A polybutylene terephthalate modified material and its preparation method and application

By adding glass fiber, carbon black and clay to polybutylene terephthalate material, and using the high-temperature sintering effect of laser additives and clay, the problem of marking clarity and fastness in laser marking technology is solved. Achieve efficient laser marking effect.

CN116333463BActive Publication Date: 2024-12-03JIANGSU KINGFA SCI & TECH ADVANCED MATERIALS CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202310481793.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-04-28
Publication Date
2024-12-03
Estimated Expiration
2043-04-28

AI Technical Summary

Technical Problem

In the existing laser marking technology, although the black and white marking effect is clear, due to the fragility of micro foaming, the marking fonts are prone to fall off, resulting in insufficient fastness and making it difficult to maintain long-term durability in practical applications.

Method used

Glass fiber, carbon black and clay are added to the polybutylene terephthalate material, and the clarity and fastness of the mark are improved through the absorption of laser additives and the high-temperature sintering of the clay.

Benefits of technology

It achieves the double improvement of the clarity and fastness of laser marking black and white marking, and the marking is more durable and is suitable for other dark-colored materials with dark background and white marking, with a wide range of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004207429480000051
    Figure BDA0004207429480000051
  • Figure BDA0004207429480000061
    Figure BDA0004207429480000061
Patent Text Reader

Abstract

The invention relates to the technical field of polymer engineering plastic modification, and specifically discloses a polybutylene terephthalate modified material, a preparation method and an application thereof. The polybutylene terephthalate modified material comprises the following components in parts by weight: 40 to 85 parts of PBT resin, 20 to 50 parts of glass fiber, 0.1 to 1 part of carbon black, 0.3 to 2 parts of laser auxiliary agent and 0.5 to 5 parts of clay. The polybutylene terephthalate modified material can achieve the dual effects of high clarity of black and white laser marking and high fastness of marking characters, and the method for realizing the modified material is simple, low in cost and high in laser marking efficiency; wherein a clay component is added and sintered at a high temperature to stabilize and enhance the microbubbles of the marking characters, thereby improving the fastness of laser marking. The polybutylene terephthalate modified material prepared by the invention can be applied to other dark-colored materials with white characters on a dark background, and has a wide range of applications.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer engineering plastic modification, in particular to a polybutylene terephthalate modified material and a preparation method and application thereof. Background Art

[0002] With the improvement of environmental protection requirements and production efficiency, traditional printing methods such as mimeograph and silk screen are being further replaced by laser marking. Laser marking technology has the advantages of high efficiency, low cost, low pollution and wide application range. The application of laser marking is mainly divided into light background color on dark text and dark background color on white text. In recent years, it has also been used to mark colored text. The more mature laser marking is mainly based on light background color on black text and dark background color on white text. The former is referred to as white on black and the latter is referred to as black on white. The mechanism of white on black is that the surface of the material absorbs laser energy, degrades and carbonizes, and then turns into black text. For black on white, the material decomposes under heat to produce gas, and micro-bubbles occur on the surface of the material, and the diffuse reflection of light creates a visual white text effect.

[0003] Regarding the black-on-white technology, patent CN103467956A discloses a laser-markable polycarbonate composite and its preparation method, which adds a laser marking additive with a silicon-oxygen bond and a benzene ring to achieve a laser marking effect. Patent CN112266500B provides a laser marking powder, which is a PAN-based carbon fiber powder with an oxazole group. When used in PC resin, it can not only reduce the light-to-heat conversion efficiency, but also absorb light energy in some bands and reflect blue light to obtain a clearer black-on-white effect.

[0004] At present, there are few black-on-white laser marking technologies. The existing technologies mainly focus on solving the problem of whether the marking can be done. Some patents mention improving the clarity of the marking, but there is no public and effective technology to explore the problem of improving the fastness of the marking. The black-on-white marking effect comes from the micro-bubbles on the surface of the material. These micro-bubbles are relatively fragile and easily fall off when scratched by external forces, resulting in a significant decrease in the marking effect. In practical applications, both clear marking and durable marking are essential. Therefore, it is very necessary to develop a material that can mark clearly and has high marking fastness. Summary of the invention

[0005] The purpose of the present invention is to overcome the shortcomings of the above-mentioned prior art and provide a polybutylene terephthalate modified material and a preparation method and application. The polybutylene terephthalate modified material of the present application solves the technical problems of the clarity and fastness of the marking of black and white laser marking.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] The first object of the present invention is to provide a polybutylene terephthalate modified material, comprising the following components in parts by weight:

[0008] 40-85 parts of PBT resin, 20-50 parts of glass fiber, 0.1-1 parts of carbon black, 0.3-2 parts of laser auxiliary agent and 0.5-5 parts of clay.

[0009] The polybutylene terephthalate modified material prepared by the invention is suitable for black and white laser marking by adding glass fiber, carbon black, laser auxiliary agent and clay into PBT resin, and has high laser marking clarity and marking fastness.

[0010] Among them, the added laser additive can homogenize the absorption of light by the polybutylene terephthalate modified material, making the boundary of the marking clearer. Adding an appropriate amount of carbon black can promote the absorption of laser by the polybutylene terephthalate modified material and improve the foaming degree of the polybutylene terephthalate modified material. Compounding the laser additive and carbon black can better improve the clarity of laser marking.

[0011] In addition, clay is added during the preparation of the polybutylene terephthalate modified material. During laser marking, the position burned by the laser beam instantly reaches high temperature, and the clay component is sintered at high temperature to stabilize and enhance the microbubbles of the marking characters, thereby improving the laser marking fastness.

[0012] As a preferred embodiment of the polybutylene terephthalate modified material of the present invention, the weight portion of the carbon black is 0.2 to 0.6 parts, and the weight portion of the clay is 1 to 3 parts.

[0013] The invention optimizes the weight proportions of carbon black and clay, and the prepared polybutylene terephthalate modified material has a higher laser marking clarity for white characters on a black background, and the marking fastness is significantly improved, and the material is durable, achieving a dual effect. The prepared polybutylene terephthalate modified material is applied to other dark-colored materials for white characters on a dark background, and has a wide range of applications.

[0014] As a preferred embodiment of the polybutylene terephthalate modified material of the present invention, the clay is at least one of kaolinite clay, sepiolite clay, montmorillonite clay, and bentonite clay, and preferably, the clay is sepiolite clay. The above clays are preferred because they have high temperature sintering characteristics and do not react with the modified material components to cause excessive performance attenuation.

[0015] When the clay is selected from at least one of kaolinite clay, sepiolite clay, montmorillonite clay and bentonite clay, the microbubbles of the marking characters can be better stabilized and enhanced, thereby improving the laser marking fastness and durability.

[0016] As a preferred embodiment of the polybutylene terephthalate modified material of the present invention, the specific surface area of ​​the clay is ≥90m 2 / g, preferably, the specific surface area of ​​the clay is > 100m 2 / g. The test method for the specific surface area of ​​clay refers to GB / T 19587-2004 "Determination of the specific surface area of ​​solid substances by gas adsorption BET method".

[0017] When the specific surface area of ​​clay is greater than 100m 2 / g, the clay component is sintered at high temperature, which can better stabilize and enhance the microbubbles of the marking characters, thereby improving the laser marking fastness. The specific surface area of ​​the clay can be 110, 120, 150, 160, 180, etc., and the specific surface area of ​​the clay selected in the present invention is not limited thereto.

[0018] Preferably, the specific surface area of ​​the clay is 210 to 230 m 2 / g.

[0019] When the specific surface area of ​​clay is 210~230m 2 / g, the microbubbles of the logo are better stabilized and enhanced, thereby improving the laser marking fastness. When the specific surface area is too large, it is easy to cause difficulty in dispersing the clay, resulting in significant deterioration of the performance of the modified material, and it is also not smooth during extrusion feeding.

[0020] Preferably, the carbon black is an inorganic carbon black used as a pigment.

[0021] As a preferred embodiment of the polybutylene terephthalate modified material of the present invention, the glass fiber is an alkali-free glass fiber, and the average diameter of the glass fiber is 7 to 13 μm.

[0022] The use of the alkali-free glass fiber with the above diameter can improve the mechanical properties of the prepared polybutylene terephthalate modified material, and the tensile strength thereof is relatively high.

[0023] As a preferred embodiment of the polybutylene terephthalate modified material of the present invention, the laser auxiliary agent includes a basic copper phosphonate laser auxiliary agent, a laser auxiliary agent of a mixture of titanium oxide and pigment, or a tin antimony compound laser auxiliary agent. Preferably, the laser auxiliary agent is at least one of Iriotec 8800 series laser auxiliary agent, Iriotec 8200 series laser auxiliary agent, and FABULASE series laser auxiliary agent.

[0024] Adding the above-mentioned laser additives can homogenize the light absorption of the polybutylene terephthalate modified material, making the boundary of the marking characters clearer; compounding the above-mentioned laser additives with carbon black can better improve the clarity of laser marking.

[0025] As a preferred embodiment of the polybutylene terephthalate modified material of the present invention, the polybutylene terephthalate modified material further comprises 0 to 2 parts of a processing aid, wherein the processing aid is at least one of an antioxidant, a lubricant, a weathering aid, a coupling agent, an antibacterial agent, an anti-dripping agent, an ester exchange inhibitor and a colorant. Preferably, the processing aid is an antioxidant and a lubricant.

[0026] The second object of the present invention is to provide a method for preparing the above-mentioned polybutylene terephthalate modified material, comprising the following steps:

[0027] According to the proportion, PBT resin, glass fiber, carbon black, laser auxiliary agent, clay and processing auxiliary agent are added into an extruder, melt-extruded at 180° C. to 260° C., cooled and granulated to obtain the polybutylene terephthalate modified material.

[0028] The third purpose of the present invention is to provide the application of the above-mentioned polybutylene terephthalate modified material in automobile products such as controller housings and sensor housings, and electronic appliances such as miniature circuit breakers and connectors.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] The present invention provides a polybutylene terephthalate modified material, a preparation method and an application thereof. The polybutylene terephthalate modified material can achieve the dual effects of high clarity of black and white laser marking and high fastness of marking characters, and the method that can be achieved by the polybutylene terephthalate modified material is simple, low cost and high laser marking efficiency; wherein a clay component is added and sintered at a high temperature to stabilize and enhance the microbubbles of the marking characters, thereby improving the fastness of laser marking. The polybutylene terephthalate modified material prepared by the present invention can be applied to other dark-colored materials with white characters on a dark background, and has a wide range of applications. DETAILED DESCRIPTION

[0031] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments.

[0032] In the following examples and comparative examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.

[0033] The sources of raw materials used in the following examples and comparative examples are as follows:

[0034] PBT resin, model PBT GX121, relative density 1.31, intrinsic viscosity 1.00 dl / g, purchased from Yizheng Branch of Sinopec Asset Management Co., Ltd.; PBT resin intrinsic viscosity test method is based on GB / T 14190-2017;

[0035] Glass fiber, alkali-free chopped, average diameter 11 μm, model ECS11-4.5-534A, purchased from China Jushi Co., Ltd.;

[0036] Carbon black, model M717, inorganic carbon black, purchased from Cabot Corporation;

[0037] Clay 1, model Clay 80T, is sepiolite clay with a specific surface area of ​​210m 2 / g, purchased from Shanghai Zhuangjing Chemical Co., Ltd.;

[0038] Clay 2, model Clay 20, is a sepiolite clay with a specific surface area of ​​230m 2 / g, purchased from Shanghai Zhuangjing Chemical Co., Ltd.;

[0039] Clay 3, model CMP-1, is kaolinite clay with a specific surface area of ​​255m 2 / g, purchased from China Kaolin Co., Ltd.;

[0040] Clay 4, type kaolin, is kaolinite clay, with a specific surface area of ​​90m 2 / g, 600 mesh, the main component of the product is Al2O3 / SiO2=45 / 52, CAS number is 1332-58-7, purchased from Baiyi Mineral Products Processing Plant in Lingshou County;

[0041] Clay 5, type bentonite, is an organic bentonite clay with a specific surface area of ​​195m 2 / g, 1000 mesh, the main component of the product is Al2O3 / SiO2=57 / 19, CAS No. is 1302-78-9, purchased from Inner Mongolia Ningcheng Tianyu Chemical Co., Ltd.;

[0042] Laser auxiliary agent 1, model FABULASE 330, basic copper phosphonate, purchased from Budenheim Company;

[0043] Laser auxiliary agent 2, model Iriotec 8850, mainly a mixture of titanium oxide and pigment, purchased from Merck;

[0044] Antioxidant, pentaerythritol tetrakis[β(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, commercially available;

[0045] Lubricant, pentaerythritol fatty acid ester, commercially available.

[0046] In the following examples and comparative examples, the PBT resin, glass fiber, antioxidant and lubricant used in parallel experiments were the same.

[0047] The components (in parts by weight) of the polybutylene terephthalate modified materials of Examples 1-16 and Comparative Examples 1-4 are shown in Table 1.

[0048] The preparation method of the polybutylene terephthalate modified material is:

[0049] According to the ratio, PBT resin, carbon black, laser auxiliary agent, clay and processing auxiliary agent are added to a premixer and mixed for 1-2 minutes to obtain a premix, and then the premix is ​​added to the main feeding port of a twin-screw extruder, and glass fiber is added at the side feeding port of the fifth zone of the twin-screw extruder, wherein the temperature of the first zone of the twin-screw extruder is 30-200°C, the temperature of the second zone is 220-260°C, the temperature of the third zone is 210-250°C, the temperature of the fourth zone is 200-240°C, the temperature of the fifth zone is 180-240°C, the temperature of the sixth zone is 180-240°C, the temperature of the seventh zone is 180-240°C, the temperature of the eighth zone is 180-240°C, the temperature of the ninth zone is 180-240°C, the temperature of the die head is 210-250°C, the main engine speed is 300-500 rpm, and after extrusion, the extruder is cooled, pelletized and dried to obtain a polybutylene terephthalate modified material. The process conditions of the preparation method in each parallel experiment were the same.

[0050] Table 1

[0051]

[0052]

[0053] The specific test methods for the mechanical properties and laser marking effects of the polybutylene terephthalate modified materials of Examples 1-16 and Comparative Examples 1-4 of the present invention are as follows:

[0054] 1) Tensile strength: Tested according to ISO 527-2-2012, sample size is 150*10*4mm, tensile speed is 10mm / min;

[0055] 2) Contrast: In the middle of a color plate with a size of 80*55*2mm, laser marking is performed using a laser engraving machine with an infrared light source. The marking size is a circle with a diameter of not less than 30mm. The hue before and after the laser marking position is tested under a D65 light source, and the color difference is recorded as the contrast. The higher the contrast, the higher the clarity of the logo perceived by the human visual sense.

[0056] 3) Fastness: In the middle of a color plate with a size of 80*55*2mm, laser marking is performed using a laser engraving machine with an infrared light source. The logo pattern is a QR code. The QR code is scratched three times by reciprocating abrasion. The reciprocating abrasion scratching speed is 200mm / s, the load is 20N, and the friction medium is #400 mesh sandpaper selected in accordance with GB / T9258-2000. The fastness is determined by the clarity and microbubble shedding of the QR code after being scratched three times. Among them, after the QR code is scratched:

[0057] Excellent: The proportion of the area of ​​the detached microbubbles to the total area of ​​the microbubbles is less than 30%;

[0058] Good: The area of ​​the detached microbubbles accounts for 30-60% of the total microbubble area;

[0059] Poor; the area of ​​the detached microbubbles accounts for more than 60% of the total area of ​​the microbubbles;

[0060] Table 2 Test results of embodiments and comparative examples

[0061] Group Tensile Strength Contrast Fastness Example 1 138 27.66 excellent Example 2 145 26.02 excellent Example 3 135 17.40 excellent Example 4 141 19.25 excellent Example 5 140 25.74 excellent Example 6 136 24.16 excellent Example 7 138 29.75 excellent Example 8 135 29.76 excellent Example 9 130 27.78 excellent Example 10 137 29.2 excellent Embodiment 11 142 29.35 good Example 12 121 30.3 excellent Embodiment 13 140 29.52 excellent Embodiment 14 136 29.82 excellent Embodiment 15 137 27.78 good Example 16 131 27.92 good Comparative Example 1 138 27.66 Difference Comparative Example 2 145 5.11 good Comparative Example 3 139 6.62 good Comparative Example 4 136 5.32 excellent

[0062] From the results in Table 2, it can be seen that the polybutylene terephthalate modified materials prepared in Examples 1-16 of the present invention can achieve the dual effects of improving the clarity and fastness of laser marking black and white, and the mechanical properties of the modified materials are also good, and the overall performance is good. In the examples of the present invention, the tensile strength reaches more than 121 MPa, the contrast reaches 17.4, and the fastness grade is good or above.

[0063] The weight percentage of clay was adjusted in Examples 7, 11-14. The polybutylene terephthalate modified materials prepared in Examples 7, 13-14 can achieve the effect of improving the marking fastness of black and white laser marking better than that in Example 11. The tensile strength of Example 12 is reduced due to the high proportion of clay. Compared with Comparative Example 1, clay is added during the preparation of the polybutylene terephthalate modified material. When the laser marking additive is used, the position burned by the laser beam is instantly heated, and the clay component is sintered at high temperature to stabilize and enhance the microbubbles of the marking characters, thereby improving the laser marking fastness.

[0064] Comparing Examples 3-7 with Comparative Example 2, adding 0.1 to 1 parts by weight of carbon black can promote the absorption of laser light by the polybutylene terephthalate modified material, improve the foaming degree of the polybutylene terephthalate modified material, and further improve the clarity of the black and white laser marking. The contrast of Examples 5-7 is better than that of Examples 3-4, and the clarity of the marking is good.

[0065] Comparing Example 7 with Comparative Examples 3 and 4, when the amount of laser auxiliary agent is too small and the amount of carbon black is excessive, or when the amount of carbon black is too small and the amount of laser auxiliary agent is excessive, good laser marking black and white clarity cannot be obtained.

[0066] Comparing Examples 7-9 with Examples 15 and 16, when the clay specific surface area is less than 200m 2 / g, the marking fastness of the prepared polybutylene terephthalate modified material is reduced.

[0067] The polybutylene terephthalate modified material prepared by the invention is suitable for black and white laser marking by adding glass fiber, carbon black, laser auxiliary agent and clay into PBT resin, and has high laser marking clarity and marking fastness.

[0068] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A polybutylene terephthalate modified material, characterized in that: The composition comprises the following components in parts by weight: 40-85 parts of PBT resin, 20-50 parts of glass fiber, 0.1-1 parts of carbon black, 0.3-2 parts of laser auxiliary agent and 0.5-5 parts of clay; The clay is at least one of kaolinite clay, sepiolite clay, montmorillonite clay and bentonite clay; The specific surface area of ​​the clay is 90 to 230 m 2 / g.

2. The polybutylene terephthalate modified material according to claim 1, characterized in that: The weight portion of the carbon black is 0.2 to 0.6 parts, and the weight portion of the clay is 1 to 3 parts.

3. The polybutylene terephthalate modified material according to claim 1 or 2, characterized in that: The clay is sepiolite clay.

4. The polybutylene terephthalate modified material according to claim 1, characterized in that: The specific surface area of ​​the clay is greater than 100m 2 / g, less than or equal to 230m 2 / g.

5. The polybutylene terephthalate modified material according to claim 4, characterized in that: The specific surface area of ​​the clay is 210-230m 2 / g.

6. The polybutylene terephthalate modified material according to claim 1, characterized in that: The glass fiber is an alkali-free glass fiber, and the average diameter of the glass fiber is 7 to 13 μm.

7. The polybutylene terephthalate modified material according to claim 1, characterized in that: The laser auxiliary agent includes a basic copper phosphonate laser auxiliary agent, a laser auxiliary agent of a mixture of titanium oxide and a pigment, or a laser auxiliary agent of a tin antimony compound.

8. The polybutylene terephthalate modified material according to claim 1, characterized in that: The polybutylene terephthalate modified material further comprises 0 to 2 parts of a processing aid, wherein the processing aid is at least one of an antioxidant, a lubricant, a weathering aid, a coupling agent, an antibacterial agent, an anti-dripping agent, an ester exchange inhibitor and a colorant.

9. The method for preparing the polybutylene terephthalate modified material according to any one of claims 1 to 8, characterized in that: The following steps are involved: According to the proportion, PBT resin, glass fiber, carbon black, laser auxiliary agent, clay and processing auxiliary agent are added into an extruder, melt-extruded at 180° C. to 260° C., cooled and granulated to obtain the polybutylene terephthalate modified material.

10. Use of the polybutylene terephthalate modified material according to any one of claims 1 to 8 in automobiles and electronic and electrical products.

Citation Information

Patent Citations

  • Polycarbonate compound capable of performing laser marking

    CN103467956A

  • A marking powder, its preparation method and application; a high-rigidity PC alloy suitable for laser marking and its preparation method.

    CN112266500B

  • Glass fiber reinforced polybutylene terephthalate resin composition with laser printing marking function and preparation method thereof

    CN101423653A

  • PET resin composition with laser mark function and preparation method thereof

    CN102070889A