A high-efficiency diamond wire cutting coolant
By adding organic boron surfactant and water-based wax to the diamond wire cutting coolant, the problem of insufficient protection of the diamond wire by the existing coolant is solved, the cutting force and yield are improved, and a more efficient diamond wire cutting effect is achieved.
Patent Information
- Application Number
- CN202111585491.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-23
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2041-12-23
AI Technical Summary
The existing coolant does not adequately protect the diamond wire, resulting in insufficient cutting force, abnormal cutting process, and low yield.
A high-efficiency diamond wire cutting coolant is used, and organic boron surfactant and water-based wax are added to improve the lubrication performance and enhance the cutting ability of the diamond wire. The composition includes silicon powder dispersant, wetting and penetrating agent, solubilizer, and organic boron surface activity. agents and water-based waxes.
It significantly enhances the lubricity of the cutting system, reduces the torque during the cutting process, protects the diamond wire, improves the cutting capacity, and significantly improves the cutting yield.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of diamond wire cutting and relates to a high-efficiency diamond wire cutting coolant. Background Art
[0002] In recent years, with the rapid development of the photovoltaic industry, the cost of solar power generation has dropped significantly. As the basic material in the photovoltaic industry, the quality and cost of silicon wafers determine the prospects and development trends of the entire industry.
[0003] At present, the auxiliary materials used in the process of front-of-cabinet cutting are mainly diamond wire and coolant. The role of diamond wire is to cut silicon ingots into silicon wafers, and the role of coolant is to protect diamond wire, disperse silicon powder, and dissipate heat and cool down.
[0004] With the advancement of thinning and filming in the industry, the protection of diamond wire by existing coolants has gradually weakened. The diamond wire is excessively worn during the cutting process, resulting in insufficient cutting force, which leads to abnormal cutting process and low cutting yield. Summary of the invention
[0005] In view of the problem that the current coolant does not provide sufficient protection for the diamond wire, the present invention provides a high-efficiency diamond wire cutting coolant. The coolant has excellent steel wire protection ability, silicon powder dispersion ability, excellent wetting performance, good cooling and heat dissipation performance, and outstanding foam control performance. By adding organic boron surfactant and aqueous wax, the lubrication performance of the coolant is greatly improved, and the cutting ability of the diamond wire is effectively enhanced.
[0006] A high-efficiency diamond wire cutting coolant comprises the following components recorded by mass fraction: 25%-50% of silicon powder dispersant, 5%-15% of wetting penetrant, 5%-15% of solubilizer, 2%-5% of organic boron surfactant, 3%-10% of water-based wax, and the balance is deionized water.
[0007] Wherein, the silicon powder dispersant is a monohydric alcohol and / or a polyhydric alcohol polyether;
[0008] The monohydric alcohol polyether and / or polyhydric alcohol polyether is a composite product of one or more of alkylphenol polyoxyethylene polyoxypropylene ether, propylene glycol polyoxyethylene polyoxypropylene ether, allyl polyoxyethylene polyoxypropylene ether, and tetra- to ten-carbon fatty alcohol polyoxyethylene polyoxypropylene ether.
[0009] Among them, the wetting and penetrating agent is a composite product of one or more of isooctyl alcohol polyoxyethylene ether, isomeric dodecanol polyoxyethylene ether, hexa- to octa-carbon acetylene glycol polyoxyethylene ether, and isomeric tridecanol polyoxyethylene ether.
[0010] The solubilizer is a compound product of one or more of ethylene glycol, diethylene glycol, propylene glycol, diethylene glycol monobutyl ether, polyethylene glycol 400, and polyethylene glycol 600.
[0011] Among them, the organic boron surfactant is a composite product of one or more of twelve to twenty carbon alkyl polyoxyethylene ether monoboric acid glyceryl ester and ten to eighteen carbon alkyl polyoxyethylene diboric acid glyceryl ester.
[0012] The aqueous wax is a composite product of one or more aqueous wax emulsions and aqueous wax dispersions.
[0013] Compared with existing coolants, the high-efficiency diamond wire cutting coolant of the present invention has the following advantages: it greatly enhances the lubricity of the cutting system, effectively reduces the torque during the cutting process, protects the diamond wire, and largely retains the cutting ability of the diamond wire. DETAILED DESCRIPTION
[0014] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0015] Example 1
[0016] A high-efficiency diamond wire cutting coolant, comprising the following components by mass fraction:
[0017] Alkylphenol polyoxyethylene polyoxypropylene ether 35%
[0018] 10% polyoxyethylene isooctanol ether
[0019] Ethylene glycol 10%
[0020] Tetradecyl polyoxyethylene ether monoboric acid glyceryl ester 4%
[0021] MD-2000 water-based wax 5%
[0022] Deionized water balance
[0023] Example 2
[0024] A high-efficiency diamond wire cutting coolant, comprising the following components by mass fraction:
[0025] Allyl polyoxyethylene polyoxypropylene ether 40%
[0026] Isotridecyl alcohol polyoxyethylene ether 10%
[0027] 2-Ethylhexyl alcohol polyoxyethylene ether 5%
[0028] Diethylene glycol monobutyl ether 6%
[0029] Dodecyl polyoxyethylene ether monoboric acid glyceryl ester 2.5%
[0030] W-19 water-based wax dispersion 7.5%
[0031] Deionized water balance
[0032] Example 3
[0033] A high-efficiency diamond wire cutting coolant, comprising the following components by mass fraction:
[0034] Hexa-carbon fatty alcohol polyoxyethylene polyoxypropylene ether 50%
[0035] Octa-acetylene glycol polyoxyethylene ether 15%
[0036] Diethylene glycol 10%
[0037] Tetradecyl polyoxyethylene ether diborate glyceryl ester 3%
[0038] Sasol HW-46 water-based wax emulsion 10%
[0039] Deionized water balance
[0040] Example 4
[0041] A high-efficiency diamond wire cutting coolant, comprising the following components by mass fraction:
[0042] Propylene glycol polyoxyethylene polyoxypropylene ether 20%
[0043] 15% polyoxyethylene polyoxypropylene ether of ten carbon fatty alcohol
[0044] Isomeric dodecanol polyoxyethylene ether 15%
[0045] Polyethylene glycol 400 10%
[0046] Octadecanyl polyoxyethylene ether monoboric acid glyceryl ester 5%
[0047] PTFE-1005 water-based wax dispersion 8%
[0048] Deionized water balance
[0049] Table 1 Comparison of cutting yield rate of anti-breaking diamond wire cutting coolant
[0050] contrast Number of pieces in stock Slice A A Color difference A Silicon Falls Bright Edge Dropping Line marks TTV Disconnection and abandonment Example 1 1259487 93.65% 92.47% 1.05% 0.30% 0.56% 0.47% 0.45% 0.21% 0.33% Example 2 1138947 94.15% 93.27% 0.48% 0.12% 0.21% 0.43% 0.35% 0.57% 0.37% Example 3 1546399 95.68% 94.30% 0.15% 0.06% 0.37% 0.29% 0.42% 0.36% 0.02% Example 4 1238769 94.13% 92.66% 0.44% 0.25% 0.51% 0.50% 0.39% 0.23% 0.44% Commercially available coolant 1 1175386 92.14% 91.20% 1.21% 0.23% 0.32% 0.63% 0.43% 0.53% 0.87% Commercially available coolant 2 1602157 91.78% 91.06% 0.33% 0.28% 0.24% 0.43% 0.59% 0.32% 1.26%
[0051] The above tests were conducted with the same equipment, a unit consumption of 1.8L, a diamond wire with a diameter of 43μm, and a silicon wafer size of 182mm×182mm. The cutting comparison experiment was conducted under the same process conditions. From the analysis of the data results, the embodiment of the present invention has obvious advantages in use, and the specific yields of once A and slice A are significantly higher than those of commercially available coolants.
[0052] The above are only preferred specific embodiments of the present invention, and the protection scope of the present invention is not limited thereto. Any obvious improvement, replacement or modification made by any technician familiar with the technical field within the technical scope disclosed by the present invention without departing from the essential content of the present invention shall fall within the protection scope of the present invention.
Claims
1. A high-efficiency diamond wire cutting coolant, characterized in that: The composition comprises the following components by mass fraction: 25%-50% of silicon powder dispersant, 5%-15% of wetting and penetrating agent, 5%-15% of solubilizer, 2%-5% of organic boron surfactant, 3%-10% of water-based wax, and the balance is deionized water; The organic boron surfactant is a composite product of one or more of 12-20 carbon alkyl polyoxyethylene ether monoboric acid glyceryl ester and 10-18 carbon alkyl polyoxyethylene diboric acid glyceryl ester; The aqueous wax is a composite product of one or more aqueous wax emulsions and aqueous wax dispersions.