consumption value. In the entire preparation process, there is always a target material's consumption value that meets a smaller set consumption value, thereby improving the uniformity of the prepared TCO film.

[0020] As an optional implementation, half of the TCO targets with different consumption values ​​have a consumption value of no less than 50%, and the other half of the TCO targets with different consumption values ​​have a consumption value of no more than 50%. Furthermore, half of the TCO targets with different consumption values ​​have a consumption value of 50%, and the other half of the TCO targets with different consumption values ​​have a consumption value of 0.

[0021] In the above implementation process, when half of the TCO target materials are consumed to 100%, the other half of the TCO target materials are consumed to 50%. At this time, the consumed TCO target materials are replaced. After the replacement is completed, the consumption value of half of the quantity is just 50%, and the consumption value of the other half is 0. This cycle is repeated and will not lead to the accumulation of TCO targets with a consumption value of 50%, thereby effectively ensuring the uniformity of the TCO film and avoiding the waste of TCO targets.

[0022] As an optional implementation, during the TCO film preparation process, the target material group always includes at least one TCO target material whose target material consumption value is no more than 70%.

[0023] As an optional implementation, during the TCO film preparation process, the target material group always includes at least one TCO target material whose target material consumption value is no more than 60%.

[0024] As an optional implementation, during the TCO film preparation process, the target material group always includes at least one TCO target material whose target material consumption value is no more than 50%.

[0025] The smaller the target consumption value of this part of the TCO target material is, the better the effect of improving the phenomenon that the film formed at both ends of the corresponding target material of the battery substrate is thicker than the film formed at the middle position of the corresponding target material.

[0026] As an optional embodiment, the target material sputtering power for preparing the TCO film is 3-9 kW; and / or the battery substrate moving speed for preparing the TCO film is 20-35 mm / s.

[0027] Technicians in this field can select and match the target sputtering power and the moving speed of the battery substrate according to actual needs. For example, the target sputtering power can be 3kW, 4kW, 5kW, 6kW, 7kW, 8kW and 9kW, and the moving speed of the battery substrate can be 20mm / s, 22mm / s, 24mm / s, 26mm / s, 27mm / s, 28mm / s, 30mm / s, 32mm / s, 34mm / s and 35mm / s.

[0028] As an optional implementation, the target material group includes a plurality of TCO targets; the plurality of TCO targets are arranged side by side, so that the thickness of the TCO film deposited on the battery substrate can be more uniform.

[0029] As an optional implementation, two ends of the plurality of TCO targets are flush.

[0030] As an optional implementation, along the extension direction of the TCO target, the distance between the end of the TCO target and the end of the battery substrate is 1%-10% of the length of the TCO target.

[0031] As an optional implementation, the distance between the end of the TCO target and the end of the battery substrate is 2%-4% of the length of the TCO target.

[0032] As an optional embodiment, a method for preparing a battery substrate includes: depositing intrinsic amorphous silicon layers on two surfaces of a silicon substrate, depositing an N-type amorphous silicon layer on one intrinsic amorphous silicon layer, and depositing a P-type amorphous silicon layer on another intrinsic amorphous silicon layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0034] Figure 1 A schematic diagram of the structure of a target material with a consumption value of 0 provided in an embodiment of the present application;

[0035] Figure 2 A schematic diagram of the structure of a target material after being consumed for a period of time provided in an embodiment of the present application;

[0036] Figure 3 A flowchart of a method provided in an embodiment of the present application. DETAILED DESCRIPTION

[0037] The embodiments of the present application will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. In the examples, if specific conditions are not specified, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.

[0038] SHJ (Silicon Herterojunction) silicon heterojunction battery, also known as HIT (Heterojunction with intrinsic thin layer) battery, has the characteristics of high efficiency and high Voc. The battery is generally based on N-type silicon wafers. The manufacturing process is generally: texturing, deposition of amorphous silicon, deposition of TCO, screen printing and testing. In the production process of heterojunction batteries, the PVD process not only ensures the normal electrical performance, but also needs to be responsible for the appearance and color of the battery. If the color deviation is too large, it is easy to cause color difference between the pieces, resulting in poor appearance at the subsequent component end. Adjusting the color of the battery cell is achieved by adjusting the TCO film thickness. The inventor found in the process of the invention that when the TCO target material is not consumed (such as Figure 1 ), the target material will gradually be consumed under the action of the magnetic field, and uneven etching will occur at both ends and in the middle of the target material, that is, the etching at both ends of the target material is deeper than that in the middle of the target material (such as Figure 2), at this time, the magnetic field enhances the deposition on the ends, resulting in a larger etching amount per unit time, which in turn leads to a thicker film thickness of the cell, so the film formed at both ends of the target corresponding to the silicon substrate will be thicker than the film formed in the middle of the target. This phenomenon is more obvious when the target consumption value is larger, especially when the consumption value exceeds 80%.

[0039] Please refer to Figure 3 The present invention provides a method for preparing a solar cell, the method comprising:

[0040] S1. configuring the TCO target to obtain a target set;

[0041] In some embodiments, configuring TCO targets to obtain a target group specifically includes: configuring TCO targets with different consumption values ​​to obtain a target group; wherein the consumption value range between TCO targets with different consumption values ​​is not less than 20%.

[0042] By limiting the consumption value difference between TCO targets to no less than 20% when configuring the target group, it is not necessary to monitor each TCO target in real time to see whether the consumption value X of the TCO target is met during the subsequent TCO film preparation. 消 Not greater than the set consumption value X 设 (i.e. 80%) requirement. Since the sputtering power for each target material is the same, it is only necessary to determine whether there is a TCO target material whose consumption value reaches 100%. When the consumption value of a TCO target material reaches 100%, naturally at least one TCO target material in the target material group will have a consumption value that is not greater than 80%, thereby improving the uniformity of the TCO film.

[0043] When configuring the target group, the greater the range of consumption values ​​between TCO targets, the more it can ensure that after a certain TCO target is consumed, at least one TCO target's consumption value meets the smaller set consumption value, so that in the entire preparation process, there is always a TCO target's consumption value that meets the set value, thereby improving the uniformity of the prepared TCO film. Preferably, the range of consumption values ​​between TCO targets with different consumption values ​​is not less than 40%. With the above design, it can be achieved that when the consumption value of a TCO target reaches 100%, naturally at least one TCO target in the target group has a consumption value that does not exceed 60%, so in the entire preparation process, there is always a TCO target's consumption value that meets at least one TCO target's consumption value that does not exceed 60%, thereby better achieving the effect of improving the uniformity of the TCO film.

[0044] In order to achieve full utilization of TCO targets and to ensure that the TCO targets have a longer and uniform replacement frequency, in some embodiments, the consumption value of half of the TCO targets with different consumption values ​​is 50%, and the consumption value of the other half of the TCO targets with different consumption values ​​is 0. With the above design, when half of the TCO targets are consumed to 100%, the other half of the TCO targets are consumed to 50%. At this time, the consumed TCO targets are replaced. After the replacement is completed, the consumption value of half of the targets is just 50%, and the consumption value of the other half is 0. This cycle is repeated, which effectively ensures the uniformity of the TCO film and avoids the waste of TCO targets.

[0045] S2. Prepare a TCO film on the battery substrate using a target material group to obtain a blue film; during the TCO film preparation process, the target material group always includes at least one TCO target material consumption value X 消 Not greater than the set consumption value X 设 , set the consumption value X 设 is 80%; along the extension direction of the target, the cross-sectional areas of the TCO target with a consumption value of 0 are equal at all locations.

[0046] Target consumption value X 消 The calculation formula is: X 消 =m 消 / m 初 , m 消 is the mass of TCO target after consumption, m 初 is the mass of the unconsumed TCO target. It can be understood by those skilled in the art that the above is only one way to calculate the consumption value. In other embodiments, other ways can be used to calculate the consumption value, such as using volume as an indicator or using the height difference between the end and the middle as an indicator to reflect the consumption value. The cross-sectional area of ​​the target with a consumption value of 0, that is, the unconsumed target, is equal at all locations. The TCO target of the unconsumed target can be specifically selected from (pioneer ITO target 97:3).

[0047] By controlling the target group to always have at least one TCO target consumption value X 消 Satisfy the requirement of not exceeding the set consumption value X 设 (80%), which can improve the phenomenon that the film formed at both ends of the target material corresponding to the battery substrate is thicker than the film formed at the middle position of the target material, and effectively improve the uniformity of the TCO film.

[0048] The smaller the set consumption value is, the better the improvement effect is on the phenomenon that the film formed at both ends of the target material of the battery substrate is thicker than the film formed at the middle position of the target material. In some embodiments, the set consumption value X 设 The consumption value X can be set to 70%, 60% or 50% by those skilled in the art according to the requirements of the product. 设The inventor found that the control setting consumption value X 设 A value of 50% can not only ensure the uniformity of the TCO film, but also ensure that the replacement cycle of the target material is not significantly shortened.

[0049] Satisfy consumption value X 消 Not greater than the set consumption value X 设 The more TCO targets there are, the better the improvement effect on the phenomenon that the film formed at both ends of the corresponding target material of the battery substrate is thicker than the film formed at the middle position of the corresponding target material. In some embodiments, during the preparation of the TCO film, the target material group always includes at least one-third of the TCO targets with a consumption value of X. 消 Not greater than the set consumption value X 设 At this time, regarding the consumption value X 消 Not greater than the set consumption value X 设 The number of TCO targets should be a positive integer. In specific implementation, the consumption value X 消 Not greater than the set consumption value X 设 The minimum number of TCO targets is obtained by multiplying one third by the total number and rounding off. For example, when the total number of TCO targets in the target group is 5, the consumption value X 消 Not greater than the set consumption value X 设 The number of TCO targets is 2 or more.

[0050] Preferably, during the TCO film preparation process, the target set always includes at least one-half of the TCO target material with a consumption value X 消 Not greater than the set consumption value X 设 At this time, regarding the consumption value X 消 Not greater than the set consumption value X 设 The number of TCO targets should be a positive integer. In specific implementation, the consumption value X 消 Not greater than the set consumption value X 设 The minimum number of TCO targets is obtained by multiplying the total number by half and rounding it off. For example, when the total number of targets in the target group is 5, the consumption value X 消 Not greater than the set consumption value X 设 The number of TCO targets is 3 or more. The inventors found that the control meets the consumption value X 消 Not greater than the set consumption value X 设 The number of TCO targets accounts for half, which not only ensures the uniformity of the TCO film, but also ensures the utilization rate of the target material without causing accumulation and waste of TCO targets.

[0051] It should be noted that the configuration timing of the TCO target includes: when the consumption value of the TCO target in the target group reaches 100% or when the target group does not meet the consumption value X of at least one TCO target. 消 Not greater than the set consumption value X 设 hour.

[0052] In some embodiments, the target material sputtering power for preparing the TCO film is 3-9 kW; the battery substrate moving speed for preparing the TCO film is 20-35 mm / s.

[0053] Technicians in this field can select and match the target sputtering power and the moving speed of the battery substrate according to actual needs. For example, the target sputtering power can be 3kW, 4kW, 5kW, 6kW, 7kW, 8kW and 9kW, and the moving speed of the battery substrate can be 20mm / s, 22mm / s, 24mm / s, 26mm / s, 27mm / s, 28mm / s, 30mm / s, 32mm / s, 34mm / s and 35mm / s.

[0054] S3. Prepare the blue film into electrodes to obtain solar cells.

[0055] The present application is further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present application and are not used to limit the scope of the present application.

[0056] It should be noted that the PVD equipment used in the following embodiments and comparative examples is Jinshi PVD, which contains six target mounting positions.

[0057] Comparative Example 1

[0058] A method for preparing a blue film, the method comprising:

[0059] S1. configuring the TCO target to obtain a target set;

[0060] The configuration of TCO target is shown in the following table:

[0061] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 90% 90% 90% 90% 90% 90%

[0062] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film. The process parameters for preparing the TCO film are shown in the following table:

[0063] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0064] Comparative Example 2

[0065] A method for preparing a blue film, the method comprising:

[0066] S1. configuring the TCO target to obtain a target set;

[0067] The configuration of TCO target is shown in the following table:

[0068] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 98% 98% 98% 98% 98% 98%

[0069] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film. The process parameters for preparing the TCO film are shown in the following table:

[0070] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0071] Example 1

[0072] A method for preparing a blue film, the method comprising:

[0073] S1. configuring the TCO target to obtain a target set;

[0074] The configuration of TCO target is shown in the following table:

[0075] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 98% 98% 98% 98% 98% 78%

[0076] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film. The process parameters for preparing the TCO film are shown in the following table:

[0077] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0078] Example 2

[0079] A method for preparing a blue film, the method comprising:

[0080] S1. configuring the TCO target to obtain a target set;

[0081] The configuration of TCO target is shown in the following table:

[0082] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 98% 98% 98% 98% 98% 60%

[0083] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film. The process parameters for preparing the TCO film are shown in the following table:

[0084] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0085] Example 3

[0086] A method for preparing a blue film, the method comprising:

[0087] S1. configuring the TCO target to obtain a target set;

[0088] The configuration of TCO target is shown in the following table:

[0089] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 98% 98% 98% 98% 98% 50%

[0090] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film. The process parameters for preparing the TCO film are shown in the following table:

[0091] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0092] Example 4

[0093] A method for preparing a blue film, the method comprising:

[0094] S1. configuring the TCO target to obtain a target set;

[0095] The configuration of TCO target is shown in the following table:

[0096] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 98% 98% 98% 98% 98% 40%

[0097] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film. The process parameters for preparing the TCO film are shown in the following table:

[0098] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0099] Example 5

[0100] A method for preparing a blue film, the method comprising:

[0101] S1. configuring the TCO target to obtain a target set;

[0102] The configuration of TCO target is shown in the following table:

[0103] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 98% 98% 98% 98% 98% 20%

[0104] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film. The process parameters for preparing the TCO film are shown in the following table:

[0105] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0106] Example 6

[0107] A method for preparing a blue film, the method comprising:

[0108] S1. configuring the TCO target to obtain a target set;

[0109] The configuration of TCO target is shown in the following table:

[0110] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 98% 98% 98% 98% 50% 50%

[0111] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film. The process parameters for preparing the TCO film are shown in the following table:

[0112] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0113] Example 7

[0114] A method for preparing a blue film, the method comprising:

[0115] S1. configuring the TCO target to obtain a target set;

[0116] The configuration of TCO target is shown in the following table:

[0117] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 98% 98% 98% 50% 50% 50%

[0118] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film sheet.

[0119] The process parameters for TCO membrane preparation are shown in the following table:

[0120] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0121] Example 8

[0122] A method for preparing a blue film, the method comprising:

[0123] S1. configuring the TCO target to obtain a target set;

[0124] The configuration of TCO target is shown in the following table:

[0125] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 98% 98% 50% 50% 50% 50%

[0126] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film sheet.

[0127] The process parameters for TCO membrane preparation are shown in the following table:

[0128] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Solar substrate moving speed mm / s 27 27 27 27 27 27

[0129] Example 9

[0130] A method for preparing a blue film, the method comprising:

[0131] S1. configuring the TCO target to obtain a target set;

[0132] The configuration of TCO target is shown in the following table:

[0133] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 98% 50% 50% 50% 50% 50%

[0134] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film sheet.

[0135] The process parameters for TCO membrane preparation are shown in the following table:

[0136] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0137] Example 10

[0138] A method for preparing a blue film, the method comprising:

[0139] S1. configuring the TCO target to obtain a target set;

[0140] The configuration of TCO target is shown in the following table:

[0141] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 50% 50% 50% 50% 50% 50%

[0142] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film sheet.

[0143] The process parameters for TCO membrane preparation are shown in the following table:

[0144] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0145] Embodiment 11

[0146] A method for preparing a blue film, the method comprising:

[0147] S1. configuring the TCO target to obtain a target set;

[0148] The configuration of TCO target is shown in the following table:

[0149] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 20% 20% 20% 20% 20% 20%

[0150] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film sheet.

[0151] The process parameters for TCO membrane preparation are shown in the following table:

[0152] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0153] Example 12

[0154] A method for preparing a blue film, the method comprising:

[0155] S1. configuring the TCO target to obtain a target set;

[0156] The configuration of TCO target is shown in the following table:

[0157] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 40% 40% 40% 40% 40% 40%

[0158] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film sheet.

[0159] The process parameters for TCO membrane preparation are shown in the following table:

[0160] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0161] Example 13

[0162] A method for preparing a blue film, the method comprising:

[0163] S1. configuring the TCO target to obtain a target set;

[0164] The configuration of TCO target is shown in the following table:

[0165] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 60% 60% 60% 60% 60% 60%

[0166] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film sheet.

[0167] The process parameters for TCO membrane preparation are shown in the following table:

[0168] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0169] Embodiment 14

[0170] A method for preparing a blue film, the method comprising:

[0171] S1. configuring the TCO target to obtain a target set;

[0172] The configuration of TCO target is shown in the following table:

[0173] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 80% 80% 80% 80% 80% 80%

[0174] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film sheet.

[0175] The process parameters for TCO membrane preparation are shown in the following table:

[0176] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0177] The first batch of blue film sheets prepared in each embodiment 1-14 and comparative example 1-2 were taken as samples. The specific method of taking samples was to take 11 blue film sheets parallel to the target material direction at equal intervals at the PVD feeding place as samples, and numbered them as 1-11 samples from the operating side to the pump side. The film thickness of the samples prepared in each embodiment and comparative example was tested by using an ellipsometer. The main parameter control and test results of each embodiment and comparative example are shown in the following table:

[0178]

[0179]

[0180] As can be seen from the above table, through the data of Examples 10-14 and Comparative Examples 1-2, it can be seen that when the target consumption value is larger, the extreme difference of film thickness gradually increases, and the uniformity of film thickness becomes worse and worse, especially after the target consumption value exceeds 80%, the uniformity deteriorates particularly significantly. By replacing one TCO target in Comparative Example 2 with a TCO target with a consumption value of 80% to perform Example 1, it can be seen from Example 1 and Comparative Example 2 that when a TCO target in the standby target group has a consumption value of no more than 80%, the difference of its film thickness is improved to a certain extent. Then, through the data of Examples 1-5, it can be seen that the smaller the consumption value of the replacement TCO target, the better the improvement of the difference of film thickness and the better the improvement of the extreme difference. Through the data of Examples 5-9 and Comparative Example 2, it can be seen that the more TCO targets that meet the consumption value of no more than 50%, the better the improvement of the extreme difference of film thickness.

[0181] Embodiment 15

[0182] A method for preparing a blue film, the method comprising:

[0183] S1. configuring the TCO target to obtain a target set;

[0184] The configuration of TCO target is shown in the following table:

[0185] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 0% 0% 0% 0% 0% 50%

[0186] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film sheet.

[0187] The process parameters for TCO membrane preparation are shown in the following table:

[0188] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0189] Example 16

[0190] A method for preparing a blue film, the method comprising:

[0191] S1. configuring the TCO target to obtain a target set;

[0192] The configuration of TCO target is shown in the following table:

[0193] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 0% 0% 0% 0% 50% 50%

[0194] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film sheet.

[0195] The process parameters for TCO membrane preparation are shown in the following table:

[0196] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0197] Embodiment 17

[0198] A method for preparing a blue film, the method comprising:

[0199] S1. configuring the TCO target to obtain a target set;

[0200] The configuration of TCO target is shown in the following table:

[0201] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 0% 0% 0% 50% 50% 50%

[0202] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film sheet.

[0203] The process parameters for TCO membrane preparation are shown in the following table:

[0204] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0205] Embodiment 18

[0206] A method for preparing a blue film, the method comprising:

[0207] S1. configuring the TCO target to obtain a target set;

[0208] The configuration of TCO target is shown in the following table:

[0209] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Target consumption value 0% 0% 50% 50% 50% 50%

[0210] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film sheet.

[0211] The process parameters for TCO membrane preparation are shown in the following table:

[0212] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0213] Embodiment 19

[0214] A method for preparing a blue film, the method comprising:

[0215] S1. configuring the TCO target to obtain a target set;

[0216] The configuration of TCO target is shown in the following table:

[0217]

[0218] S2. Use the target material group to prepare the TCO film on the battery substrate to obtain a blue film sheet.

[0219] The process parameters for TCO membrane preparation are shown in the following table:

[0220] Target 1 Target 2 Target 3 Target 4 Target 5 Target 6 Power kW 6 6 6 6 6 6 Battery matrix moving speed mm / s 27 27 27 27 27 27

[0221] Set the consumption value X 设The utilization of the TCO target was set to 50%, and the utilization of the TCO target was observed. At the same time, the last batch of blue film sheets prepared in each embodiment 15-19 were taken as samples. The specific method of taking samples was to take 11 blue film sheets parallel to the target direction at equal intervals at the PVD feeding place as samples, and numbered them as 1-11 samples from the operating side to the pump side. The film thickness of the samples prepared in each embodiment and the comparative example was detected by using an ellipsometer, and the film thickness range was calculated. The results are shown in the following table:

[0222]

[0223] From the above table, we can see that the control meets the consumption value X 消 Not greater than the set consumption value X 设 The number of TCO targets accounts for half, which not only ensures the uniformity of the TCO film, but also ensures the utilization rate of the TCO targets without causing accumulation and waste of TCO targets.

[0224] The above are only specific embodiments of the present application and are not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.

Claims

1. A method for preparing a solar cell, characterized in that: The method comprises: The TCO target is configured to obtain a target set; Using the target material group to prepare a TCO film on a battery substrate to obtain a solar cell; During the TCO film preparation process, the target material group always includes at least one TCO target material whose target material consumption value is not greater than 80%; Along the extension direction of the TCO target, the cross-sectional areas of the TCO target at each location where the target consumption value is 0 are all equal; The target material group includes a plurality of TCO targets; the consumption values ​​of the plurality of TCO targets are different, wherein the extreme difference in target material consumption values ​​between the TCO targets with different consumption values ​​is not less than 20%.

2. The method for preparing a solar cell according to claim 1, characterized in that: The target material group includes a plurality of TCO targets; during the preparation process of the TCO film, the target material group always includes at least one third of the TCO targets whose target material consumption value is no more than 80%.

3. The method for preparing a solar cell according to claim 2, characterized in that: During the preparation of the TCO film, the target material group always includes at least one-half of the TCO targets whose target material consumption value is no more than 80%.

4. The method for preparing a solar cell according to claim 1, characterized in that: The extreme difference in consumption values ​​between the targets with different consumption values ​​is not less than 40%.

5. The method for preparing a solar cell according to claim 1, characterized in that: The consumption values ​​of half of the targets with different consumption values ​​are not less than 50%, and the consumption values ​​of the other half of the targets with different consumption values ​​are not more than 50%.

6. The method for preparing a solar cell according to any one of claims 1 to 5, characterized in that: During the TCO film preparation process, the target material group always includes at least one TCO target material whose target material consumption value is no more than 70%.

7. The method for preparing a solar cell according to claim 6, characterized in that: The target material group always includes at least one TCO target material whose target material consumption value is no more than 60%.

8. The method for preparing a solar cell according to claim 6, characterized in that: The target material group always includes at least one TCO target material whose target material consumption value is no more than 50%.

9. The method for preparing a solar cell according to any one of claims 1 to 5, characterized in that: The target material sputtering power for preparing the TCO film is 3-9 kW; and / or, The moving speed of the battery substrate prepared by the TCO film is 20-35 mm / s.

10. The method for preparing a solar cell according to any one of claims 1 to 5, characterized in that: The target material group includes a plurality of TCO targets; the plurality of TCO targets are arranged side by side.

11. The method for preparing a solar cell according to claim 10, characterized in that: Two ends of the plurality of TCO targets are flush.

12. The method for preparing a solar cell according to any one of claims 1 to 5, characterized in that: Along the extension direction of the TCO target, the distance between the end of the TCO target and the end of the battery substrate is 1%-10% of the length of the TCO target.

13. The method for preparing a solar cell according to claim 12, characterized in that: The distance between the end of the TCO target and the end of the battery substrate is 2%-4% of the length of the TCO target.

14. The method for preparing a solar cell according to any one of claims 1 to 5, characterized in that: The method for preparing the battery matrix comprises: Intrinsic amorphous silicon layers are deposited on two surfaces of the silicon substrate respectively; Depositing an N-type amorphous silicon layer on an intrinsic amorphous silicon layer; A P-type amorphous silicon layer is deposited on another intrinsic amorphous silicon layer.