A fully solid waste tough material for carbon fixation and plugging underground fissures and a preparation method thereof
Through the combination of the gelling component and the toughening component of the all-solid waste toughness material, the problem of easy breakage and high carbon emissions of cement-based materials underground in coal mines is solved, and long-term sealing of air leakage cracks and CO2 fixation in underground coal mines are achieved. Demonstrates high toughness and environmentally friendly properties.
Patent Information
- Application Number
- CN202310062800.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-01-20
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-01-20
AI Technical Summary
Existing cement-based leakage plugging materials are easily broken underground in coal mines and have poor deformation resistance. They cannot achieve long-term sealing. Moreover, CO2 emissions are large during the cement production process and are not environmentally friendly.
It is made of all-solid waste tough materials, including desulfurized gypsum, fly ash, calcium carbide slag, steel scraps and waste rubber particles. It is prepared through physical blending and aerosol wetting to form gelling components and toughening. components to achieve gelation reaction and CO2 fixation.
It achieves long-term sealing of air leakage cracks in coal mines and reduces carbon emissions. The material has strong toughness and high wear resistance. It is suitable for industrial production, avoids high temperature and high pressure conditions, and has green and environmental protection characteristics.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of plugging materials, and in particular to a full-solid waste tough material for carbon fixation and plugging underground cracks and a preparation method thereof. Background Art
[0002] In order to increase the recovery rate of coal resources, my country's mines have implemented a narrow coal pillar and goaf-side excavation layout. Affected by mining disturbance, the original equilibrium state of the coal pillars and closed walls in the goaf of coal mines underground is destroyed, causing deformation, spalling and even collapse. Cracks develop inside the coal rock mass to form air leakage channels, which provide oxygen supply conditions for coal spontaneous combustion and increase the risk of coal spontaneous combustion.
[0003] To solve this problem, underground coal mines usually use cement-based plugging materials to seal air leakage cracks, so as to reduce air leakage and prevent coal spontaneous combustion. When using cement-based plugging materials to seal underground cracks, on the one hand, a large amount of cement will be consumed, resulting in a high cost of plugging cracks; on the other hand, cement-based plugging materials are brittle and have poor deformation resistance, which leads to the easy generation of new cracks and the formation of secondary air leakage channels under the action of mine pressure, and cannot meet the needs of long-term plugging of cracks in coal mines.
[0004] CN103396075A, CN106986597A, and CN113248228A respectively disclose the formula and preparation method of underground air leakage plugging materials, which reduce the cement dosage of the materials by adding fly ash, bentonite, gypsum and other materials to the cement system. However, the materials involved in the above patents still use cement as the main raw material, which cannot solve the problem that cement-based materials are easy to break and crack after being compressed, cannot eliminate the interference of external forces such as mine pressure, and cannot achieve long-term plugging of underground air leakage cracks. In addition, due to the large amount of CO2 emissions and environmental pollution during the production process of raw materials such as cement, and the inclusion of organic substances such as fatty alcohol polyoxyethylene ether and cellulose in the material formula, it is easy to thermally decompose and release toxic and harmful substances in the high temperature and high humidity environment of coal mines. Summary of the invention
[0005] The purpose of the present invention is to provide an all-solid waste tough material for fixing carbon and sealing underground cracks. The raw materials of this material are mainly solid waste, with low cost, and no high-carbon emission raw materials such as cement are used. It has the advantages of being green and environmentally friendly, strong toughness, and durable in sealing cracks, and can permanently fix and seal CO2. It can achieve long-term sealing of air leakage cracks in coal mines, and ultimately achieve efficient and lasting prevention and control of spontaneous combustion of coal in mines.
[0006] Another object of the present invention is to provide a method for preparing the above-mentioned all-solid waste tough material for carbon fixation and sealing underground cracks. The entire preparation process does not add any harmful substances such as strong acids and strong alkalis, nor does it use harsh environmental conditions such as high temperature and high pressure, and is suitable for industrial production.
[0007] To achieve the above purpose, the technical solution adopted by the present invention is as follows:
[0008] On the one hand, the present invention provides an all-solid waste tough material for carbon fixation and plugging underground fissures, which is made of the following raw materials in weight percentage: 47-65% of a gelling component, 3-10% of a toughening component, and the rest is water; the gelling component is prepared by physically blending desulfurized gypsum, fly ash, carbide slag, and steel scrap waste in a weight ratio of 60-68:20-25:5-10:2-5; the toughening component is prepared by physically blending waste rubber particles, steel slag, coal gangue powder, and water in a weight ratio of 10-12, 4-5, 1-2, and 1-3.
[0009] Preferably, the preparation process of the gelling component is as follows:
[0010] 1.1) Weigh desulfurized gypsum, fly ash and carbide slag respectively according to the proportion, mix them evenly with ball mill to obtain mixed gelled powder;
[0011] 1.2) Add steel scrap waste into the mixed gelled powder according to proportion, mix evenly using a three-dimensional mixer to obtain a gelled component.
[0012] Preferably, the preparation process of the toughening component is as follows:
[0013] 2.1) Weigh waste rubber particles and water in proportion, atomize the water to fully wet the waste rubber particles, and obtain wet rubber particles;
[0014] 2.2) Weigh steel slag and coal gangue powder according to the proportion, add them to the above-mentioned wet rubber particles, mix them in a three-dimensional mixer at room temperature, make the steel slag and coal gangue powder fully adhere to the wet rubber particles, and let them stand for 24 hours to obtain the hydrated toughening component;
[0015] 2.3) freeze-drying the hydrated toughening component to obtain a dry toughening component block;
[0016] 2.4) The toughening component block is ball-milled to a particle size of less than 4 mm to finally obtain the toughening component.
[0017] Preferably, the particle size of the desulfurized gypsum in the gelling component is 100-250 meshes, the fly ash is secondary fly ash, the particle size of the carbide slag is 100-200 meshes, and the particle size of the steel scrap waste is 1-3 mm.
[0018] Preferably, the particle size of the waste rubber particles in the toughening component is 1-3 mm, and the particle sizes of the steel slag and coal gangue powder are both 100-200 meshes.
[0019] Preferably, the ball milling speed in step 1.1) is 200-250 r / min, and the ball milling time is 10-20 min; the speed of the three-dimensional mixer in step 1.2) is 5-10 r / min, and the mixing time is 20-40 min.
[0020] Preferably, the rotation speed of the three-dimensional mixer in step 2.2) is 5-10 r / min, and the mixing time is 20-40 min; the rotation speed of the ball mill in step 2.4) is 200-250 r / min, and the ball milling time is 10-20 min.
[0021] Preferably, the freeze-drying temperature in step 2.3) is -80~-50°C, the vacuum degree is 2~5Pa, and the time is more than 120h.
[0022] On the other hand, the present invention also provides a method for preparing the above-mentioned all-solid waste tough material for carbon fixation and plugging underground fissures, the specific steps of which are:
[0023] 1) Add the gelling components into water in proportion and stir for 1-3 minutes at room temperature to obtain a uniform gelling slurry;
[0024] 2) Add the toughening component to the above-mentioned gel slurry in proportion, stir for 3-5 minutes at room temperature to obtain a composite slurry;
[0025] 3) CO2 gas is continuously introduced into the above-mentioned composite slurry through a pipeline, and after stirring and reacting for 2 to 5 minutes at room temperature and pressure, a fully solid waste tough material for carbon fixation and plugging underground fractures is obtained.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] 1. The present invention uses desulfurized gypsum, fly ash, carbide slag, and steel scrap waste as the main raw materials of the cementitious component, and waste rubber particles, steel slag, and coal gangue powder as the main raw materials of the toughening component. No cement is used at all during the preparation and use of the materials, thereby achieving full solid waste material sealing of underground fissures. This new all-solid waste tough material is green, environmentally friendly, and low-cost, and effectively reduces the problems of high carbon emissions and high crack sealing costs caused by the use of cement.
[0028] 2. The present invention uses desulfurized gypsum, fly ash, carbide slag, etc. as the gelling components of the all-solid waste tough plugging material. Fly ash itself has no gelling properties, but its activity is "potential". When gypsum and carbide slag are added to the slurry, the concentration of calcium hydroxide and calcium carbonate in the slurry increases, the pH value of the slurry rises, and the alkaline environment accelerates the dissolution rate of silicate ions and aluminates in the fly ash glass, thereby accelerating the formation of hydrated calcium silicate (CSH gel). At the same time, the presence of desulfurized gypsum also has a certain stimulating effect on the hydration activity of fly ash, effectively promoting the hydration of fly ash; and the desulfurized gypsum generates needle-shaped calcium sulfonate crystals in the gelling reaction of the system, which interweave and intersperse with the CSH gel to finally form a dense network structure. Desulfurized gypsum, fly ash, and carbide slag synergistically hydrate and condense in the mixed system, which ultimately promotes the condensation and solidification of the slurry and has a good effect in plugging air leakage.
[0029] 3. The present invention adds steel scrap waste to prepare plugging materials. On the one hand, it can improve the stability of the plugging material in a flowing state, enhance the homogeneity of the slurry when it seeps in the cracks, and is conducive to the complete filling and effective plugging of complex cracks underground; on the other hand, the addition of steel scrap waste improves the anti-segregation ability, deformation ability, wear resistance, scratch resistance, and impact energy absorption of the all-solid waste tough plugging material, and enhances the toughness of the plugging material and its ability to resist external forces such as mine pressure. In addition, compared with traditional cement-based plugging materials, the use of steel scrap waste improves the thermal conductivity of the all-solid waste tough plugging material, and its thermal conductivity is also significantly higher than that of underground coal and rock tunnel walls, etc., so that the all-solid waste tough plugging material can effectively respond to high-temperature abnormal points inside the crack plugging areas such as goafs and high-risk areas. Therefore, after using the plugging material proposed in the present invention to plug the air leakage cracks of the underground isolation coal pillar, the location of the high-temperature points in dangerous areas such as goafs can be effectively predicted based on the temperature difference between the crack plugging area and the ordinary coal rock area, which helps to take measures such as inerting and cooling to quickly and effectively eliminate the high-temperature points. At the same time, due to the high temperature and high humidity environment in the coal mine, the steel scraps and waste materials in the plugging material can react with the oxygen in the cracks, thereby achieving the effect of deoxygenation, and further improving the purpose of plugging the cracks and isolating oxygen by the plugging material.
[0030] 4. The present invention uses waste rubber particles with good elasticity as the main toughening component. At the same time, in order to eliminate the problems of oxidation and release of harmful gases by heat during the use of waste rubber particles, the waste rubber particles are treated by atomization wetting and three-way mixer mixing. Steel slag and coal gangue powder are used to treat the waste rubber particles. Since steel slag itself has certain self-gelling properties, after 24 hours of hydration, a layer of wrapping shell with steel slag and coal gangue powder as the main components and a thickness of about 0.5 mm can be formed on the surface of the waste rubber particles, which can not only achieve the wrapping and oxygen isolation of the waste rubber particles, but also does not lose the elasticity of the waste rubber particles. Moreover, the coal gangue in the wrapping shell can also undergo a low-temperature oxidation reaction with the oxygen in the crack leakage airflow, thereby achieving the effect of eliminating oxygen in the cracks and isolating and sealing. After the waste rubber particles treated with steel slag and coal gangue are added to the all-solid waste tough plugging material, when sealing the air leakage cracks in the coal mine, the waste rubber particles can be used to effectively reduce the interference of external forces such as underground blasting, mine earthquakes, and mine pressure, which is beneficial to eliminate the problem of cracking of the plugging material and secondary air leakage in the cracks, thereby effectively solving the problem of high brittleness and poor deformation resistance of cement-based plugging materials.
[0031] 5. The whole preparation process of the all-solid waste tough material for carbon fixation and sealing underground cracks proposed in the present invention does not have any stringent requirements for experimental environments such as high temperature and high pressure, and does not harm the bodies of underground workers, especially avoiding damage to the underground environment, strata and groundwater of coal mines, and is green and environmentally friendly. During the preparation process of the all-solid waste tough material, the adsorption and storage of CO2 greenhouse gas can be achieved, and fine carbonate precipitates such as calcium carbonate and magnesium carbonate can be produced in the slurry, which enhances the accumulation of the all-solid waste tough material in the complex air leakage cracks in underground coal mines, which is beneficial to the long-term filling and sealing of the cracks, and the application prospect is very broad. Implementation
[0032] The present invention is further described in detail below with reference to specific embodiments.
[0033] The gelling component used in the following examples is prepared according to the following steps: (1) Desulfurized gypsum (particle size of 100-250 mesh), fly ash (secondary fly ash), carbide slag (particle size of 100-200 mesh), and steel scrap waste (particle size of 1-3 mm) are weighed in a weight ratio of 60-68:20-25:5-10:2-5, and the desulfurized gypsum, fly ash, and carbide slag are ball-milled and mixed for 10-20 minutes until they are uniformly mixed. The ball milling speed is 200-250 r / min to obtain a mixed gelling powder; (2) The steel scrap waste is added to the above-mentioned mixed gelling powder, and mixed uniformly using a three-dimensional mixer. The speed is 5-10 r / min and the mixing time is 20-40 min to prepare a gelling component.
[0034] The toughening component used in the following examples is prepared according to the following steps: (1) waste rubber particles (particle size of 1-3 mm), steel slag (particle size of 100-200 mesh), coal gangue powder (particle size of 100-200 mesh), and water are weighed in a weight ratio of 50-60, 20-25, 5-10, and 5-15, respectively, and the water is atomized to fully wet the waste rubber particles to obtain wet rubber particles; (2) the weighed steel slag and coal gangue powder are added to the wet rubber particles, and mixed using a three-dimensional mixer at room temperature, with a rotation speed of 5-10 r / min and a mixing time of 20 (3) the hydrated toughening component is placed in a freeze drying oven for freeze drying at a temperature of -80 to -50 °C, a vacuum degree of 2 to 5 Pa, and a time of more than 120 h to obtain a dry toughening component block; (4) the dry toughening component block is ball milled to a particle size of less than 4 mm, the speed of the ball mill is 200 to 250 r / min, and the ball milling time is 10 to 20 min to finally obtain the toughening component. Example 1
[0035] A fully solid waste tough material for carbon fixation and plugging underground fissures is made of the following raw materials in percentage by weight: 47% of a gelling component, 3% of a toughening component, and the remainder being water.
[0036] The preparation method of the all-solid waste tough material for carbon fixation and plugging underground fissures in this embodiment comprises the following specific steps:
[0037] First, the gelling components are added to water in proportion, and stirred at room temperature for 1 to 3 minutes to obtain a uniform gelling slurry; then, the toughening components are added to the above-mentioned gelling slurry in proportion, and stirred at room temperature for 3 to 5 minutes to obtain a composite slurry; finally, CO2 gas is continuously introduced into the above-mentioned composite slurry through a pipeline, and after stirring and reacting at room temperature and pressure for 2 to 5 minutes, an all-solid waste tough material for carbon fixation and plugging underground cracks is prepared. Example 2
[0038] A fully solid waste tough material for carbon fixation and plugging underground fissures is made of the following raw materials in percentage by weight: 47% of a gelling component, 5% of a toughening component, and the remainder being water.
[0039] The preparation method of the all-solid waste tough material used for carbon fixation and plugging underground fissures in this embodiment is the same as that in Example 1. Example 3
[0040] A fully solid waste tough material for carbon fixation and plugging underground fissures is made of the following raw materials in percentage by weight: 47% of a gelling component, 10% of a toughening component, and the remainder being water.
[0041] The preparation method of the all-solid waste tough material used for carbon fixation and plugging underground fissures in this embodiment is the same as that in Example 1. Example 4
[0042] A fully solid waste tough material for carbon fixation and plugging underground fissures is made of the following raw materials in percentage by weight: 55% of a gelling component, 3% of a toughening component, and the remainder being water.
[0043] The preparation method of the all-solid waste tough material used for carbon fixation and plugging underground fissures in this embodiment is the same as that in Example 1. Example 5
[0044] A fully solid waste tough material for carbon fixation and plugging underground fissures is made of the following raw materials in percentage by weight: 55% of a gelling component, 5% of a toughening component, and the remainder being water.
[0045] The preparation method of the all-solid waste tough material used for carbon fixation and plugging underground fissures in this embodiment is the same as that in Example 1. Example 6
[0046] A fully solid waste tough material for carbon fixation and plugging underground fissures is made of the following raw materials in percentage by weight: 55% of a gelling component, 10% of a toughening component, and the remainder being water.
[0047] The preparation method of the all-solid waste tough material used for carbon fixation and plugging underground fissures in this embodiment is the same as that in Example 1. Example 7
[0048] A fully solid waste tough material for carbon fixation and plugging underground fissures is made of the following raw materials in percentage by weight: 65% of a gelling component, 3% of a toughening component, and the remainder being water.
[0049] The preparation method of the all-solid waste tough material used for carbon fixation and plugging underground fissures in this embodiment is the same as that in Example 1. Example 8
[0050] A fully solid waste tough material for carbon fixation and plugging underground fissures is made of the following raw materials in percentage by weight: 65% of a gelling component, 5% of a toughening component, and the remainder being water.
[0051] The preparation method of the all-solid waste tough material used for carbon fixation and plugging underground fissures in this embodiment is the same as that in Example 1. Example 9
[0052] A fully solid waste tough material for carbon fixation and plugging underground fissures is made of the following raw materials in percentage by weight: 65% of a gelling component, 10% of a toughening component, and the remainder being water.
[0053] The preparation method of the all-solid waste tough material used for carbon fixation and plugging underground fissures in this embodiment is the same as that in Example 1.
[0054] The all-solid waste tough material for carbon fixation and plugging underground cracks prepared in the above Examples 1 to 9 was used to obtain the initial setting time of the all-solid waste tough material according to the water consumption, setting time and stability test method of cement standard consistency GB / T 1346-2011; the toughness coefficient (also called flexural-compression ratio, i.e. the ratio of the flexural strength to the compressive strength of the material) was used to reflect the toughness of the all-solid waste tough material. If the toughness coefficient of the material is larger, it indicates that its deformation resistance is better, the influence of external forces such as mine pressure is smaller, and the plugging effect of underground cracks is better. Otherwise, it indicates that the toughness of the material is worse.
[0055] Table 1 Performance parameters of all-solid waste toughness materials with different raw material ratios
[0056]
[0057] As can be seen from Table 1, the all-solid waste toughness material for carbon fixation and plugging underground fissures of the present invention can achieve controllable adjustment of the initial setting time of 8 to 40 minutes of all-solid waste toughness by changing the weight ratio of the raw materials; through the synergistic hydration and coagulation of the three desulfurized gypsum, fly ash, and carbide slag in the cementitious components in the mixed system, the coagulation and solidification of the slurry without the addition of cement is achieved, and the 24h compressive strength reaches more than 1.88Mpa, which meets the requirement of 0.5Mpa minimum compressive strength of the material for plugging underground fissures in coal mines. No cement is added at all during the preparation and use of the all-solid waste toughness material, and the plugging of underground fissures with all-solid waste materials is achieved. It is green, environmentally friendly, and low-cost, and effectively reduces the problems of high carbon emissions and high fissure plugging costs caused by the use of cement. Compared with the toughness coefficient of ordinary Portland cement of about 0.11, the toughness coefficient of the all-solid waste tough material of the present invention is increased by more than 40%, which significantly enhances the toughness and anti-destruction performance of the plugging material, is beneficial to resisting the damage to the plugging material by external forces such as mine earthquakes and mine pressure, and reduces the occurrence of problems such as cracking of plugging materials and secondary air leakage in cracks.
[0058] The present invention utilizes steel scrap waste to prepare plugging materials, thereby improving the thermal conductivity of the all-solid waste tough plugging materials, so that the plugging materials can effectively respond to high-temperature abnormal points inside crack plugging areas such as goaf areas and high-risk areas, and effectively predict the positions of high-temperature points in dangerous areas such as goaf areas, which helps to take inerting, cooling and other measures to quickly and effectively eliminate high-temperature points; and steel scrap waste and the like can react with oxygen in the cracks, thereby achieving a deoxygenation effect, thereby achieving the purpose of further improving the plugging materials to plug cracks and isolate oxygen.
[0059] The present invention utilizes waste rubber particles with good elasticity as the main toughening component, and utilizes solid wastes with gelling properties such as steel slag and coal gangue powder to wrap the waste rubber particles, thereby eliminating the problems of oxidation of the waste rubber particles and release of harmful gases when heated during use; the toughening components can effectively eliminate the moisture contained in the waste rubber particles, steel slag and coal gangue through processes such as freeze drying, thereby avoiding oxidation of the waste rubber particles caused by processes such as high-temperature drying, thereby preventing aging, brittleness and even cracking.
[0060] The all-solid waste tough material can enhance the toughness of the plugging material by taking advantage of the anti-impact, buffering, energy absorption and rebound properties of waste rubber particles, thereby solving the problem of cement-based plugging materials being brittle and poor in deformation resistance. At the same time, when preparing the all-solid waste tough material, by absorbing CO2 greenhouse gas, a chemical reaction occurs in the slurry to generate fine calcium carbonate, magnesium carbonate and other precipitates, which enhances its accumulation in complex air leakage cracks in coal mines, and is conducive to the efficient plugging of air leakage cracks.
[0061] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Any modifications, equivalent substitutions and improvements made by any technician familiar with the technical field within the technical scope disclosed by the present invention and within the spirit and principle of the present invention should be covered by the protection scope of the present invention.
Claims
1. A fully solid waste tough material for carbon fixation and plugging underground fissures, characterized in that: The invention is prepared from the following raw materials in weight percentage: 47-65% of a gelling component, 3-10% of a toughening component, and the rest being water; the gelling component is prepared by physically blending desulfurized gypsum, fly ash, carbide slag, and steel scrap waste in a weight ratio of 60-68:20-25:5-10:2-5; the toughening component is prepared by aerosol wetting, physical dry mixing, static hydration, and freeze drying of waste rubber particles, steel slag, coal gangue powder, and water in a weight ratio of 10-12, 4-5, 1-2, and 1-3. The specific preparation process is as follows: 2.1) Weigh waste rubber particles and water in proportion, atomize the water to fully wet the waste rubber particles, and obtain wet rubber particles; 2.2) Weigh steel slag and coal gangue powder according to the proportion, add them to the above-mentioned wet rubber particles, mix them in a three-dimensional mixer at room temperature, make the steel slag and coal gangue powder fully adhere to the wet rubber particles, and let them stand for 24 hours to obtain the hydrated toughening component; 2.3) freeze-drying the hydrated toughening component to obtain a dry toughening component block; 2.4) The toughening component block is ball-milled to a particle size of less than 4 mm to finally obtain the toughening component.
2. The all-solid waste tough material for carbon fixation and plugging underground fissures according to claim 1, characterized in that: The preparation process of the gelling component is as follows: 1.1) Weigh desulfurized gypsum, fly ash and carbide slag respectively according to the proportion, mix them evenly with ball mill to obtain mixed gelled powder; 1.2) Add steel scrap waste into the above mixed gelled powder in proportion, mix evenly using a three-dimensional mixer to obtain a gelled component.
3. The all-solid waste tough material for carbon fixation and plugging underground fissures according to claim 1 or 2, characterized in that: The particle size of the desulfurized gypsum in the gelling component is 100-250 meshes, the fly ash is secondary fly ash, the particle size of the calcium carbide slag is 100-200 meshes, and the particle size of the steel scrap waste is 1-3 mm.
4. The all-solid waste tough material for carbon fixation and plugging underground fissures according to claim 1, characterized in that: The particle size of the waste rubber particles in the toughening component is 1-3 mm, and the particle sizes of the steel slag and coal gangue powder are both 100-200 meshes.
5. The all-solid waste tough material for carbon fixation and plugging underground fissures according to claim 2, characterized in that: The ball milling speed in step 1.1) is 200-250 r / min, and the ball milling time is 10-20 min; the three-dimensional mixer speed in step 1.2) is 5-10 r / min, and the mixing time is 20-40 min.
6. The all-solid waste tough material for carbon fixation and plugging underground fissures according to claim 1, characterized in that: The rotation speed of the three-dimensional mixer in step 2.2) is 5-10 r / min, and the mixing time is 20-40 min; the rotation speed of the ball mill in step 2.4) is 200-250 r / min, and the ball milling time is 10-20 min.
7. The all-solid waste tough material for carbon fixation and plugging underground fissures according to claim 1, characterized in that: The freeze-drying temperature in step 2.3) is -80~-50°C, the vacuum degree is 2~5Pa, and the time is more than 120h.
8. The method for preparing the all-solid waste tough material for carbon fixation and plugging underground fissures according to any one of claims 1 to 7, characterized in that: The specific steps are: 1) Add the gelling components into water in proportion and stir for 1-3 minutes at room temperature to obtain a uniform gelling slurry; 2) Add the toughening component to the above-mentioned gel slurry in proportion, stir for 3-5 minutes at room temperature to obtain a composite slurry; 3) CO2 gas is continuously introduced into the above-mentioned composite slurry through a pipeline, and after stirring and reacting for 2 to 5 minutes at room temperature and pressure, a fully solid waste tough material for carbon fixation and plugging underground fractures is obtained.
Citation Information
Patent Citations
Flame-retardant paste material for coal mine downhole air leakage blocking and preparation method thereof
CN103396075A
Inhibiting slurry material for blocking air leakage in underground coal mine and preparation method of inhibiting slurry material
CN106986597A
A Cementitious Material, A Concrete Prepared And Its Preparation Method
AU2020101154A4
Rubber-caustic dross-mineral waste residue composite cementing material concrete
CN108726965A
Coal mine mined-out area filling paste prepared from classified materials of waste automobile tires and preparation method thereof